Gallium nitride device for improving heat dissipation performance by adopting radiation refrigeration and preparation method thereof
By adopting radiation refrigeration technology in GaN devices, using silver reflective layer and multi-layer SiO2/Si3N4 cylindrical structure radiation refrigeration layer, the thermal management problem of GaN devices in high-power applications is solved, the heat dissipation performance and stability are improved, and the thermal dissipation performance and stability are simplified. The process is reduced and energy loss is reduced.
Patent Information
- Application Number
- CN202411061585.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
AI Technical Summary
Existing GaN devices have thermal management problems in high-power applications, resulting in reduced carrier mobility, deterioration of electrical characteristics and stability effects. The existing technologies such as diamond substrates and boron nitride/diamond heterojunction substrates exist. The problem of unsatisfactory lattice matching, complex process and high cost.
By using radiation refrigeration technology, the heat dissipation performance of the device is improved by setting the silver reflective layer and the multi-layer SiO2/Si3N4 cylindrical structure of the substrate layer, the heat dissipation performance of the device is improved, the high thermal conductivity material is avoided directly contact with the GaN epitaxial layer, reducing thermal resistance and improving Electrical properties.
It effectively improves the heat dissipation performance and stability of GaN devices, reduces energy losses, enhances the long-term working reliability and overall electrical performance of the device, and simplifies the process.
Smart Images

Figure CN118969751A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor devices, and in particular relates to a GaN device and a preparation method thereof, which can be used as a microwave power device and a power electronic device. Background Art
[0002] With the booming development of the semiconductor industry, devices based on GaN, an emerging wide bandgap semiconductor material, have been widely used in various fields. With its ultra-high electron saturation drift velocity and electron mobility, GaN materials have great advantages in efficient power switching and handling large currents. Therefore, GaN devices perform well in high-power and high-frequency applications, providing an ideal solution for power amplifiers, RF power devices, etc. With its wide bandgap and high breakdown electric field, GaN materials show outstanding stability under high temperature conditions, which makes it very suitable for various harsh working environments and is widely used in key industries such as communications, energy, and military. Looking to the future, with the advancement of technology, GaN devices will continue to use their unique properties to strongly promote the innovation of electronic technology and its wide application in various fields.
[0003] However, as device performance continues to improve, the operating power of the device also increases, and the high heat flow caused by high power becomes impossible to ignore. Due to the serious self-heating effect in the device, the carrier mobility of the device will be greatly reduced, which will not only deteriorate the electrical properties of the device, but also affect the long-term stability of the device. For GaN materials, their thermal conductivity is low, causing the heat generated during the operation of the device to accumulate rapidly in the device, limiting the output power density and efficiency of GaN devices. Therefore, effective thermal management technology is needed to improve the electrical properties and reliability of the device.
[0004] Patent document with application number CN201910326079.X discloses a GaN device based on a diamond substrate and a method for preparing the same. Figure 1 As shown, it includes a source electrode 6, a drain electrode 7 and a gate electrode 8, a barrier layer 5, a buffer layer 4, a nucleation layer 3, a gallium nitride material layer 1 and a diamond layer 2 from bottom to top. That is, diamond material is directly grown on the first surface of the gallium nitride material layer, and an AlN nucleation layer and a GaN buffer layer are grown on the second surface to form a two-dimensional electron gas channel, so as to realize the preparation of a diamond substrate as a substrate for a GaN device. The device epitaxially grows GaN material directly on a diamond substrate and prepares a GaN device therefrom, thereby utilizing diamond with high thermal conductivity to perform thermal management on the GaN device. However, due to the unsatisfactory lattice matching between GaN materials and materials such as diamond, the quality of the GaN epitaxial layer grown on materials such as diamond is difficult to guarantee, and the advantages of GaN materials cannot be brought into play.
[0005] Patent document with application number CN202211651146.3 discloses a heat dissipation structure for a gallium nitride device and a preparation method thereof, which uses a boron nitride (BN) / diamond heterojunction substrate to dissipate heat for gallium nitride devices. Boron nitride and diamond have high thermal conductivity, but the compatibility of their materials with gallium nitride cannot be guaranteed, and the growth process of diamond and boron nitride is difficult and costly, resulting in reduced device reliability and high prices.
[0006] Patent document with application number CN202310476236.1 discloses a method for preparing a gallium nitride / diamond composite heat dissipation layer with low interface thermal resistance. Diamond is grown on the gallium nitride layer by magnetron sputtering as a heat dissipation layer, and this is used as the heat dissipation layer of the gallium nitride device. However, it is difficult to guarantee the electrical performance of the gallium nitride device prepared in this way, because diamond needs to be grown on the gallium nitride material, and its parameters such as lattice matching and thermal expansion coefficient will affect the device performance.
[0007] Patent document with application number CN202210100966.7 discloses a gallium nitride epitaxial growth method that is beneficial to improving heat dissipation. Gallium nitride is directly epitaxially grown on a copper single crystal, and the high thermal conductivity of copper is used to improve the heat dissipation capacity of gallium nitride devices. Due to the adverse effects of lattice mismatch between metallic copper and gallium nitride materials, the quality of the epitaxial layer is difficult to guarantee, and the heat dissipation capacity of metallic copper is limited, so it is impossible to effectively dissipate heat, and a more effective heat dissipation method is still needed. Summary of the invention
[0008] The purpose of the present invention is to address the deficiencies in the prior art and propose a GaN device and a preparation method that use radiative cooling to improve heat dissipation performance, so as to avoid lattice mismatch and additional stress caused by direct contact between the GaN epitaxial layer and the high thermal conductivity material, improve the thermal conductivity of the device, and while reducing the energy loss of the device, further improve the long-term working stability and reliability of the device.
[0009] The technical solutions for achieving the purpose of the present invention include the following:
[0010] 1. A GaN device that uses radiation cooling to improve heat dissipation performance, comprising from bottom to top: a substrate layer 2, a nucleation layer 3, a buffer layer 4, a channel layer 5, a barrier layer 6 and a passivation layer 7, wherein the barrier layers 6 on both sides of the passivation layer 7 are provided with source and drain electrodes, and the barrier layers between the source and drain electrodes near the source electrode are provided with a drain electrode, characterized in that:
[0011] The substrate layer 2 has a silver reflective layer 1 on its lower surface to effectively conduct the heat generated in the device, improve the heat reflection efficiency, and enhance the heat dissipation capacity of the device;
[0012] The passivation layer 7 has a plurality of SiO2 / Si3N4 cylindrical structures composited up and down between the metal electrodes on its upper surface, forming a radiation cooling layer 8 to enhance the heat dissipation performance of the device.
[0013] Furthermore, the silver reflective layer 1 has a thickness of 1 to 20 μm and is made of a high-metal silver material with a thermal conductivity of 400 to 450 W / mK to improve the heat reflection efficiency and the heat dissipation capacity of the device.
[0014] Furthermore, the radiation cooling layer 8 has a composite SiO2 / Si3N4 cylindrical structure with a thickness of 1 to 15 μm. The composite cylindrical structure can also be made of any one of aluminum oxide, hafnium oxide or titanium oxide materials and Si 3 N 4 Perform upper and lower compounding.
[0015] Furthermore, the substrate layer 2 is made of Si or SiC, and its thickness is 150-650 μm; the nucleation layer 3 is made of AlN, and its thickness is 120-250 nm. Si, SiC or AlN can also be used. 2 O 3 .
[0016] Furthermore, the buffer layer 4 is made of any one of GaN, AlN or AlGaN, and has a thickness of 0.1 to 5 μm; the channel layer 5 is made of GaN, and has a thickness of 30 to 800 nm.
[0017] Furthermore, the barrier layer 6 is made of AlGaN with a thickness of 10 to 35 nm, and may also be made of an AlGaN / AlN structure; the passivation layer 7 is made of SiO 2 or Si 3 N 4 Insulating medium, used for electrical isolation, with a thickness of 60 to 200 nm.
[0018] 2. A method for preparing a GaN device using radiative cooling to improve heat dissipation performance, comprising the following steps:
[0019] S1: epitaxially depositing a nucleation layer, a buffer layer, a channel layer, and a barrier layer in sequence on the front side of the substrate by metal organic chemical vapor deposition (MOCVD);
[0020] S2: Electrode metal is first deposited on the barrier layer by electron beam evaporation (E-Beam), followed by ion implantation for isolation, and then a passivation layer is deposited by atomic layer deposition (ALD);
[0021] S3: connecting the upper surface of the passivation layer to an external carrier wafer through a bonding process;
[0022] S4: pre-treatment of the back side of the substrate by thinning the substrate and polishing the surface;
[0023] S5: depositing a metallic silver reflective layer on the back side of the pre-treated substrate by electron beam evaporation E-Beam, and removing the carrier wafer;
[0024] S6: The pattern of the radiation cooling layer is set on the front side of the device by photolithography, and then SiO2 and Si3N4 are deposited by plasma enhanced chemical vapor deposition (PECVD) and atomic layer deposition (ALD) respectively to form a radiation cooling layer composed of multiple SiO2 / Si3N4 cylindrical structures composited up and down;
[0025] S7: Through the stripping process, the wafer with the radiation cooling layer is immersed in a photoresist stripping solution to remove excess photoresist, thereby completing the device preparation.
[0026] Compared with the existing invention, the present invention has the following advantages:
[0027] 1) Since the present invention has a radiation cooling layer prepared on the passivation layer, it can absorb the heat inside the device. There is no need to add an additional water pump to realize water circulation like a microchannel, and there is no need to contact the conductive channel material. The heat can be radiated to the outside of the device efficiently, and the heat generated by the device can be absorbed and reflected through multiple layers of radiation materials, effectively reflecting the heat generated by the device to the external environment, thereby improving the heat dissipation performance of the device.
[0028] 2) Since the present invention prepares a silver reflective layer under the substrate, it can reflect part of the heat to the surface radiation cooling layer, thereby improving the heat reflection efficiency. At the same time, metallic silver has good thermal conductivity, which can help reflect heat while improving the thermal conductivity of the substrate, further improving the heat dissipation performance of the device.
[0029] 3) The radiation cooling layer of the present invention adopts a cylindrical structure of multiple upper and lower composite SiO2 / Si3N4, and does not need to be in direct contact with the GaN epitaxial layer. It not only has no effect on the quality of the epitaxial layer, but can more effectively reduce the thermal resistance of the device, and can effectively avoid the lattice mismatch and damage of the GaN material caused by the high thermal conductivity material, and can greatly improve the heat dissipation performance of the device while achieving excellent electrical performance.
[0030] 4) Since the present invention integrates the radiation cooling layer directly on the front side of the device, a shorter heat transfer path is achieved, the overall heat dissipation efficiency of the device is improved, and the device integration is convenient, which helps to reduce the size and weight of the equipment. At the same time, the process complexity of the device is reduced, and the reliability, stability and overall electrical performance of the device are improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a diagram of the existing GaN device structure.
[0032] Figure 2It is a schematic diagram of the structure of a GaN HEMT that uses radiation cooling to improve heat dissipation performance in the present invention;
[0033] Figure 3 The invention is made Figure 2 Schematic diagram of device process flow;
[0034] Figure 4 It is a schematic diagram of the process flow of manufacturing GaN Schottky diode SBD according to the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below with reference to the accompanying drawings and embodiments.
[0036] Reference Figure 2 The GaN high electron mobility transistor HEMT of the present invention comprises a silver reflective layer 1, a substrate layer 2, a nucleation layer 3, a buffer layer 4, a channel layer 5, a barrier layer 6, a passivation layer 7, a radiation layer 8, and a source electrode S, a drain electrode D, and a gate electrode G. Wherein:
[0037] The silver reflector 1 is made of high-metal silver material with a thickness of 1 to 20 μm and a thermal conductivity of 400 to 450 W / mK, and is attached to the lower surface of the substrate layer 2 to improve the heat reflection efficiency and the heat dissipation capacity of the device.
[0038] The substrate layer 2 is made of Si or SiC and has a thickness of 80 to 650 μm.
[0039] The nucleation layer 3 is made of AlN and has a thickness of 120-250 nm. It is located on the upper surface of the substrate layer 2 .
[0040] The buffer layer 4 is made of any one of GaN, AlN or AlGaN, has a thickness of 0.1-5 μm, and is located on the nucleation layer 3 .
[0041] The channel layer 5 is made of GaN and has a thickness of 30-850 nm. It is located on the buffer layer 4 .
[0042] The barrier layer 6 is made of AlGaN and has a thickness of 10-30 nm. It is located on the channel layer 5 .
[0043] The source electrode S and the drain electrode D are made of Ti / Au with a thickness of 20-60 / 80-200 nm, and are located at both ends of the barrier layer 6;
[0044] The gate G is made of Ni / Au and has a thickness of 20-60 / 60-200 nm. It is located between the source S and the drain D.
[0045] The passivation layer 7 is made of SiO 2 or Si 3 N 4, with a thickness of 80 to 250 nm, which wraps around the source S, drain D, and gate G.
[0046] The radiation cooling layer 8 is formed by a plurality of SiO2 / Si3N4 cylindrical structures composited up and down and arranged at a pitch of 5 to 20 μm to enhance the heat dissipation performance of the device. Each SiO2 / Si3N4 cylindrical structure composited up and down has a thickness of 1 to 15 μm and a diameter of 4 to 50 μm. The composite cylindrical structure can also be made of any one of aluminum oxide, hafnium oxide or titanium oxide materials and Si 3 N 4 The upper and lower composites are carried out and located on the upper surface of the passivation layer 7 .
[0047] The above-mentioned device based on the radiation cooling layer structure can be used not only for GaN high electron mobility transistor HEMT, but also for GaN Schottky diode SBD to improve the heat dissipation performance of the device.
[0048] Reference Figure 3 and Figure 4 The present invention provides the following three embodiments.
[0049] In Example 1, a silver reflective layer with a thickness of 10 μm and a thermal conductivity of 430 W / mK is made on a Si substrate; a radiation cooling layer is SiO 2 / Si 3 N 4 The composite layer has a thickness of 1.5 μm; the buffer layer is GaN and has a thickness of 1 μm. High electron mobility transistor HEMT.
[0050] Step 1: epitaxially deposit a group III nitride material on the front side of the Si substrate 2, such as Figure 3 (a).
[0051] 1.1) Deposition of AlN nucleation layer 3:
[0052] A Si-based substrate with a size of 6 inches, a thickness of 500 μm, and a crystal orientation of
[111] was selected;
[0053] Using metal organic chemical vapor deposition (MOCVD) technology, 3 Under the process conditions of a flow rate ratio of 1800 to TMAl, a temperature of 500° C., and a growth pressure of 100 mbar, an AlN nucleation layer 3 with a thickness of 250 nm is epitaxially grown on the front surface of the Si substrate 2;
[0054] 1.2) Deposition of GaN buffer layer 4:
[0055] Similar to the deposition of the nucleation layer, metal organic compound chemical vapor deposition MOCVD technology is used to deposit the 3Under the process conditions of a flow rate ratio of 1800 to TMGa, a temperature of 950 °C, and a growth pressure of 50 mbar, an epitaxial growth layer with a thickness of 1 μm and a Fe doping concentration of 5×10 18 cm -3 GaN buffer layer 4;
[0056] 1.3) Deposition of GaN channel layer 5:
[0057] Using metal organic chemical vapor deposition (MOCVD) technology, 3 Under the process conditions of a flow rate ratio of 2000 to TMGa, a temperature of 900° C., and a growth pressure of 120 mbar, a non-intentionally doped GaN channel layer 5 with a thickness of 200 nm is epitaxially grown on the GaN buffer layer 4;
[0058] 1.4) Deposition of AlGaN barrier layer 6:
[0059] Using metal organic chemical vapor deposition (MOCVD) technology, 3 Under the process conditions of a flow rate ratio of 2000 to TMGa, a flow rate ratio of TMGa to TMAl of 4, a temperature of 950° C., and a growth pressure of 50 mbar, an AlGaN barrier layer 6 with an Al composition of 0.25 and a thickness of 20 nm is epitaxially grown on the GaN channel layer 5 .
[0060] Step 2: Deposit source S, drain D, and gate G metal electrodes on the surface of the barrier layer 6, and perform device isolation and deposit a passivation layer 7, such as Figure 3 (b).
[0061] 2.1) First, a layer of photoresist is coated on the surface of the barrier layer 6, and then alignment, exposure, development and pattern detection are performed to form the source and drain regions of the device; then, Ar plasma is used to bombard the source and drain regions for 35 seconds to reduce the source and drain contact resistance;
[0062] 2.2) At a vacuum degree of 2.0×10 -4 In Pa's workroom, electron beam evaporation E-Beam technology was used, with the electron gun acceleration voltage set to 10kV and the electron beam current set to 0.3A. After a 1000-second evaporation process, 60nm and 1000nm thick Ti / Au metal layers were deposited in the source S and drain D regions, respectively. The wafer covered with the metal layer was then immersed in a photoresist stripping solution to remove the remaining photoresist.
[0063] 2.3) After the source and drain metals are grown and stripped, the wafer is placed in a rapid thermal annealing furnace at N 2Rapid annealing in an environment for 30 seconds, with the annealing temperature in the furnace being 850° C., so as to form a good ohmic contact at the contact surface of the source, drain and barrier layer 6;
[0064] 2.4) Perform a second photolithography process on the surface of the barrier layer 6 to define the gate region and -4 In Pa's workroom, the electron beam evaporation E-Beam technology is used, the electron gun acceleration voltage is set to 10kV and the electron beam current is set to 0.3A. After a 1000-second evaporation process, 40nm and 1000nm thick Ni / Au metal layers are deposited in the gate area in sequence, thereby forming a Schottky contact between the gate G and the barrier layer 6; then the wafer is immersed in a photoresist stripping solution to remove the residual photoresist;
[0065] 2.5) Using ion implantation technology, the implantation energy is 310keV and the ion concentration is 8×10 14 cm -2 Under the process conditions, high-energy ions are implanted into the surface of the barrier layer 6 outside the active area of the wafer to form device isolation;
[0066] 2.6) Using atomic layer deposition (ALD) technology, a 120 nm thick Si layer is epitaxially grown along the barrier layer 6 around the source S, drain D and gate G at a temperature of 200°C and a pressure of 1.3 mbar in the reaction chamber. 3 N 4 Passivation layer 7.
[0067] Step 3: Paste the surface of the passivation layer 7 to the sapphire carrier wafer 202 through the high-temperature paraffin layer 201, and apply pressure to bond them, such as Figure 3 (c).
[0068] Step 4: Process the back side of the Si substrate 2, such as Figure 3 (d).
[0069] 4.1) The back side of the Si substrate 2 of the device containing the substrate 2, the nucleation layer 3, the buffer layer 4, the channel layer 5, the barrier layer 6, the passivation layer 7, the source S, the drain D and the gate G is ground and thinned to reduce its thickness to 150 μm.
[0070] 4.2) The back side of the thinned Si substrate 2 is polished by a polishing process to improve the smoothness and uniformity of the wafer surface.
[0071] Step 5: Deposit a silver reflective layer 1 on the back of the substrate 2, such as Figure 3 (e).
[0072] 5.1) Through electron beam evaporation E-Beam, the vacuum in the working room is evacuated to 3×10 -4Under the process conditions of 9KV electron gun acceleration voltage, 0.6A electron gun beam current and 5000s evaporation time, a metal Ag with a thickness of 10μm is deposited on the back side of the Si substrate 2 as a back side silver reflective layer 1;
[0073] Step 6: Remove the carrier wafer and grow the radiation layer material on the passivation layer 7.
[0074] 6.1) Using a wax removal liquid to remove the sapphire carrier 202 bonded to the surface of the passivation layer;
[0075] 6.2) Spin-coat a layer of photoresist on the surface of the passivation layer 7, perform alignment, exposure, development and pattern detection, and then cover the metal electrode layer with 301 photoresist to protect the metal electrode and define the radiation layer pattern.
[0076] 6.3) According to the defined radiation layer pattern, using plasma chemical vapor deposition (PECVD) technology, under the conditions of maintaining a temperature of 300°C and a pressure of 1.3 mbar in the reaction chamber, along the passivation layer 7 around the source S, drain D and gate G covered with photoresist, multiple SiO2 layers with a thickness of 0.75 μm and a diameter of 10 μm are epitaxially grown at a spacing of 10 μm. 2 layer;
[0077] 6.4) Keeping the temperature and pressure of the reaction chamber constant, using the atomic layer deposition ALD technology, along the passivation layer 7 covered with the photoresist source S, drain D and gate G periphery, at each HfO 2 A Si layer with a thickness of 0.75 μm and a diameter of 10 μm is epitaxially grown on the layer. 3 N 4 layer, forming multiple columnar SiO 2 / Si 3 N 4 radiation layer, and transfer it to the surface of the passivation layer 7, such as Figure 3 (f);
[0078] Step 7: Remove excess SiO using a lift-off process 2 / Si 3 N 4 Composite layer, forming a radiation cooling layer 8, such as Figure 3 (g).
[0079] The wafer with the above-mentioned radiation layer is placed in a photoresist stripping solution for immersion stripping to remove excess SiO 2 / Si 3 N 4 The composite layer forms a radiation cooling layer 8 consisting of a plurality of composite columnar radiation layer structures, thereby completing the device preparation.
[0080] Example 2: A silver reflective layer with a thickness of 2 μm and a thermal conductivity of 429 W / mK is made on a SiC substrate; a radiation cooling layer is made of HfO 2 / Si 3 N 4 The composite layer has a thickness of 2 μm; the buffer layer is AlGaN, the Al component is 0.05, and the thickness is 1.5 μm with a back barrier structure GaN high electron mobility transistor HEMT.
[0081] Step 1: epitaxially depositing a group III nitride material on the front side of the SiC substrate 2, such as Figure 3 (a).
[0082] The size is 6 inches and the thickness is 600 μm.
[0083] Setting NH 3 Under the process conditions of a flow rate ratio of 1800 to TMAl, a temperature of 700°C, and a growth pressure of 150 mbar, epitaxial growth is performed on the front side of the SiC substrate 2 by using a metal organic chemical vapor deposition MOCVD technology to form an AlN nucleation layer 3 with a thickness of 160 nanometers;
[0084] Setting NH 3 Under the process conditions of a flow rate ratio of 2200 to TMGa, a flow rate ratio of TMGa to TMAl of 20, a temperature of 1050°C, and a growth pressure of 120 mbar, an AlGaN buffer layer 4 with an Al component content of 0.05 and a thickness of 2 μm is epitaxially grown on the AlN nucleation layer 3 by using a metal organic chemical vapor deposition MOCVD technology;
[0085] The process conditions are set such that the flow rate ratio of NH3 to TMGa is 2000, the temperature is 950°C, and the pressure is 100 mbar, and a non-intentionally doped GaN channel layer 5 with a thickness of 250 nanometers is epitaxially grown on the AlGaN buffer layer 4 using a metal organic chemical vapor deposition MOCVD technology;
[0086] Setting NH 3 Under the process conditions of a flow rate ratio of 2400 to TMGa, a flow rate ratio of TMGa to TMAl of 4, a temperature of 1100°C and a pressure of 90 mbar, an AlGaN barrier layer 6 with an Al component of 0.25 and a thickness of 25 nm is epitaxially grown on the GaN channel layer 5 using metal organic chemical vapor deposition (MOCVD) technology.
[0087] Step 2: Deposit source S, drain D, and gate G metal electrodes on the surface of the barrier layer 6, and perform device isolation and deposit a passivation layer 7, such as Figure 3 (b).
[0088] The surface of the barrier layer 6 is photolithographically processed. First, a layer of photoresist is spin-coated on the barrier layer 6. Then, alignment, exposure, development, and pattern detection are performed in sequence to form the source and drain regions of the device. Then, Ar plasma treatment is used to bombard the source and drain regions for 30 seconds to reduce the source and drain contact resistances.
[0089] The process conditions were set as follows: the vacuum degree of the working chamber was 2.0×10^-4Pa, the acceleration voltage of the electron gun was 9.5kV, the beam current of the electron gun was 0.6A, and the evaporation time was 1200 seconds. The electron beam evaporation E-Beam technology was used to deposit 40nm and 1200nm thick Ti / Au metal layers in the source S and drain D regions, respectively. The device was then placed in a photoresist stripping solution to remove the residual photoresist.
[0090] The wafer with the source and drain metal deposited was placed in an annealing furnace and the annealing temperature was set to 850°C under N 2 Rapid annealing in an environment for 60 seconds to form ohmic contacts at the contact surfaces of the source, drain and barrier layer 6;
[0091] The surface of the barrier layer 6 is again photolithographically formed into a gate region, and the vacuum degree of the working chamber is set to 2.0×10 -4 Pa, an electron gun acceleration voltage of 9.5 Kv, and an electron gun beam current of 0.6 A, and an electron beam evaporation E-Beam technology is used to evaporate for 1200 s, and a Ni / Al layer with a thickness of 40 / 1200 nm is deposited in the gate region as the gate G to form a Schottky contact at the contact surface of the gate G and the barrier layer 6, and then it is placed in a photoresist stripping solution to remove the photoresist;
[0092] The implantation energy was set to 320 keV and the ion concentration was set to 8×10 14 cm -2 Under the process conditions, high-energy ions are implanted into the surface of the barrier layer 6 outside the active area of the wafer by ion implantation technology to complete device isolation;
[0093] The process conditions of the reaction chamber temperature is set to 360°C and the pressure is set to 2.0 mbar. Atomic layer deposition (ALD) technology is used to epitaxially grow SiO with a thickness of 120 nm on the barrier layer 6 around the source S, drain D, and gate G. 2 Passivation layer 7.
[0094] Step 3: Paste the surface of the passivation layer 7 to the sapphire carrier wafer 202 through the high-temperature paraffin layer 201, and apply pressure to bond them, such as Figure 3 (c).
[0095] Step 4: Making a silver reflective layer 1 on the back of the SiC substrate 2
[0096] The back side of the SiC substrate 2 after the above steps is thinned by grinding to reduce its thickness to 250 μm; the back side of the thinned SiC substrate 2 is then polished by using a polishing technique to improve the smoothness and flatness of the wafer surface. Figure 3 (d).
[0097] Set the working chamber to evacuate to 2 × 10 -4 Pa, electron gun acceleration voltage of 9Kv, electron gun beam current of 0.6A, and evaporation time of 1000s, by electron beam evaporation E-Beam technology, a metal Ag with a thickness of 2μm is deposited on the back side of the Si substrate 2 as the back side silver reflective layer 1, such as Figure 3 (e).
[0098] Step 5: growing a radiation cooling layer 8 on the passivation layer 7 .
[0099] 5.-1) Remove the carrier wafer and use photolithography to define the radiation heat dissipation layer pattern between the upper surface of the passivation layer 7 and the metal electrode:
[0100] The sapphire carrier 202 bonded to the surface of the passivation layer is removed by using a wax removal liquid.
[0101] First, a layer of photoresist is spin-coated on the surface of the passivation layer 7, and then alignment, exposure, development and pattern detection are performed, the metal electrode layer is covered with photoresist, and the radiation layer pattern is set.
[0102] 5-.2) epitaxially growing a radiation layer 8 on the passivation layer 7 according to the set radiation layer pattern:
[0103] Covering the metal electrode with photoresist 301 to protect the metal electrode;
[0104] The process conditions of the reaction chamber temperature was set to 300°C and the pressure was set to 1.3 mbar. The plasma chemical vapor deposition (PECVD) technology was used to epitaxially grow multiple HfO layers with a thickness of 0.75 μm and a diameter of 20 μm along the passivation layer 7 around the source S, drain D and gate G covered with photoresist at a spacing of 15 μm. 2 layer;
[0105] Keeping the temperature and pressure of the reaction chamber constant, using the atomic layer deposition ALD technology, along the passivation layer 7 covered with the photoresist source S, drain D and gate G periphery, at each HfO 2 A Si layer with a thickness of 0.75 μm and a diameter of 20 μm is epitaxially grown on the layer. 3 N 4 layers, forming multiple HfO 2 / Si 3 N 4 The composite column material layer is then transferred to the surface of the passivation layer 7, such as Figure 3 (f);
[0106] 5-3) Making a radiation cooling layer 8, such as Figure 3 (g)
[0107] Place the wafer with the composite material layer into the photoresist stripping solution to remove excess HfO 2 / Si 3 N 4 The composite layer forms a radiation cooling layer 8 on the surface of the passivation layer 7. The device is manufactured.
[0108] Example 3: A silver reflective layer with a thickness of 16 μm and a thermal conductivity of 425 W / mK is made on a Si substrate; a radiation cooling layer is SiO 2 / Si 3 N 4 The composite layer has a thickness of 2μm; the buffer layer is AlN and the thickness is 2μm. GaN Schottky diode SBD.
[0109] Step A: epitaxially depositing a group III nitride material on the front side of the Si substrate 2, such as Figure 4 (a).
[0110] A1) A Si substrate with a size of 6 inches, a thickness of 650 μm, and a crystal orientation of
[111] is selected;
[0111] A2) using metal organic chemical vapor deposition MOCVD technology to epitaxially grow an AlN nucleation layer 3 with a thickness of 300 nm on the front side of the Si substrate 2, wherein the process conditions are: NH 3 The flow rate ratio to TMAl is 2400, the temperature is 720°C, and the growth pressure is 190 mbar:
[0112] A3) using metal organic chemical vapor deposition MOCVD technology, epitaxially growing an AlN buffer layer 4 with a thickness of 2 μm on the AlN nucleation layer 3, the process conditions are: NH 3 The flow rate ratio to TMAl was 2500, the temperature was 700°C, and the growth pressure was 150 mbar;
[0113] A4) epitaxially growing a 300 nm thick, unintentionally doped GaN channel layer 5 on the AlN buffer layer 4 using metal organic chemical vapor deposition (MOCVD) technology, wherein the process conditions are: NH 3 The flow rate ratio to TMGa was 2400, the temperature was 1050°C, and the growth pressure was 55 mbar;
[0114] A5) using metal organic chemical vapor deposition MOCVD technology to epitaxially grow an AlGaN barrier layer 6 with an Al content of 0.25 and a thickness of 30 nm on the GaN channel layer 5, the process conditions are NH 3 The flow rate ratio of TMGa and TMAl is 2400, the flow rate ratio of TMGa and TMAl is 4, the temperature is 920℃, and the growth pressure is 55mbar.
[0115] Step B: Deposit cathode and anode metal electrodes on the surface of the barrier layer 6, and perform device isolation and deposit a passivation layer 7, such as Figure 4 (b).
[0116] B1) performing photolithography on the surface of the barrier layer 6, that is, firstly spin coating a layer of photoresist on the barrier layer 6, then sequentially performing alignment, exposure, development, and pattern detection to form the cathode region of the device, and finally bombarding the cathode region with Ar plasma for 30 seconds to reduce the contact resistance;
[0117] B2) Using electron beam evaporation E-Beam technology, Ti / Au with a thickness of 40 / 1100 nm is deposited in the cathode area as the cathode, and then the wafer is placed in a photoresist stripping solution to remove excess photoresist. The process conditions of electron beam evaporation are: the vacuum degree of the studio is 2.0×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 0.65A, and the evaporation time is 1100s;
[0118] B3) Place the above-mentioned cathode metal-deposited wafer into an annealing furnace at N 2 Rapid annealing for 60 seconds in an environment with an annealing temperature of 760°C in a furnace to form a good ohmic contact between the cathode and the barrier layer 6;
[0119] B4) The surface of the barrier layer 6 is again photolithographically processed to form an anode region. Ni / Au with a thickness of 40 / 1100 nm is deposited in the anode region by electron beam evaporation (E-Beam) to form a good Schottky contact at the contact surface between the anode and the barrier layer 6. Finally, the wafer is placed in a photoresist stripping solution to remove the photoresist. The process conditions of the electron beam evaporation (E-Beam) are: the vacuum degree of the working chamber is 2.0×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 0.65A, and the evaporation time is 1100s;
[0120] B5) Using ion implantation technology, high-energy ions are implanted into the surface of the barrier layer 6 outside the active area of the wafer to complete device isolation. The process conditions of ion implantation are as follows: the implantation energy is 320 keV and the ion concentration is 9×10 14 cm -2 ;
[0121] B6) Using atomic layer deposition ALD technology, epitaxially grow Si with a thickness of 260nm on the barrier layer 6 around the cathode and anode 3 N 4 The passivation layer 7, wherein the process conditions of atomic layer deposition ALD are: the reaction chamber temperature is 300°C, and the reaction chamber pressure is 5mbar.
[0122] Step C: Paste the surface of the passivation layer 7 to the sapphire carrier wafer 202 through a high temperature paraffin layer, and apply pressure to bond them, such as Figure 4 (c).
[0123] Step D: Making a back silver reflective layer 1 on the back of the Si substrate 2
[0124] D1) grinding and thinning the back side of the Si substrate 2 on which the device having the substrate layer 2, the nucleation layer 3, the buffer layer 4, the channel layer 5, the barrier layer 6, the passivation layer 7, and the cathode and the anode is made, so that the thickness is reduced to 200 μm;
[0125] D2) Using polishing technology, the back side of the thinned Si substrate 2 is polished to improve the smoothness and flatness of the wafer surface. Figure 4 (d);
[0126] D3) Using electron beam evaporation E-Beam technology, a metal Ag with a thickness of 12 μm is deposited on the back side of the Si substrate 2 as a back side silver reflective layer 1, as shown in FIG. Figure 4 (e).
[0127] The process conditions of electron beam evaporation E-Beam are: the working room is evacuated to 3×10 -4 Pa, the electron gun acceleration voltage is 9Kv, the electron gun beam current is 0.6A, and the evaporation time is 8000s.
[0128] Step E: Remove the carrier wafer, use photolithography to define the radiation heat dissipation layer pattern between the metal electrodes and the passivation layer 7, and grow a radiation layer on the passivation layer, such as Figure 4 (f).
[0129] E1) removing the sapphire carrier 202 bonded to the surface of the passivation layer by using a wax removal liquid;
[0130] E.2) first spin-coat a layer of photoresist on the surface of the passivation layer 7, then perform alignment, exposure, development and pattern detection, then cover the metal electrode layer with photoresist and set the radiation layer pattern;
[0131] E.3) Using plasma chemical vapor deposition (PECVD) technology, epitaxially grow multiple SiO2 layers with a thickness of 1 μm and a diameter of 40 μm along the passivation layer 7 covered with photoresist on the periphery of the anode and cathode at a spacing of 5 μm. 2The plasma chemical vapor deposition (PECVD) process conditions are as follows: the reaction chamber is maintained at a temperature of 300°C and the pressure is set to 1.3 mbar;
[0132] E.4) Using atomic layer deposition (ALD) technology, along the passivation layer 7 covering the periphery of the anode and cathode, 2 A layer with a thickness of 1 μm and a diameter of the same as SiO 2 Same Si 3 N 4 layer, wherein the process conditions of the atomic layer deposition ALD technology are the same as the process conditions of step E.3);
[0133] E.4) The columnar SiO2 deposited by the above steps E.3) and E.4) 2 / Si 3 N 4 The composite radiation layer is transferred to the surface of the passivation layer 7 .
[0134] Step F: Remove excess SiO using a stripping process 2 / Si 3 N 4 Composite layer, which will grow multiple columnar SiO 2 / Si 3 N 4 The composite radiation layer is placed in a photoresist stripping solution to remove excess SiO 2 / Si 3 N 4 Composite layer, the clock prepares the radiation cooling layer 8 on the surface of the passivation layer 7 to complete the device preparation, such as Figure 4 (g).
[0135] The above descriptions are only three specific examples of the present invention and do not constitute any limitation to the present invention. It is obvious that after understanding the content and principle of the present invention, professionals in this field may make various modifications and changes in form and details without departing from the principle and result of the present invention. 2 / Si 3 N 4 Composite layer and HfO 2 / Si 3 N 4 Composite layer, TiO 2 / Si 3 N 4 Composite layer, Al 2 O 3 / Si 3 N 4In addition to the two-layer composite structure used in this example, the radiation layer can also be composed of multiple composite layers, such as SiO 2 / Si 3 N 4 / SiO 2 / Si 3 N 4 Multilayer composite layer, or hfo2. However, these modifications and changes based on the concept of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A GaN device that uses radiation cooling to improve heat dissipation performance, comprising, from bottom to top: a substrate layer (2), a nucleation layer (3), a buffer layer (4), a channel layer (5), a barrier layer (6) and a passivation layer (7), wherein the barrier layers (6) on both sides of the passivation layer (7) are provided with source and drain electrodes, and the barrier layer between the source and drain electrodes and close to the source electrode is provided with a drain electrode, characterized in that: The substrate layer (2) has a silver reflective layer (1) on its lower surface to effectively conduct the heat generated in the device, improve the heat reflection efficiency, and enhance the heat dissipation capacity of the device; The passivation layer (7) has a plurality of upper and lower composite SiO2 / Si3N4 cylindrical structures arranged between the metal electrodes on its upper surface, forming a radiation cooling layer (8) to enhance the heat dissipation performance of the device.
2. The device according to claim 1, characterized in that: The silver reflective layer (1) is made of a high-metal silver material with a thermal conductivity of 400-450 W / mK and has a thickness of 1-20 μm.
3. The device according to claim 1, characterized in that: The radiation cooling layer (8) has each SiO2 / Si3N4 cylindrical structure composited on top and bottom, with a thickness of 1 to 15 μm and a diameter of 4 to 50 μm, and a spacing of 5 to 20 μm between adjacent cylindrical structures. The composite cylindrical structure can also be composited on top and bottom with Si3N4 using any one of aluminum oxide, hafnium oxide or titanium oxide materials.
4. The device according to claim 1, characterized in that: The substrate layer (2) is made of Si or SiC and has a thickness of 150 to 650 μm; The nucleation layer (3) is made of AlN with a thickness of 120-250 nm, and may also be made of Si, SiC or Al2O3.
5. The device according to claim 1, characterized in that: The buffer layer (4) is made of any one of GaN, AlN or AlGaN, and has a thickness of 0.1 to 5 μm; The channel layer (5) is made of GaN and has a thickness of 30 to 800 nm.
6. The device according to claim 1, characterized in that: The barrier layer (6) is made of AlGaN with a thickness of 10 to 35 nm, and may also be made of an AlGaN / AlN structure; The passivation layer (7) is made of SiO2 or Si3N4 insulating medium and is used for electrical isolation. Its thickness is 60-200nm.
7. A method for preparing a GaN device using radiative cooling to improve heat dissipation performance, comprising the following steps: S1: epitaxially depositing a nucleation layer, a buffer layer, a channel layer, and a barrier layer in sequence on the front side of the substrate by metal organic chemical vapor deposition (MOCVD); S2: Electrode metal is first deposited on the barrier layer by electron beam evaporation (E-Beam), followed by ion implantation for isolation, and then a passivation layer is deposited by atomic layer deposition (ALD); S3: connecting the upper surface of the passivation layer to an external carrier wafer through a bonding process; S4: pre-treatment of the back side of the substrate by thinning the substrate and polishing the surface; S5: depositing a metallic silver reflective layer on the back side of the pre-treated substrate by electron beam evaporation E-Beam, and removing the carrier wafer; S6: The pattern of the radiation cooling layer is set on the front side of the device by photolithography, and then SiO2 and Si3N4 are deposited by plasma enhanced chemical vapor deposition (PECVD) and atomic layer deposition (ALD) respectively to form a radiation cooling layer consisting of multiple upper and lower composite SiO2 / Si3N4 cylindrical structures; S7: Through the stripping process, the wafer with the radiation cooling layer is immersed in a photoresist stripping solution to remove excess photoresist, thereby completing the device preparation.
8. The method according to claim 7, characterized in that The process conditions of metal organic chemical vapor deposition MOCVD in step S1 are as follows: TMGa was used as Ga precursor, TMAl was used as Al precursor, H2 and N2 mixed gas was used as carrier gas, and NH3 was used as nitrogen source; The NH3 to TMAl flow rate ratio for depositing AlN is 1450-2500, the temperature is maintained at 460-750°C, and the growth pressure is maintained at 100-200 mbar; The flow rate ratio of NH3 to TMGa for depositing GaN is 1450-2500, the temperature is maintained at 900-1100°C, and the growth pressure is maintained at 50-150mbar; The flow rate ratio of NH3 to TMGa for depositing AlGaN is 1450-2500, the flow rate ratio of TMGa to TMAl is 4-20, the temperature is maintained at 900-1100°C, and the growth pressure is maintained at 50-100 mbar.
9. The method according to claim 7, characterized in that: In step S6: The plasma enhanced chemical vapor deposition PECVD process conditions are as follows: Using SiH4 and N2O as precursor gases, The flow rate of SiH4 is between 50 and 80 cm 3 / min, The flow rate of N2O is 150~200cm 3 / min; The temperature is maintained at 240-300°C, the growth pressure is maintained at 75-100 Pa, and the RF power is set to 60-100 W. The ALD process conditions are: The reaction chamber temperature is between 300 and 450°C; The pressure in the reaction chamber is 1-3 mbar.
10. The method according to claim 7, characterized in that: The process conditions of the electron beam evaporation E-Beam in step S2 are as follows: The vacuum degree of the working room is evacuated to 2.0×10 -4 Pa, The electron gun acceleration voltage is 8~10Kv, The electron gun beam current is 0.25~0.8A, Evaporation time is 80 to 220 seconds; The process conditions of the electron beam evaporation E-Beam in step S5 are as follows: The vacuum degree of the working room is evacuated to 2.5×10 -4 Pa, The electron gun acceleration voltage is 6~10Kv, The electron gun beam current is 0.25~1A, The evaporation time is 200 to 2200 seconds.
Citation Information
Patent Citations
Gallium nitride device based on diamond substrate and preparation method of gallium nitride device
CN110164766A
Gallium nitride epitaxial growth method beneficial to improving heat dissipation performance
CN114438595A
Gallium nitride device heat dissipation structure and preparation method thereof
CN115863276A
Preparation method of gallium nitride / diamond composite heat dissipation layer with low interface thermal resistance
CN116463629A
Substrate with electric conduction, heat conduction and heat dissipation effects
CN112113154A