Gallium oxide device based on radiation refrigeration layer and preparation method thereof
By adopting a radiation refrigeration layer structure in Ga2O3 devices, and using the combination of silver reflective layer and SiO2/Si3N4 cylindrical structure, the problem of insufficient heat dissipation caused by the low thermal conductivity of the device is solved, the heat dissipation performance and electrical performance are improved, and the stability of the device is enhanced Sex and reliability.
Patent Information
- Application Number
- CN202411061586.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-08-05
AI Technical Summary
The low thermal conductivity of Ga2O3 devices leads to insufficient heat dissipation in high power and high temperature environments, affecting their electron mobility and stability. The prior art has lattice defects and boundary thermal resistance problems when improving heat dissipation performance.
The design based on the radiation refrigeration layer includes the arrangement of a silver reflective layer under the substrate and the formation of a plurality of SiO2/Si3N4 cylindrical structures on the passivation layer to enhance the heat dissipation performance of the device and avoid the high thermal conductivity of the material to Ga2O3. Lattice damage.
It effectively improves the heat dissipation performance of the device, reduces thermal resistance, avoids lattice defects, improves electrical performance and reliability, simplifies the device structure, and reduces the device size and weight.
Smart Images

Figure CN118969752A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of semiconductor devices, and in particular relates to a gallium oxide device and a preparation method thereof, which can be used as a microwave power device and a power electronic device. Background Art
[0002] Ga2O3 is an ultra-wide bandgap semiconductor material. According to different crystal structures, it can be divided into α-Ga2O3, β-Ga2O3, γ-Ga2O3, δ-Ga2O3 and ε-Ga2O3. Among these different crystal structures, β-Ga2O3 is the most stable at room temperature and pressure, and has excellent chemical stability. At present, most Ga2O3 devices use β-Ga2O3. Compared with the third-generation semiconductor materials SiC and GaN, β-Ga2O3 has excellent physical properties such as an ultra-wide bandgap width of 4.8eV and an ultra-high critical breakdown field strength of 8MV / cm. In addition, Ga2O3 is the only material among wide bandgap semiconductors that can be grown in wafers by the melting method. This method can greatly reduce the cost of wafer growth. Therefore, Ga2O3 has a natural low-cost advantage and is a strong competitor in the field of future electronic devices.
[0003] As a key semiconductor material, Ga2O3 performs very well in application fields such as microwave power devices and power electronic devices. However, despite the many advantages of Ga2O3, its thermal conductivity is relatively low, only one-thirtieth of SiC and one-tenth of GaN. This low thermal conductivity limits the application of Ga2O3 in high-power and high-temperature environments. When operating at high power, the device will cause a sharp rise in temperature due to insufficient heat dissipation, which will seriously affect the device's electron mobility and stability. In addition, the thermal stress inside the device caused by high temperature can easily cause the device to fail or shorten its life. Therefore, solving the problem of low thermal conductivity of Ga2O3 is crucial to improving device performance and stability.
[0004] Patent document with application number CN202311267759.1 discloses a Ga2O3 LDMOSFET device with high efficiency heat dissipation performance and a preparation method thereof, such as Figure 1As shown, it includes from top to bottom: gate metal 8, high-K electrode insulating layer 7, source metal 6, drain gold layer 5, N channel region 4, N+ source region 3p-type lightly oxidized drift region 2 and diamond insulating layer 1, that is, a lightly doped oxidized drift layer is directly grown on a diamond substrate, and then ion implantation is performed to form source, drain and channel regions. This method directly manufactures Ga,O; devices on a diamond substrate, thereby enhancing the heat dissipation capacity of the device and improving its performance at high temperatures. However, the lattice matching degree between the oxide material and diamond is not ideal, which will lead to an increase in lattice defects in the oxide material, and its material advantages cannot be fully utilized. In addition, due to the large boundary thermal resistance between the high thermal conductivity substrate and GaO;, the heat dissipation performance of the device needs to be further improved. This method directly manufactures Ga2O3 devices on a diamond substrate, thereby enhancing the heat dissipation capacity of the device and improving its performance at high temperatures. Nevertheless, due to the large boundary thermal resistance between the high thermal conductivity substrate and Ga2O3, the heat dissipation performance of the device needs to be further improved.
[0005] Patent document with application number CN202311558965.8 discloses a double-sided heat dissipation gallium oxide chip flip-chip packaging structure and its preparation method, which uses a flip-chip packaging method to add high thermal conductivity materials on both sides of the device to help the device dissipate heat, thereby solving the device heat dissipation problem from the chip packaging perspective. However, the thermal conductivity of the thermal conductive material used in this type of packaging method is limited, and the heat dissipation effect needs to be improved.
[0006] Patent document with application number CN202311555216.X discloses a diamond-based gallium oxide semiconductor structure and its preparation method, in which a silicon carbide layer is prepared on a diamond substrate to form a diamond-silicon carbide composite structure, and the heat dissipation capacity of the gallium oxide device is enhanced by virtue of the high thermal conductivity of diamond and silicon carbide. However, considering that the gallium oxide material grows directly on the diamond-silicon carbide composite layer, due to factors such as lattice mismatch and mismatch of thermal expansion coefficient, the lattice of the gallium oxide material may have many defects, resulting in loss of electrical performance of the device. Summary of the invention
[0007] The purpose of the present invention is to address the deficiencies of the above-mentioned prior art and propose a gallium oxide 3 device based on a radiation cooling layer and a preparation method, so as to further improve the heat dissipation performance of the Ga2O3 device, avoid the loss of device electrical performance and device failure due to thermal effects, and improve the reliability of the device.
[0008] The technical solutions for achieving the purpose of the present invention include the following:
[0009] Technical solution 1:
[0010] 1. A Ga2O3 metal oxide semiconductor field effect transistor based on a radiation cooling layer, comprising from bottom to top: a substrate layer 2, a buffer layer 3, a channel layer 4 and a dielectric layer 5, wherein the dielectric layer 5 is provided with source, drain and gate metal electrodes, and the periphery of the metal electrodes is wrapped with a passivation layer 6, characterized in that:
[0011] A silver reflective layer 1 is provided on the lower surface of the substrate layer 2 to effectively conduct the heat generated in the device and improve the heat reflection efficiency;
[0012] The passivation layer 6 has a radiation cooling layer 7 composed of a plurality of SiO2 / Si3N4 cylindrical structures composited up and down, arranged between the metal electrodes on its upper surface to enhance the heat dissipation performance of the device.
[0013] Furthermore, the silver reflective layer 1 is made of a high-metal silver material with a thermal conductivity of 400-450 W / mK, and has a thickness of 1-15 μm.
[0014] Furthermore, the radiation cooling layer 7 has each SiO2 / Si3N4 cylindrical structure composited on top and bottom, with a thickness of 1 to 15 μm and a diameter of 4 to 50 μm, and a spacing of 5 to 30 μm between adjacent cylindrical structures. The composite cylindrical structure can also be composited on top and bottom with Si3N4 using any one of aluminum oxide, hafnium oxide or titanium oxide materials.
[0015] Furthermore, the substrate layer 2 is made of SiC or AlN, and its thickness is 150-600 μm; the buffer layer 3 is made of β-Ga2O3, and its thickness is 0.5-2.5 μm; the channel layer 4 is made of β-Ga2O3, and its thickness is 20-600 nm; the dielectric layer 5 is made of Al2O3, NiO, Al2O3, Hf 0.5 Zr 0.5 O2, any one of the species, with a thickness of 20 to 260 nm; the passivation layer 6 is SiO2 or Si3N4, with a thickness of 80 to 250 nm.
[0016] Technical solution 2:
[0017] A vertical Ga2O3 heterojunction diode based on a radiation cooling layer comprises, from bottom to top, a cathode electrode, an n+β-Ga2O3 substrate layer, an n-β-Ga2O3 epitaxial layer, a p-NiO dielectric layer and an anode electrode, wherein the periphery of the anode electrode is wrapped with a Si3N4 passivation layer, and is characterized in that:
[0018] A circle of multiple SiO2 / Si3N4 cylindrical structures are distributed above the passivation layer with a spacing of 10 to 20 μm between the anode metal. Each cylindrical structure is composed of a radiation cooling layer and a silver reflective layer. The spacing between two adjacent cylindrical structures is 10 to 40 microns to reflect the heat generated inside the device and improve the heat dissipation performance.
[0019] Further: the thickness of each SiO2 / Si3N4 cylindrical structure is 1-15 μm and the ring width is 10-50 μm, wherein the thickness of the silver reflective layer is 100-500 nm and is located between the Si3N4 passivation layer and the radiation cooling layer.
[0020] Furthermore, the silver reflective layer is made of high-metal silver material with a thermal conductivity of 400-450 W / mK; the composite annular structure can also be made of any one of aluminum oxide, hafnium oxide or titanium oxide materials and Si3N4 for upper and lower composite.
[0021] Furthermore, the n + The thickness of the β-Ga2O3 substrate layer is 400-650 μm, the doping element is Si or Sn, and the doping concentration is 1×10 18 ~1×10 19 cm -3 ; said n - The thickness of the β-Ga2O3 epitaxial layer is 6 to 20 μm, the doping element is Si or Sn, and the doping concentration is 1×10 15 ~1×10 17 cm -3 The thickness of the p-NiO dielectric layer is 200-600 nm, the doping element is B, and the doping concentration is 1×10 17 ~5×10 18 cm -3 ; The thickness of the Si3N4 passivation layer is 100 to 300 nm.
[0022] Technical solution 3:
[0023] A method for preparing the Ga2O3 metal oxide semiconductor field effect transistor according to claim 1, characterized in that it comprises the following steps:
[0024] S1) heterogeneously bonding a pre-prepared β-Ga2O3 wafer having a buffer layer and a channel layer to a substrate by high temperature annealing, and thinning the β-Ga2O3 wafer by ion cutting;
[0025] S2) smoothing the surface of the channel layer and epitaxially depositing a dielectric layer on the channel layer;
[0026] S3) firstly perform photolithography on the channel layer and the dielectric layer to define the pattern of the metal electrode, then deposit the electrode metal on the channel layer and the dielectric layer by electron beam evaporation E-Beam, and perform ion implantation isolation and deposit a passivation layer;
[0027] S4) connecting the upper surface of the passivation layer on which the metal electrode is deposited to an external carrier wafer through a bonding process;
[0028] S5) performing abrasive thinning and surface polishing on the back side of the substrate;
[0029] S6) depositing a silver reflective layer on the back of the polished substrate by using electron beam evaporation (E-Beam);
[0030] S7) Remove the carrier wafer, define the radiation cooling layer pattern on the passivation layer by photolithography, and then prepare the radiation cooling layer by plasma enhanced chemical vapor deposition PECVD and atomic layer deposition ALD to complete the device manufacturing.
[0031] Technical solution 4:
[0032] A method for manufacturing the vertical Ga2O3 heterojunction diode according to claim 6, characterized in that it comprises the following steps:
[0033] 1) Set n + The β-Ga2O3 substrate was first cleaned by organic ultrasonic cleaning and then dried in a N2 environment;
[0034] 2) In n + Epitaxial deposition of n on β-Ga2O3 substrate by metal organic chemical vapor deposition MOCVD - β-Ga2O3 epitaxial layer;
[0035] 3) In n - A p-NiO dielectric layer is deposited on the β-Ga2O3 epitaxial layer by magnetron sputtering technology;
[0036] 4) In n + The cathode electrode is deposited on the back of the β-Ga2O3 substrate by electron beam evaporation E-beam, and then rapidly annealed to obtain a good ohmic contact;
[0037] 5) forming an anode electrode region on the p-NiO dielectric layer by a photolithography development process, and then depositing the anode electrode by electron beam evaporation E-beam;
[0038] 6) depositing a Si3N4 passivation layer on the periphery of the anode electrode by atomic layer deposition ALD;
[0039] 7) defining a silver reflective layer pattern on the passivation layer by photolithography, and depositing the silver reflective layer by electron beam evaporation E-Beam technology;
[0040] 8) On the Si3N4 passivation layer prepared with the silver reflective layer, a radiation cooling layer pattern consistent with the silver reflective layer is defined by photolithography, and SiO2 / Si3N4 composite layers are prepared by plasma enhanced chemical vapor deposition (PECVD) and atomic layer deposition (ALD) respectively to complete the device manufacturing.
[0041] Compared with the prior art, the present invention has the following advantages:
[0042] 1) Technical solution 2 of the present invention can absorb the heat inside the device because a radiation cooling layer is prepared on the passivation layer. There is no need to add an additional water pump to achieve water circulation like a microchannel, and there is no need to contact the conductive channel material. It can efficiently radiate heat to the outside of the device, and can absorb and reflect the heat generated by the device through multiple layers of radiation materials, effectively reflecting the heat generated by the device to the external environment, thereby improving the heat dissipation performance of the device.
[0043] 2) Since a silver reflective layer is prepared under the substrate, technical solution 1 of the present invention can reflect part of the heat to the surface radiation cooling layer, thereby improving the heat reflection efficiency. At the same time, metallic silver has good thermal conductivity, which can help reflect heat while improving the thermal conductivity of the substrate, further improving the heat dissipation performance of the device.
[0044] 3) In technical solution 2 of the present invention, a radiation cooling layer is prepared around the anode of the gallium oxide Schottky diode, and a silver reflective layer is prepared directly below the radiation cooling layer, which greatly improves the thermal conductivity of the device surface and increases the speed at which the heat inside the device is radiated to the outside.
[0045] 3) The radiation cooling layer of the present invention adopts a cylindrical structure of multiple upper and lower composite SiO2 / Si3N4, and does not need to be in direct contact with the Ga2O3 epitaxial layer. It not only has no effect on the quality of the epitaxial layer, but can more effectively reduce the thermal resistance of the device, and can effectively avoid the lattice mismatch and damage of the Ga2O3 material caused by the high thermal conductivity material, and can greatly improve the heat dissipation performance of the device while achieving excellent electrical performance.
[0046] 4) Since the present invention integrates the radiation cooling layer directly on the front side of the device, a shorter heat transfer path is achieved, the overall heat dissipation efficiency of the device is improved, and the device integration is convenient, which helps to reduce the size and weight of the equipment. At the same time, the process complexity of the device is reduced, and the reliability, stability and overall electrical performance of the device are improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] Figure 1 This is the structure diagram of the existing Ga,O;LDMOSFET device;
[0048] Figure 2 It is a structural schematic diagram of a device of technical solution 1 of the present invention;
[0049] Figure 3 It is a structural schematic diagram of a device of technical solution 2 of the present invention;
[0050] Figure 4 It is a schematic diagram of the manufacturing process flow of the device of technical solution 1 of the present invention;
[0051] Figure 5 It is a schematic diagram of the manufacturing process flow of the device of technical solution 2 of the present invention. DETAILED DESCRIPTION
[0052] The Ga2O3 metal oxide semiconductor based on the radiation cooling layer of the present invention includes a Ga2O3 metal oxide semiconductor field effect transistor, a vertical Ga2O3 heterojunction diode and their respective manufacturing methods. The following is a further detailed description of the two device structures and their manufacturing methods of the present invention in combination with the accompanying drawings and embodiments.
[0053] Reference Figure 2 The Ga2O3 metal oxide semiconductor field effect transistor based on the radiation cooling layer of the present invention comprises a silver reflection layer 1, a substrate layer 2, a buffer layer 3, a channel layer 4, a dielectric layer 5, a passivation layer 6, a radiation cooling layer 7, and a source electrode S, a drain electrode D, and a gate electrode G. Among them:
[0054] The substrate layer 2 is made of SiC or AlN, and has a thickness of 200-650 μm.
[0055] The buffer layer 3 is made of β-Ga2O3 and has a thickness of 0.3-2.5 μm. It is located on the substrate layer 2 .
[0056] The channel layer 4 is made of β-Ga2O3 and has a thickness of 20-600 nm. It is located on the buffer layer 3 .
[0057] The dielectric layer 5 is made of Al2O3 or NiO or Al2O3 and Hf 0.5 Zr 0.5 O2 has a thickness of 20 to 200 nm and is located on the channel layer 4 .
[0058] The source electrode S and the drain electrode D are made of Ti / Au with a thickness of 20-60 / 80-2000 nm, and are located on the channel layer 4;
[0059] The gate G is made of Ni / Au with a thickness of 20-60 / 60-2000 nm and is located on the dielectric layer 5 between the source S and the drain D.
[0060] The passivation layer 6 is made of SiO2 or Si3N4, with a thickness of 80-200 nm, and is wrapped around the source S, drain D, and gate G.
[0061] The silver reflective layer 1 is located below the substrate layer 2 and has a thickness of 0.1 to 15 μm;
[0062] The radiation cooling layer is formed by a plurality of SiO2 / Si3N4 cylindrical structures composited up and down and arranged at a spacing of 5 to 30 μm to enhance the heat dissipation performance of the device. Each SiO2 / Si3N4 cylindrical structure composited up and down has a thickness of 1 to 15 μm and a diameter of 4 to 50 μm. The composite cylindrical structure can also be composited up and down with Si3N4 using any one of aluminum oxide, hafnium oxide or titanium oxide materials, and is located on the upper surface of the passivation layer.
[0063] Reference Figure 3 The vertical Ga2O3 heterojunction diode based on the radiation cooling layer of the present invention comprises a cathode electrode 1, n + β-Ga2O3 substrate layer 2, n - β-Ga2O3 epitaxial layer 3, p-NiO dielectric layer 4, anode electrode 5, Si3N4 passivation layer 6, silver reflection layer 7 and radiation cooling layer 8, wherein:
[0064] The + The β-Ga2O3 substrate layer 1 has a thickness of 400 to 600 μm.
[0065] The cathode electrode 2 is made of Ti / Au and has a thickness of 20-60 / 80-300 nm. + Back side of β-Ga2O3 substrate layer.
[0066] The - β-Ga2O3 epitaxial layer 3, with a thickness of 6 to 20 μm, is located at n + On top of the β-Ga2O3 substrate layer.
[0067] The p-NiO dielectric layer 4 has a thickness of 300-600 nm and is located at n - On top of the β-Ga2O3 epitaxial layer.
[0068] The anode electrode 5 is made of Ni / Au, has a thickness of 20-60 / 60-2000 nm, and is located on the p-NiO dielectric layer.
[0069] The Si3N4 passivation layer has a thickness of 100-300 nm and wraps around the periphery of the anode electrode.
[0070] The silver reflective layer 7 is made of high metallic silver material with a thermal conductivity of 400-450 W / mK. It is composed of a plurality of silver reflective cylinders distributed in a circle on the upper part of the Si3N4 passivation layer. The thickness of each silver reflective cylinder is 100-500 nm, the diameter is 4-50 μm, the spacing between it and the anode electrode is 10-20 μm, and the spacing between adjacent silver reflective cylinders is 20-50 μm.
[0071] The radiation cooling layer 8 is composed of a plurality of SiO2 / Si3N4 radiation cooling cylinders composited up and down, each radiation cooling SiO2 / Si3N4 cylinder has a thickness of 1 to 20 μm and a diameter the same as that of the silver reflective cylinder, and is located on the upper part of the silver reflective cylinder. In addition to using a composite layer of silicon dioxide and silicon nitride, the radiation cooling composite cylindrical structure can also use any one of aluminum oxide, hafnium oxide or titanium oxide materials to composite with Si3N4 up and down.
[0072] Reference Figure 4 The present invention provides three embodiments of manufacturing Ga2O3 metal oxide semiconductor field effect transistors that use radiative cooling to improve heat dissipation performance, but the embodiments of the present invention are not limited thereto. The experimental methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials described can be obtained from commercial sources unless otherwise specified.
[0073] In the first embodiment, a silver reflective layer with a thickness of 10 μm and a thermal conductivity of 426 W / mK is manufactured on a SiC substrate; the radiation cooling layer is a SiO2 / Si3N4 composite layer with a thickness of 1.5 μm, and the dielectric layer is a Ga2O3 metal oxide semiconductor field effect transistor with a thickness of 20 nm of Al2O3.
[0074] Step 1: heterogeneously bond the pre-prepared β-Ga2O3 wafer with the buffer layer 5 and the channel layer 6 to the substrate 2 by high temperature annealing, and thin the β-Ga2O3 wafer by ion cutting, such as Figure 4 (a).
[0075] 1.1) A series of organic ultrasonic cleanings were performed on the SiC substrate 2 with a thickness of 500 μm, first using acetone for 10 minutes, then using isopropanol for 10 minutes, and finally using deionized water for 5 minutes. During the entire cleaning process, the ultrasonic power was maintained at 120 W. After the cleaning was completed, the surface of the SiC substrate 2 was blown dry with nitrogen;
[0076] 1.2) A pre-prepared β-Ga2O3 wafer was selected, the structure of which includes an unintentionally doped β-Ga2O3 buffer layer 3 with a thickness of 0.8 μm and a 500 μm thick β-Ga2O3 layer with a doping concentration of 2×10 17 cm -3The β-Ga2O3 channel layer 4 is formed by performing H ion implantation on one side of the buffer layer 3 of the β-Ga2O3 wafer to form a defect in the β-Ga2O3 wafer at a distance of 1.5 μm from the surface of the buffer layer 3;
[0077] 1.3) The front side of the SiC substrate 2 is subjected to Ar ion bombardment treatment for 1 min to form an amorphous layer, and then the front side of the SiC substrate 2 and one side of the β-Ga2O3 wafer buffer layer 3 are subjected to high-temperature annealing bonding in a vacuum at a temperature of 800° C. for 45 s;
[0078] 1.4) The annealed wafer is annealed again at a temperature of 800°C in a N2 environment for 30 minutes to remove the β-Ga2O3 wafer from the defects and leave a buffer layer 3 with a thickness of 0.8 μm and a channel layer 4 with a thickness of 0.7 μm on the surface of the SiC substrate 2.
[0079] Step 2: Smooth the surface of the channel layer 4 and epitaxially grow a dielectric layer 5 on the channel layer 4, such as Figure 4 (b).
[0080] 2.1) using chemical mechanical polishing (CMP) technology to grind and polish the surface of the channel layer 4 to reduce the thickness of the channel layer 4 to 0.3 μm;
[0081] 2.2) Atomic layer deposition (ALD) technology is used to deposit an Al2O3 dielectric layer 5 with a thickness of 25 nm on the channel layer 4 under process conditions of a reaction chamber temperature of 325°C and a pressure of 1.5 mbar.
[0082] Step 3: Deposit source S, drain D and gate G metal on the channel layer 4 and dielectric layer 5 respectively, and perform ion implantation to achieve isolation, and deposit a passivation layer 8, such as Figure 4 (c).
[0083] 3.1) Photolithography is performed on the surface of the dielectric layer 5. First, a layer of photoresist is spin-coated on the surface of the dielectric layer 5, and then alignment, exposure, development, and pattern detection are performed in sequence to form an active region from the source S to the drain D of the device;
[0084] 3.2) Using inductively coupled plasma etching (ICP) technology to etch the dielectric layer 5 outside the active area, it is necessary to etch to the channel layer 4, and then put the wafer into a photoresist stripping solution for stripping to remove the photoresist;
[0085] 3.3) The surface of the channel layer 4 is patterned by photolithography to form the source and drain regions, and the channel layer 4 between the source and drain regions is doped by ion implantation to reduce the resistance of the source and drain regions. The doping element is Si, and the doping concentration is 6×10 18 cm -3;
[0086] 3.4) Through electron beam evaporation E-Beam, the vacuum in the working room is evacuated to 2.0×10 -4 Under the process conditions of 9KV electron gun acceleration voltage, 0.3A electron gun beam current and 1200s evaporation time, Ti / Au with a thickness of 50 / 1500nm is deposited in the source and drain regions as the source S and drain D, and then the wafer with evaporated metal is placed in a photoresist stripping solution to remove the photoresist;
[0087] 3.5) Performing a rapid thermal annealing treatment on the wafer after the metal deposition of the source S and the drain D, annealing in a N2 environment for 60s at a temperature of 850°C, so as to form a good ohmic contact at the contact surface of the source, drain and channel layer 4;
[0088] 3.6) The surface of the dielectric layer 5 is again photolithographically formed into a gate region, and the vacuum is evacuated to 2.0×10 -4 Under the process conditions of 1000 s, 40 / 1200 nm thick Ni / Au is deposited in the gate region as the gate G, so as to form a Schottky contact between the gate G and the dielectric layer 5, and then the wafer is placed in a photoresist stripping solution to remove the photoresist;
[0089] 3.7) Using ion implantation technology, the implantation energy is 320keV and the ion concentration is 1×10 15 cm -2 Under the process conditions, high-energy ion implantation is performed on the surface of the channel layer 4 outside the active area of the wafer to complete device isolation;
[0090] 3.8) Under the conditions of the reaction chamber temperature set to 300° C. and the pressure set to 2.6 mbar, an Si3N4 passivation layer 6 with a thickness of 100 nanometers is epitaxially grown on the channel layer 4 and the dielectric layer 5 around the source S, drain D, and gate G using atomic layer deposition (ALD) technology.
[0091] Step 4: Paste the surface of the passivation layer 6 to the sapphire carrier wafer 202 through the high-temperature paraffin layer 201, and apply pressure to bond them, such as Figure 4 (d).
[0092] Step 5: Process the back side of the SiC substrate 2, such as Figure 4 (e).
[0093] 5.1) The SiC substrate 2 of the device having the substrate layer 2, the buffer layer 3, the channel layer 4, the dielectric layer 5, the passivation layer 6, the source electrode S, the drain electrode D, and the gate electrode G is thinned to reduce the thickness to 200 μm;
[0094] 5.2) The thinned SiC substrate 2 is polished on the back side using polishing technology to improve the smoothness and flatness of the wafer surface.
[0095] Step 6: Prepare a silver reflective layer on the back of the substrate. Figure 4 (f).
[0096] The chamber was evacuated to a vacuum of 3 × 10 -4 Under the process conditions of 9KV electron gun acceleration voltage, 0.6A electron gun beam current and 5000s evaporation time, a 10μm thick metal Ag is deposited on the back of the Si substrate 2 as the back silver reflective layer 1.
[0097] Step 7: Remove the carrier wafer, define the radiation heat dissipation layer pattern on the passivation layer 6 and between the metal electrodes using a photolithography process, protect the metal electrodes by covering the metal electrodes with photoresist 301, and then grow the radiation cooling layer material, such as Figure 4 (g).
[0098] 7.1) Use wax removal liquid to remove the sapphire carrier 202 bonded to the surface of the passivation layer.
[0099] 7.2) First, a layer of photoresist is spin-coated on the surface of the passivation layer 6, and then alignment, exposure, development and pattern detection are performed, the metal electrode layer is covered with photoresist, and the pattern of the radiation layer 7 is defined.
[0100] 7.3) According to the defined radiation layer pattern, using plasma chemical vapor deposition (PECVD) technology, while maintaining a temperature of 300°C and a pressure of 1.3 mbar in the reaction chamber, a plurality of SiO2 layers with a thickness of 0.75 μm and a diameter of 12 μm are epitaxially grown along the passivation layer 6 around the source S, drain D and gate G covered with photoresist at a spacing of 12 μm.
[0101] 7.4) Using atomic layer deposition (ALD) technology, while maintaining a temperature of 300°C and a pressure of 1.3 mbar in a reaction chamber, a Si3N4 layer with a thickness of 0.75 μm and a diameter of 12 μm is epitaxially grown on each passivation layer 6 along the passivation layer 6 covered with a photoresist source S, a drain D and a gate G, to form a plurality of columnar SiO2 / Si3N4 radiation layers, which are then transferred to the surface of the passivation layer 6.
[0102] Step 8: Use a stripping process to remove the excess SiO2 / Si3N4 composite layer to form a radiation cooling layer 7, such as Figure 4 (h).
[0103] The wafer with the radiation layer 7 is placed in a photoresist stripping solution for stripping to remove the excess SiO2 / Si3N4 composite layer, thereby forming a radiation cooling layer 7 with a structure of multiple composite columnar radiation layers. The device preparation is now complete.
[0104] In the second embodiment, a silver reflective layer with a thickness of 12 μm and a thermal conductivity of 428 W / mK is made on an AlN substrate; the radiation cooling layer is a HfO2 / Si3N4 composite layer with a thickness of 2 μm, the dielectric layer is 100 nm NiO, and a Ga2O3 metal oxide semiconductor field effect transistor with a heterojunction is provided.
[0105] Step 1: heterogeneously bond the pre-prepared β-Ga2O3 wafer with the buffer layer 3 and the channel layer 4 to the substrate 2 by high temperature annealing, and thin the β-Ga2O3 wafer by ion cutting, such as Figure 4 (a).
[0106] A series of organic ultrasonic cleanings were performed on the AlN substrate 2 with a thickness of 500 μm, first using acetone for 10 minutes, then using isopropanol for 10 minutes, and finally using deionized water for 5 minutes. During the entire cleaning process, the ultrasonic power was maintained at 120 W. After the cleaning was completed, the surface of the AlN substrate 2 was blown dry using nitrogen (N2);
[0107] A pre-prepared β-Ga2O3 wafer was selected, which had a structure including an unintentionally doped β-Ga2O3 buffer layer 3 with a thickness of 0.8 μm and a 500 μm thick β-Ga2O3 layer with a doping concentration of 2×10 17 cm -3 The β-Ga2O3 channel layer 4 is formed by performing H ion implantation on one side of the buffer layer 3 of the β-Ga2O3 wafer to form a defect in the β-Ga2O3 wafer at a distance of 1.5 μm from the surface of the buffer layer 3;
[0108] The front side of the AlN substrate 2 is subjected to Ar ion bombardment treatment for 1 minute to form an amorphous layer, and then the front side of the AlN substrate 2 and one side of the β-Ga2O3 wafer buffer layer 3 are subjected to high-temperature annealing bonding in vacuum at a temperature of 800°C for 60 seconds;
[0109] The annealed wafer is annealed again at a temperature of 500°C in a N2 environment for 120 minutes to remove the β-Ga2O3 wafer from the defects and leave a buffer layer 3 with a thickness of 0.6μm and a channel layer 4 with a thickness of 0.5μm on the surface of the AlN substrate 2.
[0110] Step 2: Smooth the surface of the channel layer 4 and epitaxially grow a dielectric layer 5 on the channel layer 4, such as Figure 4 (b).
[0111] The vacuum degree of the deposition chamber was set to 5.6×10 -4 Pa, a growth pressure of 1.5 Pa, and a sputtering power of 26 W. A p-type NiO dielectric layer 5 with a thickness of 100 nm is deposited on the channel layer 4 by magnetron sputtering technology. The doping concentration is 1×10 18 cm -3 .
[0112] The surface of the channel layer 4 is ground and polished by using a chemical mechanical polishing (CMP) technique to reduce the thickness of the channel layer 4 to 0.2 μm.
[0113] Step 3: Deposit source S, drain D and gate G metal on the channel layer 4 and dielectric layer 5 respectively, perform ion implantation isolation, and deposit a passivation layer 6, such as Figure 4 (c).
[0114] The surface of the dielectric layer 5 is photolithographically processed. First, a layer of photoresist is spin-coated on the dielectric layer 5, and then alignment, exposure, development, and pattern detection are performed in sequence to form an active region from the source S to the drain D of the device;
[0115] The dielectric layer 5 outside the active area is etched using an inductively coupled plasma etching (ICP) technique until the channel layer 4 is exposed. After the etching is completed, a photoresist stripping solution is used to remove the photoresist.
[0116] Photolithography is performed on the surface of the channel layer 4 to form source and drain regions. Subsequently, these source and drain regions are doped by ion implantation to reduce the resistance of these regions. The element used in the doping process is Si, and the doping concentration is 5×10 18 cm -3 ;
[0117] The vacuum degree of the working chamber was set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 8Kv, the electron gun beam current is 0.6A, and the evaporation time is 1500s. Through electron beam evaporation E-Beam, Ti / Au with a thickness of 40 / 1500nm is deposited in the source and drain regions as the source S and drain D. After the metal deposition is completed, the excess photoresist and metal are removed using a photoresist stripping solution;
[0118] The wafer after the metal deposition of the source electrode S and the drain electrode D is placed in an annealing furnace and rapidly annealed in a N2 environment for 60 seconds at a temperature of 800° C. to form a good ohmic contact at the contact surface of the source electrode, the drain electrode and the channel layer 4;
[0119] The surface of the dielectric layer 5 is subjected to secondary photolithography to form a gate region, and the vacuum degree of the working chamber is set to 2.0×10 -4Pa, the electron gun acceleration voltage is 9Kv, the electron gun beam current is 0.6A, and the evaporation time is 1200s. Through electron beam evaporation E-Beam, Ni / Au with a thickness of 50 / 1500nm is deposited in the gate area as the gate G, so as to form a good Schottky contact at the contact surface of the gate G and the dielectric layer 5. After the metal deposition is completed, the photoresist stripping liquid is used for degumming.
[0120] A second photolithography is performed on the surface of the dielectric layer 5 to form a gate region; and the vacuum degree of the working chamber is set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 9kV, the electron gun beam current is 0.6A, and the evaporation time is 1200 seconds. A 50 / 1500nm Ni / Au metal layer is deposited in the gate area by electron beam evaporation E-Beam technology as the gate G, so as to form a good Schottky contact between the gate G and the dielectric layer 5. After the metal deposition is completed, a photoresist stripping solution is used to remove the residual photoresist;
[0121] The implantation energy was set to 320 keV and the ion concentration was set to 1×10 15 cm -2 Under the process conditions, ion implantation technology is used to implant high-energy ions into the surface of the channel layer 4 outside the active area of the wafer to complete device isolation;
[0122] The reaction chamber temperature is set to 400° C. and the pressure is set to 3 mbar. A SiO2 passivation layer 6 with a thickness of 140 nm is epitaxially grown on the channel layer 4 and the dielectric layer 5 around the source S, drain D, and gate G using atomic layer deposition ALD technology.
[0123] Step 4: Paste the surface of the passivation layer 6 to the sapphire carrier wafer 202 through the high-temperature paraffin layer 201, and apply pressure to bond them, such as Figure 4 (d).
[0124] Step 5: Process the back side of the AlN substrate 2, such as Figure 4 (e).
[0125] The back side of the AlN substrate 2 of the device including the substrate layer 2, the buffer layer 3, the channel layer 4, the dielectric layer 5, the passivation layer 6, the source electrode S, the drain electrode D and the gate electrode G is ground and thinned to reduce the thickness to 300 μm;
[0126] The back side of the thinned AlN substrate 2 is polished by using a polishing technique to improve the smoothness and flatness of the wafer surface.
[0127] Step 6: Deposit a silver reflective layer 1 on the back of the substrate 2, such as Figure 4 (f).
[0128] The working chamber was evacuated to 3 × 10 -4 Pa, set the process conditions of electron gun acceleration voltage to 9Kv, electron gun beam current to 0.6A, and evaporation time to 6000s, and deposit metal Ag with a thickness of 12μm on the back side of the Si substrate 2 as the back silver reflective layer 1 through electron beam evaporation E-Beam.
[0129] Step 7: Remove the carrier wafer, define the radiation heat dissipation layer pattern on the passivation layer 6 and between the metal electrodes using a photolithography process, protect the metal electrodes by covering the metal electrodes with photoresist 301, and then grow the radiation cooling layer material, such as Figure 4 (g).
[0130] The sapphire carrier 202 bonded to the surface of the passivation layer is removed by using a wax removal liquid.
[0131] First, a layer of photoresist is spin-coated on the surface of the passivation layer 6 , and then alignment, exposure, development and pattern detection are performed, the metal electrode layer is covered with the photoresist, and the pattern of the radiation layer 7 is defined.
[0132] The process conditions of the reaction chamber temperature being 300° C. and the pressure being 1.3 mbar were set, and a plurality of HfO2 layers with a thickness of 1 μm and a diameter of 20 μm were epitaxially grown along the passivation layer 6 around the source S, the drain D and the gate G covered with photoresist at a spacing of 15 μm by using the plasma chemical vapor deposition PECVD technology;
[0133] The reaction chamber temperature was set to 300°C and the pressure was set to 1.3 mbar. ALD technology was used to epitaxially grow a Si3N4 layer with a thickness of 1 μm and a diameter of 20 μm on each HfO2 layer along the passivation layer 6 covered with the photoresist source S, drain D and gate G, to form multiple HfO2 / Si3N4 composite column material layers.
[0134] Step 8: Use a stripping process to remove the excess SiO2 / Si3N4 composite layer to form a radiation cooling layer 8, such as Figure 4 (h).
[0135] The wafer with the radiation layer 7 is placed in a photoresist stripping solution for stripping to remove the excess SiO2 / Si3N4 composite layer, and a radiation layer cooling 7 is formed on the surface of the passivation layer 6, thereby completing the device preparation.
[0136] Example 3: A silver reflective layer with a thickness of 2 μm and a thermal conductivity of 429 W / mK is made on a SiC substrate; a radiation cooling layer is a SiO2 / Si3N4 composite layer with a thickness of 1.2 μm, and a dielectric layer is an Al2O3 layer with a thickness of 10 nm and a Hf 0.5 Zr 0.5Ga2O3 metal oxide semiconductor field effect transistor with O2 thickness of 20nm.
[0137] Step A: heterogeneously bond the β-Ga2O3 wafer having the buffer layer 3 and the channel layer 4 to the substrate 2 by high temperature annealing, and thin the β-Ga2O3 wafer by ion cutting, such as Figure 4 (a).
[0138] A1) A series of organic ultrasonic cleanings were performed on a SiC substrate 2 with a thickness of 500 μm, first using acetone for 10 minutes, then using isopropanol for 10 minutes, and finally using deionized water for 5 minutes. During the entire cleaning process, the ultrasonic power was maintained at 120 W. After the cleaning was completed, the surface of the SiC substrate 2 was blown dry with nitrogen;
[0139] A2) A pre-prepared β-Ga2O3 wafer is selected, the structure of which includes an unintentionally doped β-Ga2O3 buffer layer 3 with a thickness of 0.8 μm and a 500 μm thick β-Ga2O3 layer with a doping concentration of 2×10 17 cm -3 The β-Ga2O3 channel layer 4 is formed by performing H ion implantation on one side of the buffer layer 3 of the β-Ga2O3 wafer to form a defect in the β-Ga2O3 wafer at a distance of 1.5 μm from the surface of the buffer layer 3;
[0140] A3) performing Ar ion bombardment treatment on the front side of the SiC substrate 2 for 1 min to form an amorphous layer, and then performing high-temperature annealing bonding on the front side of the SiC substrate 2 and one side of the β-Ga2O3 wafer buffer layer 3 in a vacuum at a temperature of 800° C. for 45 s;
[0141] A4) The annealed wafer is annealed again at a temperature of 800°C in a N2 environment for 30 minutes to remove the β-Ga2O3 wafer from the defects and leave a buffer layer 3 with a thickness of 0.8μm and a channel layer 4 with a thickness of 0.7μm on the surface of the SiC substrate 2.
[0142] Step B: Smooth the surface of the channel layer 4 and epitaxially grow a dielectric layer 5 on the channel layer 4. Figure 4 (b).
[0143] B1) using chemical mechanical polishing (CMP) technology to grind and polish the surface of the channel layer 4 to reduce the thickness of the channel layer 4 from 0.7 μm to 0.35 μm;
[0144] B2) Using atomic layer deposition ALD technology, Al2O3 with a thickness of 10nm and Hf with a thickness of 20nm are deposited on the channel layer 4 in sequence. 0.5 Zr 0.5O2 is used as the dielectric layer 5, wherein the process conditions of atomic layer deposition ALD are:
[0145] The process conditions of atomic layer deposition ALD for depositing Al2O3 are: reaction chamber temperature of 360°C and reaction chamber pressure of 1.7 mbar;
[0146] Deposition of Hf 0.5 Zr 0.5 The process conditions of atomic layer deposition ALD of O2 are: reaction chamber temperature is 260°C and reaction chamber pressure is 2.7 mbar.
[0147] Step C: Deposit source S, drain D and gate G metal on the channel layer 4 and dielectric layer 5 respectively for ion implantation isolation, and deposit a passivation layer 6, such as Figure 4 (c).
[0148] C1) performing photolithography on the surface of the dielectric layer 5, that is, firstly spin coating a layer of photoresist on the dielectric layer 5, and then sequentially performing alignment, exposure, development, and pattern detection to form an active region from the source S to the drain D of the device;
[0149] C2) using inductively coupled plasma etching (ICP) technology to etch the dielectric layer 5 outside the active area, the etching depth is required to etch to the channel layer 4, and after the etching is completed, a photoresist stripping solution is used for de-bonding treatment;
[0150] C3) The surface of the channel layer 4 is photolithographically formed into source and drain regions, and ion implantation is performed on the channel layer 4 in the source and drain regions to reduce the resistance of the source and drain regions. The doping element is Si, and the doping concentration is 4×10 18 cm -3 ;
[0151] C4) Ti / Au with a thickness of 50 / 1500 nm is deposited in the source and drain regions as the source S and drain D by electron beam evaporation E-Beam. After the metal deposition is completed, the wafer is placed in a photoresist stripping solution to remove excess photoresist. The process conditions of electron beam evaporation E-Beam are as follows:
[0152] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0153] The electron gun acceleration voltage is 9Kv.
[0154] The electron gun beam current is 0.7A.
[0155] The evaporation time is 1000s;
[0156] C5) placing the wafer after the source and drain metal deposition in a rapid thermal annealing furnace, and rapidly annealing for 60 seconds in a N2 environment at a temperature of 750° C., so as to form a good ohmic contact at the contact surface of the source, drain and channel layer 4;
[0157] C6) The surface of the dielectric layer 5 is again photolithographically formed into a gate region, and Ni / Au with a thickness of 40 / 1500 nm is deposited in the gate region as a gate G by electron beam evaporation E-Beam, so as to form a Schottky contact at the contact surface between the gate G and the dielectric layer 5, and then the wafer is placed in a photoresist stripping solution to remove the photoresist, wherein the process conditions of the electron beam evaporation E-Beam are as follows:
[0158] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0159] The electron gun acceleration voltage is 8Kv.
[0160] The electron gun beam current is 0.7A.
[0161] The evaporation time is 1000s;
[0162] C7) Using ion implantation technology, high-energy ions are implanted into the surface of the channel layer 4 outside the active area of the wafer to complete device isolation, wherein the process conditions of ion implantation are as follows:
[0163] The injection energy is 330keV,
[0164] The ion concentration is 1×10 15 cm -2 ;
[0165] C8) Atomic layer deposition (ALD) technology is used to epitaxially grow a SiO2 passivation layer 6 with a thickness of 180 nm on the channel layer 4 and the dielectric layer 5 around the source S, the drain D, and the gate G, wherein the process conditions of the atomic layer deposition (ALD) are as follows:
[0166] The reaction chamber temperature is 360°C.
[0167] The reaction chamber pressure was 3.5 mbar.
[0168] Step D: Paste the surface of the passivation layer 6 to the sapphire carrier wafer 202 through the high temperature paraffin layer 201, and apply pressure to bond them, such as Figure 4 (d).
[0169] Step E: Process the back side of the SiC substrate 2, such as Figure 4 (e).
[0170] E1) grinding and thinning the back side of the SiC substrate 2 of the device having the substrate layer 2, the buffer layer 3, the channel layer 4, the dielectric layer 5, the passivation layer 6, the source electrode S, the drain electrode D, and the gate electrode G, so that the thickness is reduced to 260 μm;
[0171] E2) The back side of the thinned SiC substrate 2 is polished by using a polishing technique to improve the smoothness and flatness of the wafer surface.
[0172] Step F: Prepare a silver reflective layer on the back of the substrate. Figure 4 (f).
[0173] By electron beam evaporation E-Beam, metal Ag with a thickness of 2 μm is deposited on the back side of the Si substrate 2 as the back side silver reflective layer 1 , wherein the process conditions of the electron beam evaporation E-Beam are as follows.
[0174] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0175] The electron gun acceleration voltage is 8Kv.
[0176] The electron gun beam current is 0.7A.
[0177] The evaporation time is 1000s.
[0178] Step G: Remove the carrier wafer, define the radiation heat dissipation layer pattern on the passivation layer 6 and between the metal electrodes using a photolithography process, protect the metal electrodes by covering the metal electrodes with photoresist 301, and then grow the radiation cooling layer material, such as Figure 4 (g).
[0179] G1) removing the sapphire carrier 202 bonded to the surface of the passivation layer by using a wax removal liquid;
[0180] G2) first spin-coating a layer of photoresist on the surface of the passivation layer 6, then performing alignment, exposure, development and pattern detection, covering the metal electrode layer with the photoresist, and defining the pattern of the radiation layer 7;
[0181] G3) Using plasma enhanced chemical vapor deposition (PECVD) technology, along the passivation layer 6 on the periphery of the source S, drain D and gate G covered with photoresist, multiple SiO2 layers with a thickness of 0.6 μm and a diameter of 45 μm are epitaxially grown at a spacing of 5 μm, wherein the process parameters of the plasma enhanced chemical vapor deposition (PECVD) technology are as follows:
[0182] SiH4 and N2O are precursor gases;
[0183] The flow rate is 80cm 3 / min、160cm 3 / min;
[0184] The reaction chamber is maintained at 300°C;
[0185] The reaction chamber pressure is 1.3 mbar;
[0186] The RF power is 100W;
[0187] Sedimentation time 750 s;
[0188] G4) Using atomic layer deposition ALD technology, along the passivation layer 6 covered with the photoresist source S, drain D and the periphery of the gate G, multiple Si3N4 layers with a thickness of 0.6 μm and a diameter of 45 μm are epitaxially grown at a spacing of 5 μm, wherein the process parameters of the atomic layer deposition ALD technology are:
[0189] The reaction chamber temperature is 360°C;
[0190] The reaction chamber pressure is 3.5 mbar;
[0191] The deposition time was 750 s.
[0192] Step H: Remove the excess SiO2 / Si3N4 composite layer by stripping process to form a radiation cooling layer 7, such as Figure 4 (h).
[0193] The wafer with the radiation layer 7 is placed in a photoresist stripping solution for stripping to remove the excess SiO2 / Si3N4 composite layer, forming a radiation cooling layer, and completing the device preparation.
[0194] Reference Figure 5 The present invention provides the following three embodiments for making a vertical Ga2O3 heterojunction diode based on a radiation cooling layer, but the embodiments of the present invention are not limited thereto. The experimental methods described in the following embodiments are conventional methods unless otherwise specified; the reagents and materials described are commercially available unless otherwise specified.
[0195] Example 4: A vertical Ga2O3 heterojunction diode is manufactured, wherein the silver reflective layer has a thickness of 100 nm and a thermal conductivity of 425 W / mK; and the radiation cooling layer is a SiO2 / Si3N4 composite layer with a thickness of 1.5 μm.
[0196] Step 1: Clean the substrate, such as Figure 5 (a).
[0197] The thickness is 500 μm and the Si doping concentration is 5×10 18 cm -3 n +The β-Ga2O3 substrate was first ultrasonically cleaned in acetone solution for 10 minutes, then ultrasonically cleaned in isopropanol solution for 10 minutes, and finally ultrasonically cleaned in deionized water for 10 minutes with an ultrasonic power of 100 W. After cleaning, the substrate surface was blown dry with N2.
[0198] Step 2: Deposition of epitaxial layers, such as Figure 5 (b).
[0199] Using metal organic chemical vapor deposition (MOCVD) technology, under the process conditions of O2 and TMGa flow rate ratio of 20, temperature of 610℃, and growth pressure of 56mbar, the growth temperature of TMGa was 1000℃ and 10000℃, respectively. + The deposition thickness on the β-Ga2O3 substrate is 10 μm and the Si doping concentration is 1×10 16 cm -3 n - β-Ga2O3 epitaxial layer.
[0200] Step 3: Deposition of dielectric layer, such as Figure 5 (c).
[0201] Using magnetron sputtering technology, the reaction chamber was first evacuated to 5.6×10 -4 Pa, growth pressure of 1.6 Pa, sputtering power of 30 W, and then - The thickness of the β-Ga2O3 epitaxial layer deposited on the surface is 300nm and the doping concentration is 1×10 18 cm -3 p-NiO dielectric layer.
[0202] Step 4: Make the cathode electrode, such as Figure 5 (d).
[0203] (4.1) Through electron beam evaporation E-beam, the vacuum in the working room is evacuated to 2.0×10 -4 Pa, electron gun acceleration voltage of 9Kv, electron gun beam current of 0.3A, evaporation time of 250s, first in n + A Ti / Au cathode electrode with a thickness of 50 / 200 nm is deposited on the back of the β-Ga2O3 substrate;
[0204] (4.2) Place the wafer after cathode electrode deposition in an annealing furnace and perform rapid annealing in a N2 environment at a furnace temperature of 475°C for 60 seconds to form a bond between the cathode electrode and the n + The contact surface of the β-Ga2O3 substrate forms a good ohmic contact.
[0205] Step 5: Make the anode electrode, such as Figure 5 (e).
[0206] (5.1) Photolithography is performed on the surface of the p-NiO dielectric layer. First, a layer of photoresist is spin-coated on the p-NiO dielectric layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form the device anode region;
[0207] (5.2) Through electron beam evaporation E-Beam, the evaporation chamber is evacuated to a vacuum of 2.5×10 -4 Under the process conditions of 300 Pa, electron gun acceleration voltage of 9 Kv, electron gun beam current of 0.4 A and evaporation time of 1200 s, a Ni / Au anode electrode with a thickness of 50 / 1200 nm is deposited in the anode area to form a Schottky contact at the contact surface of the anode electrode and the p-NiO dielectric layer. After the metal deposition is completed, the wafer is stripped with a photoresist stripping solution to remove excess photoresist and metal.
[0208] Step 6: Using atomic layer deposition ALD technology, under the process conditions of a reaction chamber temperature of 300°C and a pressure of 1.5 mbar, a Si3N4 passivation layer with a thickness of 150 nm is deposited on the periphery of the anode electrode. Figure 5 (f).
[0209] Step 7: Make a silver reflective layer, such as Figure 5 (g).
[0210] (7.1) Photolithography is performed on the dielectric layer on which the anode metal has been grown. First, photoresist is spin-coated on the surface of the dielectric layer. Then, alignment, exposure, development, and pattern detection are performed in sequence to form a circular silver reflective layer pattern, which is located between the anode metals and does not contact the metals;
[0211] (7.2) Through electron beam evaporation E-beam, the vacuum in the working room is evacuated to 2.6×10 -4 Under the process conditions of 100 nm thick silver was deposited on the dielectric layer, the electron gun acceleration voltage was 9 kv, the electron gun beam current was 0.3 A, and the evaporation time was 100 s. After the metal deposition was completed, the wafer was stripped with a photoresist stripping solution to remove excess photoresist and metal, forming a silver reflective layer with a thickness of 100 nm, a diameter of 10 μm, and a spacing of 40 μm between adjacent silver columns.
[0212] Step 8: Deposit the radiative cooling layer, e.g. Figure 5 (h).
[0213] (8.1) Photolithography is performed on the dielectric layer on which the anode metal and the silver reflective layer have been grown. First, photoresist is spin-coated on the surface of the dielectric layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form a radiation cooling layer pattern that overlaps with the pattern of the silver reflective layer;
[0214] (8.2) using plasma chemical vapor deposition (PECVD) technology, in a reaction chamber maintained at a temperature of 300°C and a pressure of 1.3 mbar, epitaxially grow a SiO2 layer with a thickness of 0.75 μm, a diameter of 10 μm and a spacing of 40 μm along the dielectric layer around the anode metal covered with photoresist;
[0215] (8.3) Using atomic layer deposition (ALD) technology, under the conditions of a temperature of 300°C and a pressure of 1.3 mbar in a reaction chamber, epitaxially grow a Si3N4 layer with a thickness of 0.75 μm, a diameter of 10 μm and a spacing of 40 μm along the dielectric layer covered with the outer periphery of the photoresist anode metal;
[0216] (8.4) The wafer with the radiation cooling layer is placed in a photoresist stripping solution for stripping to remove excess photoresist and SiO2 / Si3N4 composite layer, so that the radiation cooling layer is prepared on the silver reflective layer on the surface of the dielectric layer, thus completing the device preparation.
[0217] Example 5: A vertical Ga2O3 heterojunction diode is manufactured, wherein the silver reflective layer has a thickness of 300 nm and a thermal conductivity of 429 W / mK; and the radiation cooling layer is a HfO2 / Si3N4 composite with a thickness of 2 μm.
[0218] §1: Clean the substrate, such as Figure 5 (a).
[0219] The thickness is 650 μm and the Sn doping concentration is 5×10 18 cm -3 n + The β-Ga2O3 substrate was first ultrasonically cleaned in acetone solution for 10 minutes, then ultrasonically cleaned in isopropanol solution for 10 minutes, and finally ultrasonically cleaned in deionized water for 10 minutes with an ultrasonic power of 100 W. After cleaning, the substrate surface was blown dry with N2.
[0220] §2: Deposition of epitaxial layers, such as Figure 5 (b).
[0221] Metal organic chemical vapor deposition (MOCVD) technology was used, and the flow rate ratio of O2 and TMGa was set to 30, the temperature was 680℃, and the growth pressure was 65mbar. + The thickness of the grown β-Ga2O3 substrate is 15 μm and the Sn doping concentration is 2×10 16 cm -3 n - β-Ga2O3 epitaxial layer.
[0222] §3: Deposition of dielectric layer, such as Figure 5 (c).
[0223] The magnetron sputtering technology was used and the vacuum degree of the reaction chamber was set to 6×10 -4 Pa, growth pressure of 2.5 Pa, sputtering power of 35 W, in n - The surface growth thickness of β-Ga2O3 epitaxial layer is 350nm and the doping concentration is 6×10 18 cm -3 p-NiO dielectric layer.
[0224] §4: Make cathode electrode, such as Figure 5 (d).
[0225] Electron beam evaporation (E-beam) was used and the vacuum degree of the working chamber was set to 2.0×10 -4 Pa, the electron gun acceleration voltage is 7Kv, the electron gun beam current is 0.6A, and the evaporation time is 1500s. + A Ti / Au cathode electrode with a thickness of 50 / 1500nm is deposited on the back of the β-Ga2O3 substrate; then the wafer is placed in a rapid thermal annealing furnace, the furnace temperature is set to 475°C, and rapid annealing is performed in a N2 environment for 60s to form a good ohmic contact on the back of the gallium oxide substrate.
[0226] §5: Make the anode electrode, such as Figure 5 (e).
[0227] The surface of the p-NiO dielectric layer is photolithographically processed. First, a layer of photoresist is spin-coated on the p-NiO dielectric layer, and then alignment, exposure, development, and pattern detection are sequentially performed to form the device anode region.
[0228] Set the evaporation chamber to a vacuum of 2.5 × 10 -4 The process conditions are as follows: the electron gun acceleration voltage is 7Kv, the electron gun beam current is 0.4A, and the evaporation time is 1500s. Then, electron beam evaporation E-Beam is used to deposit a Ni / Au anode electrode with a thickness of 50 / 1500nm in the anode area to form a Schottky contact at the contact surface of the anode electrode and the p-NiO dielectric layer. After the metal deposition is completed, the wafer is stripped with a photoresist stripping solution to remove excess photoresist and metal.
[0229] §6: Using atomic layer deposition ALD technology, set the reaction chamber temperature to 350°C and the pressure to 5 mbar, and deposit a 200 nm thick Si3N4 passivation layer around the anode electrode, such as Figure 5 (f).
[0230] §7: Make a silver reflective layer, such as Figure 5 (g).
[0231] The dielectric layer on which the anode metal has been grown is subjected to photolithography, that is, firstly, photoresist is spin-coated on the surface of the dielectric layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form a circular silver reflective layer pattern, which is located between the anode metals and does not contact the metal;
[0232] Set the working chamber to evacuate to 2.6 × 10 -4 Pa, the electron gun acceleration voltage is 9Kv, the electron gun beam current is 0.3A, and the evaporation time is 300s. A 300nm thick metallic silver is deposited on the dielectric layer by electron beam evaporation E-beam;
[0233] After the metal deposition is completed, the wafer is stripped with a photoresist stripping solution to remove excess photoresist and metal, forming a silver reflective layer with a thickness of 300nm, a diameter of 20μm, and a spacing of 30μm between adjacent silver columns.
[0234] §8: Deposition of radiation cooling layer, such as Figure 5 (h).
[0235] Photolithography is performed on the dielectric layer on which the anode metal and the silver reflective layer have been grown, that is, firstly, photoresist is spin-coated on the surface of the dielectric layer, and then alignment, exposure, development, and pattern detection are performed in sequence to form a radiation cooling layer pattern that overlaps with the pattern of the silver reflective layer;
[0236] The temperature in the reaction chamber was set to 300°C and the pressure was set to 1.3 mbar. A HfO2 layer with a thickness of 1 μm was epitaxially grown along the dielectric layer around the anode metal covered with photoresist using plasma chemical vapor deposition (PECVD) technology.
[0237] The temperature of the reaction chamber is maintained at 300°C and the pressure is maintained at 1.3 mbar. Then, using the atomic layer deposition (ALD) technology, a 1 μm thick Si3N4 layer is epitaxially grown along the dielectric layer covered with the outer periphery of the photoresist anode metal.
[0238] The wafer with the radiation cooling layer is placed in a photoresist stripping solution for stripping treatment to remove excess photoresist and HfO2 / Si3N4 composite layer, so that the radiation cooling layer is prepared on the silver reflective layer on the surface of the dielectric layer. Each radiation cooler is located above the cylindrical silver reflective layer, the pattern is consistent with the silver reflective layer, the diameter is 20μm, and the distance between adjacent radiation cooling layers is 30μm, completing the device preparation.
[0239] Example 6: A vertical Ga2O3 heterojunction diode is manufactured, in which the silver reflective layer has a thickness of 500 nm and the radiation cooling layer is a TiO2 / Si3N4 composite layer with a thickness of 1.2 μm.
[0240] Step 1: Clean the substrate, such as Figure 5 (a).
[0241] The thickness is 600 μm and the Si doping concentration is 3×10 18 cm -3 n + The β-Ga2O3 substrate was first ultrasonically cleaned in acetone solution for 10 minutes, then ultrasonically cleaned in isopropanol solution for 10 minutes, and finally ultrasonically cleaned in deionized water for 10 minutes with an ultrasonic power of 100 W. After cleaning, the substrate surface was blown dry with N2.
[0242] Step 2: Ga2O3 epitaxial layer deposition, such as Figure 5 (b).
[0243] Using metal organic chemical vapor deposition MOCVD technology, + The deposition thickness on the β-Ga2O3 substrate is 7.5 μm, and the Sn doping concentration is 2×10 16 cm -3 n - β-Ga2O3 epitaxial layer, in which the process conditions used by metal organic chemical vapor deposition MOCVD are:
[0244] The growth pressure is 60 mbar.
[0245] The flow rate ratio of O2 and TMGa is 10,
[0246] The temperature is 640℃.
[0247] Step 3: Deposit p-NiO dielectric layer, such as Figure 5 (c).
[0248] Using magnetron sputtering technology, - The surface growth thickness of β-Ga2O3 epitaxial layer is 500nm and the doping concentration is 1×10 18 cm -3 The p-NiO dielectric layer is prepared by magnetron sputtering under the following process conditions:
[0249] The vacuum degree of the magnetron sputtering chamber is 5.6×10 -4 Pa,
[0250] The growth pressure is 1Pa,
[0251] The sputtering power is 28W.
[0252] Step 4: Make cathode electrode, such as Figure 5 (d).
[0253] (4-1) Using electron beam evaporation E-beam, +A Ti / Au cathode electrode with a thickness of 60 / 1000 nm is deposited on the back of the β-Ga2O3 substrate, wherein the process conditions of the electron beam evaporation E-beam are as follows:
[0254] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0255] The electron gun acceleration voltage is 8Kv.
[0256] The electron gun beam current is 0.4A.
[0257] The evaporation time is 1000s;
[0258] (4-2) After the cathode metal deposition is completed, the wafer is placed in a rapid thermal annealing furnace for annealing. In a N2 environment, the furnace temperature is set to 470°C and annealing is performed for 60 seconds to form a cathode electrode and n + Good ohmic contact between β-Ga2O3 substrate.
[0259] Step 5: Make the anode electrode, such as Figure 5 (e).
[0260] (5-1) firstly, a layer of photoresist is spin-coated on the p-NiO dielectric layer, and then alignment, exposure, development, and pattern detection are sequentially performed to photolithographically carve out a device anode region on the surface of the p-NiO dielectric layer;
[0261] (5-2) Ni / Au with a thickness of 50 / 1000 nm is deposited in the anode region by electron beam evaporation E-Beam to form a Schottky contact between the anode electrode and the gallium oxide epitaxial layer, wherein the process conditions used for electron beam evaporation E-Beam are as follows:
[0262] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0263] The electron gun acceleration voltage is 8Kv.
[0264] The electron gun beam current is 0.4A.
[0265] The evaporation time is 1000s;
[0266] (5-3) The wafer with the anode electrode deposited thereon is placed in a photoresist stripping solution to remove the photoresist.
[0267] Step 6: Using atomic layer deposition ALD technology, a Si3N4 passivation layer with a thickness of 180nm is deposited around the anode electrode. Figure 5 (f), wherein the process conditions of atomic layer deposition ALD are:
[0268] The reaction chamber temperature is 350°C.
[0269] The pressure is 2.5 mbar.
[0270] Step 7: Make a silver reflective layer, such as Figure 5 (g).
[0271] (7-1) performing photolithography on the dielectric layer on which the anode metal has been grown, i.e., firstly, spin coating photoresist on the surface of the dielectric layer, and then sequentially performing alignment, exposure, development, and pattern detection to form a circular silver reflective layer pattern, which is located between the anode metals and does not contact the metals;
[0272] (7-2) A 500 nm thick metallic silver layer is deposited on the dielectric layer by electron beam evaporation (E-beam). After the metal deposition is completed, the wafer is stripped using a photoresist stripping solution to remove excess photoresist and metal, thereby forming a cylindrical silver reflective layer with a diameter of 25 μm and a spacing of 25 μm between adjacent silver columns. The process conditions of the electron beam evaporation are:
[0273] The vacuum degree of the working chamber is 2.0×10 -4 Pa,
[0274] The electron gun acceleration voltage is 8Kv.
[0275] The electron gun beam current is 0.4A.
[0276] The evaporation time was 500 s.
[0277] Step 8: Deposit the radiative cooling layer, e.g. Figure 5 (h).
[0278] (8-1) performing photolithography on the dielectric layer on which the anode metal and the silver reflective layer have been grown, that is, firstly spin-coating a photoresist on the surface of the dielectric layer, and then sequentially performing alignment, exposure, development, and pattern detection to form a radiation cooling layer pattern that overlaps with the pattern of the silver reflective layer;
[0279] (8-2) Atomic layer deposition (ALD) technology is used to epitaxially grow a TiO2 layer with a thickness of 0.6 μm along the dielectric layer covered with the outer periphery of the photoresist anode metal, and then epitaxially grow a Si3N4 layer with a thickness of 0.6 μm along the dielectric layer covered with the outer periphery of the photoresist anode metal, wherein the process conditions of atomic layer deposition (ALD) are:
[0280] The reaction chamber temperature is 300°C;
[0281] The reaction chamber pressure is 1.3 mbar;
[0282] Sedimentation time 600 s;
[0283] (8-3) The wafer with the radiation cooling layer is placed in a photoresist stripping solution for stripping treatment to remove excess photoresist and the TiO2 / Si3N4 composite layer, so that the radiation cooling layer is prepared on the silver reflective layer on the surface of the dielectric layer. Each radiation cooler is located above the cylindrical silver reflective layer, and the pattern is consistent with the silver reflective layer, with a diameter of 25μm. The distance between adjacent radiation cooling layers is 25μm, and the device preparation is completed.
[0284] The above descriptions are only six specific examples of the present invention and do not constitute any limitation to the present invention. Obviously, for professionals in this field, after understanding the content and principle of the present invention, it is possible to make various modifications and changes in form and details without deviating from the principle and result of the present invention. For example, in addition to using SiO2 / Si3N4 composite layer and HfO2 / Si3N4 composite layer, the radiation layer can also use TiO2 / Si3N4 composite layer and Al2O3 / Si3N4 composite layer, and the present invention can use multiple composite layers to form a radiation cooling layer, such as SiO2 / Si3N4 / SiO2 / Si3N4 multilayer composite layer. However, these modifications and changes based on the concept of the present invention are still within the scope of protection of the claims of the present invention.
Claims
1. A Ga2O3 metal oxide semiconductor field effect transistor based on a radiation cooling layer, comprising from bottom to top: a substrate layer (2), a buffer layer (3), a channel layer (4) and a dielectric layer (5), wherein a source, a drain and a gate metal electrode are arranged on the dielectric layer (5), and a passivation layer (6) is wrapped around the periphery of the metal electrode, characterized in that: A silver reflective layer (1) is provided on the lower surface of the substrate layer (2) to effectively conduct the heat generated in the device and improve the heat reflection efficiency; The passivation layer (6) has a radiation cooling layer (7) composed of a plurality of SiO2 / Si3N4 cylindrical structures composited up and down, arranged between the metal electrodes on its upper surface, so as to enhance the heat dissipation performance of the device.
2. The effect tube according to claim 1, characterized in that: The silver reflective layer (1) is made of a high-metal silver material with a thermal conductivity of 400-450 W / mK and has a thickness of 1-15 μm.
3. The effect tube according to claim 1, characterized in that: The radiation cooling layer (7) has each SiO2 / Si3N4 cylindrical structure composited on top and bottom, with a thickness of 1 to 15 μm and a diameter of 4 to 50 μm, and a spacing of 5 to 30 μm between adjacent cylindrical structures. The composite cylindrical structure can also be composited on top and bottom with Si3N4 using any one of aluminum oxide, hafnium oxide or titanium oxide materials.
4. The effect tube according to claim 1, characterized in that: The substrate layer (2) is made of SiC or AlN and has a thickness of 150 to 600 μm; The buffer layer (3) is made of β-Ga2O3 and has a thickness of 0.5 to 2.5 μm; The channel layer (4) is made of β-Ga2O3 and has a thickness of 20 to 600 nm; The dielectric layer (5) is made of Al2O3, NiO, Hf 0.5 Zr 0.5 O2, any one of the species, with a thickness of 20 to 260 nm; The passivation layer (6) is made of SiO2 or Si3N4 and has a thickness of 80 to 250 nm.
5. A vertical Ga2O3 heterojunction diode based on a radiation cooling layer, comprising from bottom to top: a cathode electrode (1), an n+β-Ga2O3 substrate layer (2), an n-β-Ga2O3 epitaxial layer (3), a p-NiO dielectric layer (4) and an anode electrode (5), wherein the periphery of the anode electrode (5) is wrapped with a Si3N4 passivation layer (6), characterized in that: A circle of multiple SiO2 / Si3N4 cylindrical structures are distributed above the passivation layer, with a spacing of 10 to 20 μm between the anode metal and the structure. Each cylindrical structure is composed of a radiation cooling layer (8) and a silver reflection layer (7) in a composite structure. The spacing between two adjacent cylindrical structures is 10 to 40 μm, so as to reflect the heat generated inside the device and improve the heat dissipation performance.
6. The diode according to claim 5, characterized in that: Each SiO2 / Si3N4 cylindrical structure has a thickness of 1 to 15 μm and a ring width of 4 to 50 μm, wherein the silver reflective layer (7) has a thickness of 100 to 500 nm and is located between the Si3N4 passivation layer (6) and the radiation cooling layer (8).
7. The diode according to claim 5, characterized in that: The silver reflective layer (1) is made of high-metal silver material with a thermal conductivity of 400-450 W / mK. The composite annular structure can also be composited with Si3N4 using any one of aluminum oxide, hafnium oxide or titanium oxide materials.
8. The diode according to claim 5, characterized in that: The + The thickness of the β-Ga2O3 substrate layer (2) is 400-650 μm, the doping element is Si or Sn, and the doping concentration is 1×10 18 ~1×10 19 cm -3 ; The - The thickness of the β-Ga2O3 epitaxial layer (3) is 6 to 20 μm, the doping element is Si or Sn, and the doping concentration is 1×10 15 ~1×10 17 cm -3 ; The thickness of the p-NiO dielectric layer is 200-600 nm, the doping element is B, and the doping concentration is 1×10 17 ~5×10 18 cm -3 ; The thickness of the Si3N4 passivation layer (6) is 100-300 nm.
9. A method for preparing the Ga2O3 metal oxide semiconductor field effect transistor according to claim 1, characterized in that: The following steps are involved: S1) heterogeneously bonding a pre-prepared β-Ga2O3 wafer having a buffer layer and a channel layer to a substrate by high temperature annealing, and thinning the β-Ga2O3 wafer by ion cutting; S2) smoothing the surface of the channel layer and epitaxially depositing a dielectric layer on the channel layer; S3) firstly perform photolithography on the channel layer and the dielectric layer to define the pattern of the metal electrode, then deposit the electrode metal by electron beam evaporation E-Beam, perform ion implantation isolation, and deposit the passivation layer; S4) connecting the upper surface of the passivation layer on which the metal electrode is deposited to an external carrier wafer through a bonding process; S5) performing abrasive thinning and surface polishing on the back side of the substrate; S6) depositing a silver reflective layer on the back of the polished substrate by using electron beam evaporation (E-Beam); S7) removing the carrier wafer, defining the radiation cooling layer pattern on the passivation layer by photolithography, and then preparing the radiation cooling layer by plasma enhanced chemical vapor deposition (PECVD) and atomic layer deposition (ALD) to complete the device manufacturing.
10. The method according to claim 9, characterized in that: The process conditions of the electron beam evaporation E-Beam in step S3) are as follows: the working chamber is evacuated to 2.0×10 -4 Pa, the electron gun acceleration voltage is 8-10Kv, the electron gun beam current is 0.2-0.8A, and the evaporation time is 200-2000s; The process conditions of the electron beam evaporation E-Beam in step S6) are as follows: the working chamber is evacuated to 2.5×10 -4 Pa, the electron gun acceleration voltage is 6-10Kv, the electron gun beam current is 0.3-1A, and the evaporation time is 500-6000s; In the step S7), the plasma enhanced chemical vapor deposition PECVD process conditions are: SiH4 and N2O are used as precursor gases, and the flow rates are maintained at 40-80 cm 3 / min, 160~220cm 3 / min, the temperature is maintained at 260-300°C, the growth pressure is maintained at 75-100Pa, and the RF power is set to 60-100W.
11. A method for manufacturing the vertical Ga2O3 heterojunction diode according to claim 6, characterized in that: The following steps are involved: 1) Set n + The β-Ga2O3 substrate was first cleaned by organic ultrasonic cleaning and then dried in a N2 environment; 2) In n + Epitaxial deposition of n on β-Ga2O3 substrate by metal organic chemical vapor deposition MOCVD - β-Ga2O3 epitaxial layer; 3) In n - A p-NiO dielectric layer is deposited on the β-Ga2O3 epitaxial layer by magnetron sputtering technology; 4) In n + The cathode electrode is deposited on the back of the β-Ga2O3 substrate by electron beam evaporation E-beam, and then rapidly annealed to obtain a good ohmic contact; 5) forming an anode electrode region on the p-NiO dielectric layer by a photolithography development process, and then depositing the anode electrode by electron beam evaporation E-beam; 6) depositing a Si3N4 passivation layer on the periphery of the anode electrode by atomic layer deposition ALD; 7) defining a silver reflective layer pattern on the passivation layer by photolithography, and depositing the silver reflective layer by electron beam evaporation E-Beam technology; 8) On the Si3N4 passivation layer prepared with the silver reflective layer, a radiation cooling layer pattern consistent with the silver reflective layer is defined by photolithography, and SiO2 / Si3N4 composite layers are prepared by plasma enhanced chemical vapor deposition (PECVD) and atomic layer deposition (ALD) respectively to complete the device manufacturing.
12. The method according to claim 11, characterized in that: The process conditions of the metal organic chemical vapor deposition MOCVD in step 2) are: TMGa is used as a Ga precursor, O2 is used as an oxygen source, N2 is used as a carrier gas, the flow rate ratio of O2 to TMGa is 10-40, the temperature is maintained at 500-700°C, and the growth pressure is maintained at 55-75mbar; The process conditions of the magnetron sputtering in step 3) are as follows: the deposition chamber is evacuated to 5-6×10 -4 Pa, the growth pressure is maintained at 1-2.5 Pa, and the sputtering power is set to 20-35 W; The process conditions of the electron beam evaporation E-beam in step 4) and step 5) are as follows: the working chamber is evacuated to 2.0×10 - 4 Pa, the electron gun acceleration voltage is 6-10Kv, the electron gun beam current is 0.2-0.75A, and the evaporation time is 100-2000s; The process conditions of the electron beam evaporation E-beam in step 7) are as follows: the working chamber is evacuated to 2.6×10 -4 Pa, the electron gun acceleration voltage is 6~10Kv, the electron gun beam current is 0.25~1A, and the evaporation time is 200~2500s.
Citation Information
Patent Citations
Thermal radiation heat dissipation light-emitting diode structure and its fabrication method
CN102263185A
AlGaN / GaN-based field effect transistor and preparation method thereof
CN105679822A
Substrate with electric conduction, heat conduction and heat dissipation effects
CN112113154A
GaN HEMT based on interdigital composite diamond layer and preparation method
CN112510089A
Thermal detector
CN114364954A