Composite positive electrode material, preparation method thereof and all-solid-state lithium battery
By using MXene-coated fast ion conductors and positive electrode active materials in the positive electrode material of all solid lithium battery, the problems of insufficient load and low electronic conductivity are solved, and the high discharge capacity and cycle stability are improved, ensuring that High efficiency performance of the battery.
Patent Information
- Application Number
- CN202411017119.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
It is difficult for all-solid-state lithium batteries to achieve high-quality positive electrode material loads, resulting in impeded lithium ion transmission, reduced discharge capacity, insufficient cycle stability, and insufficient electronic conductivity.
The fast ion conductor coated with MXene is blended with the positive electrode active material, and by building an efficient and stable ion transport network and protective layer, the ion and electron conductivity of the composite positive electrode material is improved and the cycle stability of the battery is enhanced.
The high ionic conductivity and electronic conductivity of composite positive electrode materials are achieved, and the discharge capacity and cycle stability of all solid state lithium batteries are improved. The discharge specific capacity of the first round reaches 211.22mAh/g, and the capacity retention rate exceeds 96% after 150 rounds.
Smart Images

Figure CN118969986A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium battery positive electrode materials, and in particular to a composite positive electrode material and a preparation method thereof, and an all-solid-state lithium battery. Background Art
[0002] At present, my country is in an important period of transition from non-renewable energy such as coal, oil, and natural gas to renewable energy such as solar energy, nuclear energy, and electric energy. Among them, lithium-ion batteries are one of the important ways to replace traditional non-renewable fossil fuels due to their high energy density, long cycle life, and environmental friendliness. For traditional liquid lithium-ion batteries, since organic liquid electrolytes are used in the battery to transmit lithium ions, side reactions will inevitably occur during the charging and discharging process, and during the battery cycle, problems such as volatilization and leakage of the electrolyte may also occur. This will not only cause irreversible attenuation of the discharge capacity of the lithium-ion battery, but also some flammable and explosive organic electrolytes will cause serious safety problems after leakage.
[0003] All-solid-state lithium-ion batteries (SSLIBs), as a type of lithium-ion battery, have attracted widespread attention due to their characteristics of non-leakage, non-flammability, good mechanical properties, good electrochemical stability, high safety and excellent thermal stability. However, it is difficult for SSLIBs to achieve high mass loading of cathode materials, and thus it is difficult to achieve practical applications with high energy density. This is because the increase in loading will increase the thickness of the cathode sheet, and the side away from the electrolyte will be blocked by other particles when transmitting lithium ions, which seriously affects the stable output of lithium ions inside the cathode, resulting in only the cathode part in contact with the electrolyte to completely release lithium ions, ultimately reducing the battery discharge capacity; moreover, the increase in loading will greatly increase the charge and discharge current, which also indirectly accelerates the chemical side reactions between the cathode side and the electrolyte, and accelerates the generation of the CEI layer. Too thick CEI will lead to a decrease in battery performance, thereby reducing the battery life.
[0004] In order to improve the above problems, modifying the positive electrode material by blending or coating fast lithium ion conductors is an effective way to make solid-state batteries highly loaded. The filled fast ion conductor can not only construct a fast and stable lithium ion channel to assist the positive electrode in the transmission of lithium ions, but also the formed coating layer can protect the positive electrode material and improve the cycle stability of the battery. However, the modified SSLIBs have a decrease in the battery discharge capacity due to the decrease in the proportion of active materials, and it still has the problem of insufficient positive electrode electronic conductivity. Summary of the invention
[0005] The object of the present invention is to provide a composite positive electrode material and a preparation method thereof and an all-solid-state lithium battery. The composite positive electrode material provided by the present invention has high ionic conductivity and high electronic conductivity, and the lithium battery prepared using the composite positive electrode material has high discharge capacity and high cycle stability.
[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0007] The present invention provides a composite positive electrode material, comprising a positive electrode active material and a MXene-coated fast ion conductor.
[0008] Preferably, the mass ratio of the fast ion conductor to the positive electrode active material in the MXene-coated fast ion conductor is (0.01-5):100.
[0009] Preferably, the mass ratio of MXene to the positive electrode active material in the MXene-coated fast ion conductor is (0.01-5):100.
[0010] Preferably, the particle size of the fast ion conductor in the MXene-coated fast ion conductor is 0.1 to 10 μm.
[0011] Preferably, the positive electrode active material comprises LiFePO 4 、LiNi 0.5 Co 0.3 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Mn 0.2 O 2 or LiNi 0.8 Co 0.1 Mn 0.1 O 2 .
[0012] Preferably, the fast ion conductor in the MXene-coated fast ion conductor comprises Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 , Li 3 PO 4 , Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 、LiTi 0.5 Zr 1.5 (PO 4 ) 3 or Li 2 AlZr(PO4 ) 3 .
[0013] The present invention also provides a method for preparing the composite positive electrode material described in the above technical solution, comprising the following steps:
[0014] (1) mixing a fast ion conductor and MXene with an organic solvent respectively to obtain a fast ion conductor dispersion and a MXene dispersion;
[0015] (2) mixing the fast ion conductor dispersion obtained in step (1) with the MXene dispersion to obtain a mixed solution;
[0016] (3) Mixing the positive electrode active material with the mixed solution obtained in step (2) and drying the mixture to obtain a composite positive electrode material.
[0017] Preferably, the mass concentrations of the fast ion conductor dispersion and the MXene dispersion in step (1) are independently 1 to 100 mg / mL.
[0018] Preferably, the organic solvent in step (1) comprises anhydrous ethanol, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide.
[0019] The present invention also provides an all-solid-state lithium battery, wherein the positive electrode material in the all-solid-state lithium battery is the composite positive electrode material described in the above technical solution or the composite positive electrode material prepared by the preparation method described in the above technical solution.
[0020] The present invention provides a composite positive electrode material, including a positive electrode active material and a MXene-coated fast ion conductor. The present invention introduces a fast ion conductor into the positive electrode active material, and utilizes the high lithium ion conductivity of the fast ion conductor to construct an efficient and stable ion transport network, thereby improving the ion transport capacity of the positive electrode material; by using MXene with high electronic conductivity to coat the fast ion conductor, the electronic conductivity and discharge specific capacity of the composite positive electrode material are improved. At the same time, the functional atoms or groups such as -F, -O and -OH present in MXene can prevent the corrosion of the electrolyte, play a role in protecting the positive electrode active material, and significantly improve the long-term cycle stability of the positive electrode material. The results of the embodiment show that the ion conductivity of the composite positive electrode material provided by the present invention is 7.555×10 -3 S / cm, and the electronic conductivity is 4.761×10 -5 S / cm, with high ionic conductivity and high electronic conductivity; the all-solid-state lithium battery made of composite positive electrode material has a first-cycle discharge capacity of 211.22mAh / g, and a capacity retention rate of more than 96% after 150 cycles at 0.5C, with high discharge capacity and high cycle stability. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a SEM image of the LMN positive electrode sheet in Application Example 1 of the present invention;
[0022] Figure 2 A comparison diagram of the first cycle charge and discharge curves of the all-solid-state lithium battery in Application Example 1 of the present invention and Comparative Application Example 1;
[0023] Figure 3 This is a comparison chart of the rate performance of the all-solid-state lithium battery in Application Example 1 of the present invention and Comparative Application Example 1;
[0024] Figure 4 A comparison diagram of long cycle curves of all-solid-state lithium batteries in Application Example 1 of the present invention and Comparative Application Example 1;
[0025] Figure 5 This is a SEM image of the LML positive electrode sheet in Application Example 2 of the present invention;
[0026] Figure 6 A comparison diagram of the first cycle charge and discharge curves of the all-solid-state lithium battery in Application Example 2 of the present invention and Comparative Application Example 2;
[0027] Figure 7 This is a comparison chart of the rate performance of the all-solid-state lithium battery in Application Example 2 of the present invention and Comparative Application Example 2;
[0028] Figure 8 It is a comparison chart of the long cycle curves of the all-solid-state lithium batteries in Application Example 2 of the present invention and Comparative Application Example 2. DETAILED DESCRIPTION
[0029] The present invention provides a composite positive electrode material, comprising a positive electrode active material and a MXene-coated fast ion conductor.
[0030] In the present invention, the positive electrode active material preferably includes LiFePO 4 、LiNi 0.5 Co 0.3 Mn 0.2 O 2 、LiNi 0.6 Co 0.2 Mn 0.2 O 2 or LiNi 0.8 Co 0.1 Mn 0.1 O 2 The present invention limits the type of positive electrode active material to the above range, which can further improve the conductivity of the composite positive electrode material.
[0031] In the present invention, the fast ion conductor in the MXene-coated fast ion conductor preferably includes Li 6.4 La3 Zr 1.4 Ta 0.6 O 12 , Li 3 PO 4 , Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 、LiTi 0.5 Zr 1.5 (PO 4 ) 3 or Li 2 AlZr(PO 4 ) 3 The present invention limits the type of fast ion conductor in the MXene-coated fast ion conductor to the above range, so that the composite cathode material can have good ion conductivity.
[0032] In the present invention, the mass ratio of the fast ion conductor to the positive electrode active material in the MXene-coated fast ion conductor is preferably (0.01-5):100, more preferably (1-4):100, and further preferably (2-3):100. The present invention limits the mass ratio of the fast ion conductor to the positive electrode active material in the MXene-coated fast ion conductor to the above range, which can further improve the ionic conductivity of the composite positive electrode material.
[0033] In the present invention, the MXene is specifically Ti 3 C 2 T x , where T x The MXene is a functional group such as -F, -O and -OH. In the present invention, MXene can improve the electronic conductivity of the composite positive electrode material.
[0034] In the present invention, the mass ratio of MXene in the MXene-coated fast ion conductor to the positive electrode active material is preferably (0.01-5):100, more preferably (1-4):100, and further preferably (1-2):100. The present invention limits the mass ratio of MXene in the MXene-coated fast ion conductor to the positive electrode active material within the above range to further improve the electronic conductivity of the composite positive electrode material.
[0035] In the present invention, the particle size of the fast ion conductor in the MXene-coated fast ion conductor is preferably 0.1 to 10 μm, more preferably 2 to 8 μm, and further preferably 4 to 6 μm. The present invention limits the particle size of the fast ion conductor in the MXene-coated fast ion conductor to the above range, which can further improve the ionic conductivity of the composite positive electrode material.
[0036] The present invention introduces a fast ion conductor into the positive electrode active material, utilizes the high lithium ion conductivity of the fast ion conductor to construct an efficient and stable ion transport network, and improves the ion transport capacity of the positive electrode material; by using MXene with high electronic conductivity to coat the fast ion conductor, the electronic conductivity and discharge specific capacity of the composite positive electrode material are improved. At the same time, the functional atoms or groups such as -F, -O and -OH present in MXene can prevent the corrosion of the electrolyte, play a role in protecting the positive electrode active material, and significantly improve the long-term cycle stability of the positive electrode material.
[0037] The present invention also provides a method for preparing the composite positive electrode material described in the above technical solution, comprising the following steps:
[0038] (1) mixing a fast ion conductor and MXene with an organic solvent respectively to obtain a fast ion conductor dispersion and a MXene dispersion;
[0039] (2) mixing the fast ion conductor dispersion obtained in step (1) with the MXene dispersion to obtain a mixed solution;
[0040] (3) Mixing the positive electrode active material with the mixed solution obtained in step (2) and drying the mixture to obtain a composite positive electrode material.
[0041] The present invention mixes the fast ion conductor and MXene with an organic solvent to obtain a fast ion conductor dispersion and a MXene dispersion.
[0042] In the present invention, the mass concentration of the fast ion conductor dispersion is preferably 1 to 100 mg / mL, more preferably 5 to 50 mg / mL, and further preferably 5 to 10 mg / mL. In the present invention, the mass concentration of the MXene dispersion is preferably 1 to 100 mg / mL, more preferably 2 to 50 mg / mL, and further preferably 2 to 5 mg / mL. The present invention limits the mass concentrations of the fast ion conductor dispersion and the MXene dispersion to the above range, which can make the fast ion conductor and MXene more uniformly dispersed in the solvent and facilitate the subsequent preparation of composite positive electrode materials.
[0043] In the present invention, the preparation method of MXene preferably comprises the following steps:
[0044] (a) mixing LiF and concentrated hydrochloric acid to obtain a mixed solution 1;
[0045] (b) Ti 3 AlC 2 Mixing with the mixed solution 1 obtained in step (a) to perform an etching reaction to obtain a mixed solution 2;
[0046] (c) centrifuging, acid-washing and water-washing the mixed solution 2 obtained in step (b) to obtain a precipitate;
[0047] (d) mixing the precipitate obtained in step (c) with water, and then sequentially performing ultrasonication, centrifugation and drying to obtain MXene.
[0048] In the present invention, LiF and concentrated hydrochloric acid are preferably mixed to obtain a mixed solution 1.
[0049] In the present invention, the ratio of the mass of LiF to the volume of concentrated hydrochloric acid is preferably (1-1.6) g: (10-20) mL; the molar concentration of the concentrated hydrochloric acid is preferably 8-9 mol / L. In the present invention, the ratio of the mass of LiF to the volume of concentrated hydrochloric acid and the concentration of concentrated hydrochloric acid are limited to the above ranges to ensure that the subsequent reaction is fully carried out.
[0050] In the present invention, the mixing of LiF and concentrated hydrochloric acid is preferably carried out in a polytetrafluoroethylene reactor; the mixing temperature is preferably room temperature; the mixing is preferably carried out under stirring; the stirring speed is preferably 450-500 rpm; and the stirring time is preferably 15-30 min. The present invention limits the mixing parameters to the above range to make the materials mixed more uniformly.
[0051] After obtaining the mixed solution 1, the present invention preferably adds Ti 3 AlC 2 Mixed with the mixed solution 1 to perform etching reaction to obtain a mixed solution 2.
[0052] In the present invention, the Ti 3 AlC 2 The ratio of the mass of Ti to the volume of the mixed solution 1 is preferably (1-2) g: (10-20) mL. 3 AlC 2 The ratio of the mass of to the volume of the mixed solution 1 is limited to the above range to ensure that a MXene with excellent performance can be obtained.
[0053] In the present invention, the Ti 3 AlC 2 The mixing temperature with the mixed solution 1 is preferably 40 to 50°C; 3 AlC 2 The mixing with the mixed solution 1 is preferably carried out under stirring conditions; the stirring speed is preferably 450-500 rpm; and the stirring time is preferably 24-48 hours. The present invention sets the mixing parameters within the above range to obtain MXene with excellent performance.
[0054] After obtaining the mixed solution 2, the present invention preferably centrifuges, acid-washes and water-washes the mixed solution 2 in sequence to obtain a precipitate.
[0055] In the present invention, the centrifugation is preferably performed in a centrifuge; the rotation speed of the centrifugation is preferably 3500-5000 rpm. The present invention achieves solid-liquid separation of the mixed solution 2 by centrifugation.
[0056] In the present invention, the acid used in the pickling process is preferably hydrochloric acid; the concentration of the hydrochloric acid is preferably 0.5-1 mol / L; the number of picklings is preferably 3-5 times; centrifugation is preferably performed after each pickling; the speed of the centrifugation is preferably 3500-5000 rpm; the time of the centrifugation is preferably 5-10 min. In the present invention, the water used in the water washing is preferably deionized water; the number of water washings is preferably 5-10 times; centrifugation is preferably performed after each water washing; the speed of the centrifugation is preferably 3500-5000 rpm; the time of the centrifugation is preferably 5-10 min. The present invention can clean the impurities and acid in the precipitate by pickling and water washing.
[0057] After obtaining the precipitate, the present invention preferably mixes the precipitate with water and then sequentially performs ultrasonication, centrifugation and drying to obtain MXene.
[0058] In the present invention, the ultrasound is preferably performed in an ice-water bath; the ultrasound time is preferably 1 to 1.5 hours. In the present invention, the precipitate can be peeled off by ultrasound to obtain a single layer / few layers of MXene.
[0059] In the present invention, the centrifugal speed is preferably 3500-5000 rpm; the centrifugal time is preferably 1-1.5 h. In the present invention, the precipitate can be fully removed by centrifugation to obtain a monolayer / few-layer MXene dispersion.
[0060] In the present invention, the drying is preferably freeze drying. The present invention has no particular limitation on the temperature and time of the freeze drying, and parameters well known to those skilled in the art can be used for selection.
[0061] The MXene prepared by the above method in the present invention has a single-layer / few-layer structure, which can better improve the electronic conductivity of the composite positive electrode material.
[0062] In the present invention, the organic solvent preferably includes anhydrous ethanol, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide. The present invention limits the type of organic solvent to the above range to ensure that the organic solvent can be completely volatilized at a lower temperature during the drying process of preparing the composite positive electrode material, thereby avoiding the decomposition of MXene.
[0063] In the present invention, the mixing of the fast ion conductor and MXene with the organic solvent is preferably ultrasonic mixing; the time of the ultrasonic mixing is independently preferably 5 to 10 minutes; the ultrasonic mixing is preferably carried out in an ice water bath. The present invention does not specifically limit the frequency of the ultrasound, and the ultrasonic frequency commonly used by those skilled in the art can be used. The present invention can obtain a fast ion conductor dispersion and a MXene dispersion by ultrasonic mixing.
[0064] After obtaining the fast ion conductor dispersion and the MXene dispersion, the present invention mixes the fast ion conductor dispersion and the MXene dispersion to obtain a mixed solution.
[0065] In the present invention, the mixing of the fast ion conductor dispersion and the MXene dispersion is preferably ultrasonic mixing; the ultrasonic mixing time is preferably 30 to 60 minutes; and the ultrasonic mixing is preferably performed in an ice water bath. The present invention does not specifically limit the frequency of the ultrasound, and the ultrasonic frequency commonly used by those skilled in the art can be used.
[0066] The present invention preferably manually shakes every 5 to 10 minutes during the ultrasonic process. The present invention can prevent some solids from sinking to the bottom by manual shaking, so that the mixed solution is dispersed more evenly. The present invention can obtain a mixed solution with more uniform components through secondary mixing, and allow MXene to wrap around the fast ion conductor.
[0067] After obtaining the mixed solution, the present invention mixes the positive electrode active material with the mixed solution and then dries the mixture to obtain a composite positive electrode material.
[0068] In the present invention, the mixing of the positive electrode active material and the mixed solution is preferably performed by stirring; the stirring time is preferably 1 to 5 hours. The present invention has no special restrictions on the stirring operation and the stirring speed, and the stirring can be performed by using the operation and speed well known to those skilled in the art. The present invention can make the positive electrode active material and the mixed solution uniformly mixed by stirring.
[0069] In the present invention, the drying is preferably vacuum drying; the drying temperature is preferably 30 to 120°C, more preferably 40 to 100°C, and further preferably 50°C. The present invention has no special restrictions on the equipment and vacuum degree of the vacuum drying, and the equipment and vacuum degree commonly used by those skilled in the art can be used. The present invention can remove the organic solvent by drying to obtain a composite positive electrode material.
[0070] The present invention prepares a fast ion conductor dispersion and a MXene dispersion separately, and mixes the fast ion conductor dispersion and the MXene dispersion to uniformly coat the fast ion conductor with MXene, thereby further improving the conductivity of the composite positive electrode material, and further improving the discharge capacity and cycle stability of an all-solid-state lithium battery prepared from the composite positive electrode material.
[0071] The present invention also provides an all-solid-state lithium battery, wherein the positive electrode material in the all-solid-state lithium battery is the composite positive electrode material described in the above technical solution or the composite positive electrode material prepared by the preparation method described in the above technical solution.
[0072] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0073] Example 1
[0074] A composite positive electrode material, composed of LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622) and MXene-coated Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 (LLZTO) composition; the Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 and LiNi 0.6 Co 0.2 Mn 0.2 O 2 The mass ratio of the MXene-coated Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 MXene and LiNi in 0.6 Co 0.2 Mn 0.2 O 2 The mass ratio of Li is 1:100; 6.4 La 3 Zr 1.4 Ta 0.6 O 12 The particle size of (LLZTO) is 5 μm;
[0075] The preparation method of MXene comprises the following steps:
[0076] (a) LiF and concentrated hydrochloric acid were mixed in a polytetrafluoroethylene reactor at 500 rpm for 20 min at room temperature to obtain a mixed solution 1; the mass ratio of the LiF to the volume of the concentrated hydrochloric acid was 1.6 g:20 mL; and the molar concentration of the concentrated hydrochloric acid was 9 mol / L;
[0077] (b) Ti 3 AlC 2 The mixed solution 1 obtained in step (a) is mixed at a speed of 500 rpm and 50° C. for 48 hours to perform an etching reaction to obtain a mixed solution 2; the Ti 3 AlC 2 The ratio of the mass of to the volume of mixed solution 1 is 1g:20mL;
[0078] (c) separating the solid from the mixed solution 2 obtained in step (b) at a speed of 3500 rpm in a centrifuge, acid-washing the mixed solution 2 three times with 1 mol / L dilute hydrochloric acid, centrifuging the mixed solution at a speed of 3500 rpm for 5 min each time after each acid-washing, and then washing the mixed solution with deionized water five times, centrifuging the mixed solution at a speed of 3500 rpm for 5 min each time after each water washing, to obtain a precipitate;
[0079] (d) mixing the precipitate obtained in step (c) with water, performing ultrasound in an ice-water bath for 1 h, and then centrifuging at a speed of 3500 rpm for 1 h to obtain a MXene dispersion, and freeze-drying the MXene dispersion to obtain MXene;
[0080] The preparation method of the composite positive electrode material comprises the following steps:
[0081] (1) Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 (LLZTO) and MXene were mixed with anhydrous ethanol in an ice-water bath for 10 min by ultrasonication to obtain Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 (LLZTO) dispersion and MXene dispersion; the Li 6.4 La 3 Zr 1.4 Ta 0.6 O 12 The mass concentration of the (LLZTO) dispersion is 6.67 mg / mL; the mass concentration of the MXene dispersion is 3.33 mg / mL;
[0082] (2) Li obtained in step (1)6.4 La 3 Zr 1.4 Ta 0.6 O 12 The (LLZTO) dispersion and the MXene dispersion were ultrasonically mixed in an ice-water bath for 30 min and manually shaken every 5 min to obtain a mixed solution;
[0083] (3) LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622) and the mixed solution obtained in step (2) were stirred for 3 hours and then dried in a vacuum oven at 50° C. to obtain a composite positive electrode material, which was recorded as LMN.
[0084] Example 2
[0085] The difference between Example 2 and Example 1 is that the positive electrode active material is LiFePO 4 (LFP), and the rest is the same as in Example 1, to obtain a composite positive electrode material, denoted as LML.
[0086] Example 3
[0087] The difference between Example 3 and Example 1 is that the positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811), the rest is the same as in Example 1.
[0088] Example 4
[0089] The only difference between Example 4 and Example 1 is that the fast ion conductor in the MXene-coated fast ion conductor is Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 (LATP), and the rest is the same as in Example 1.
[0090] Example 5
[0091] The only difference between Example 5 and Example 2 is that the fast ion conductor in the MXene-coated fast ion conductor is Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 (LATP), and the rest is the same as in Example 2.
[0092] Example 6
[0093] The only difference between Example 6 and Example 3 is that the fast ion conductor in the MXene-coated fast ion conductor is Li 1.4 Al 0.4 Ti 1.6 (PO 4 ) 3 (LATP), and the rest is the same as in Example 3.
[0094] Example 7
[0095] The difference between Example 7 and Example 1 is that the fast ion conductor in the MXene-coated fast ion conductor is Li 2 AlZr(PO 4 ) 3 (LAZP), and the rest is the same as in Example 1.
[0096] Example 8
[0097] The only difference between Example 8 and Example 2 is that the fast ion conductor in the MXene-coated fast ion conductor is Li 2 AlZr(PO 4 ) 3 (LAZP), and the rest is the same as in Example 2.
[0098] Example 9
[0099] The only difference between Example 9 and Example 3 is that the fast ion conductor in the MXene-coated fast ion conductor is Li 2 AlZr(PO 4 ) 3 (LAZP), and the rest is the same as in Example 3.
[0100] Example 10
[0101] The difference between Example 10 and Example 1 is that the anhydrous ethanol in step (1) is replaced by N-methylpyrrolidone; and the drying temperature in step (3) is 120°C.
[0102] Embodiment 11
[0103] The difference between Example 11 and Example 1 is that the anhydrous ethanol in step (1) is replaced by N,N-dimethylformamide; and the drying temperature in step (3) is 70°C.
[0104] Example 12
[0105] The difference between Example 12 and Example 1 is that the anhydrous ethanol in step (1) is replaced by N,N-dimethylacetamide; and the drying temperature in step (3) is 70°C.
[0106] Application Examples 1 to 12
[0107] An all-solid-state lithium battery:
[0108] The composite positive electrode materials in Examples 1 to 12 were respectively mixed with SuperP and PVDF (polyvinylidene fluoride) in a mass ratio of 8:1:1 in NMP (N-methylpyrrolidone) and stirred for 12 hours to obtain a positive electrode slurry. The positive electrode slurry was evenly coated on an aluminum foil with a scraper, and placed in a vacuum oven at 120° C. for 12 hours until the solvent was evaporated, and a LMN positive electrode sheet with a diameter of 13 mm was cut with a cutter;
[0109] The 2025 type button all-solid-state lithium battery was assembled in an argon atmosphere glove box, wherein the positive electrode of the all-solid-state lithium battery was an LMN positive electrode sheet, the electrolyte was a PVDF-HFP (polyvinylidene fluoride-hexafluoropropylene) electrolyte, and the negative electrode was a lithium sheet.
[0110] Comparative application example 1
[0111] The difference between the comparative application example 1 and the application example 1 is that the positive electrode material in the positive electrode sheet is LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622), other details are the same as in Application Example 1.
[0112] Comparative Application Example 2
[0113] The difference between the comparative application example 2 and the application example 2 is that the positive electrode material in the positive electrode sheet is LiFePO 4 (LFP), other details are the same as those in Application Example 2.
[0114] The ionic conductivity and electronic conductivity of the composite cathode material were tested using an electrochemical workstation;
[0115] The microscopic morphology of the composite positive electrode sheet was observed using a scanning electron microscope (SEM, SU8000), and the working voltage of the scanning electron microscope was 3KV;
[0116] The NEWARE test system was used to test the charge and discharge process, long cycle performance and rate performance of the 2025 button battery. The charge and discharge voltage window was set to 2.8-4.3V, the current density of the long cycle test was set to 0.1C, and the current density of the rate performance test was set to 0.1C, 0.2C, 0.3C, 0.5C, 1C, and 2C respectively. All tests were carried out at room temperature of 25°C.
[0117] The electrochemical impedance spectroscopy (EIS) test frequency range of 2025 button battery is 0.01~100kHz, and the perturbation amplitude is 10mV.
[0118] The SEM image of the LMN cathode sheet in Application Example 1 is as follows: Figure 1 As shown, from Figure 1 It can be seen that the MXene-coated LLZTO is evenly distributed in the positive electrode, which successfully fills the gaps between the positive electrode particles.
[0119] The comparison of the first cycle charge and discharge curves of the lithium battery in Application Example 1 and Comparative Application Example 1 is shown in the figure below: Figure 2 As shown, from Figure 2 It can be seen that the first cycle discharge capacity of the lithium battery prepared by LMN positive electrode is 166.4mAh / g, while LiNi 0.6 Co 0.2 Mn 0.2 O 2 The first-cycle discharge specific capacity of the lithium battery prepared with (NCM622) positive electrode sheet is 151.9 mAh / g.
[0120] The comparison of the rate performance of lithium batteries in Application Example 1 and Comparative Application Example 1 is shown in the figure below: Figure 3 As shown, from Figure 3 It can be seen that compared with LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622), LMN can still have good capacity retention at high rates.
[0121] The comparison of the long cycle curves of lithium batteries in Application Example 1 and Comparative Application Example 1 is shown in the figure below: Figure 4 As shown, from Figure 4 It can be seen that the loading of both is 8.5 mg / cm 2 , LMN can still maintain good capacity after 30 cycles at 0.1C, while LiNi 0.6 Co 0.2 Mn 0.2 O 2 (NCM622) has decayed to 90% of its original value after 30 cycles at 0.1C.
[0122] The SEM image of the LML cathode sheet in Application Example 2 is as follows: Figure 5 As shown, from Figure 5 It can be seen that the MXene-coated LLZTO is evenly distributed in the positive electrode, which successfully fills the gaps between the positive electrode particles.
[0123] The comparison of the first cycle charge and discharge curves of the lithium battery in Application Example 2 and Comparative Application Example 2 is shown in the figure below: Figure 6 As shown, from Figure 6 It can be seen that the first cycle discharge capacity of the lithium battery prepared by LML positive electrode is 156.6mAh / g, while LiFePO 4 The first-cycle discharge capacity of the lithium battery prepared with (LFP) positive electrode sheet is 134.9 mAh / g.
[0124] The comparison of the rate performance of lithium batteries in Application Example 2 and Comparative Application Example 2 is shown in the figure below: Figure 7 As shown, from Figure 7 It can be seen that compared with LiFePO 4 (LFP), LML have higher capacity at different rates.
[0125] The long cycle curve comparison of lithium batteries in Application Example 2 and Comparative Application Example 2 is shown in the figure below: Figure 8 As shown, from Figure 8 As can be seen, the loading of both is 10 mg / cm 2 , LML has a capacity retention rate of 96% after 150 cycles at 0.5C, while LiFePO 4 (LFP) capacity retention rate is only 88%.
[0126] The ionic conductivity and electronic conductivity data of the composite positive electrode materials of Examples 1 to 12 are shown in Table 1.
[0127] Table 1 Ionic conductivity and electronic conductivity data of the composite positive electrode materials of Examples 1 to 12
[0128]
[0129]
[0130] The first-cycle discharge specific capacity and capacity retention rate data after 50 cycles at 0.1C of the all-solid-state lithium batteries in Application Examples 3 to 12 are shown in Table 2.
[0131] Table 2 The first cycle discharge specific capacity and capacity retention rate data after 50 cycles at 0.1C for all-solid-state lithium batteries in application examples 3 to 12
[0132] Application Examples First cycle discharge capacity (mAh / g) Capacity retention rate (%) Application Example 3 203.15 98.12 Application Example 4 161.31 99.50 Application Example 5 153.28 99.75 Application Example 6 211.22 99.31 Application Example 7 165.80 98.88 Application Example 8 150.87 99.18 Application Example 9 207.32 98.56 Application Example 10 164.90 99.34 Application Example 11 167.52 98.96 Application Example 12 163.22 98.55
[0133] The ionic conductivity of the composite positive electrode material provided by the present invention can reach 7.555×10 -3 S / cm, and the electronic conductivity can reach 4.761×10 -5 S / cm, with high ionic conductivity and high electronic conductivity; the all-solid-state lithium battery made of composite positive electrode material has a first-cycle discharge capacity of 211.22mAh / g, and a capacity retention rate of more than 96% after 150 cycles at 0.5C, with high discharge capacity and high cycle stability.
[0134] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A composite cathode material comprising a cathode active material and a MXene-coated fast ion conductor.
2. The composite positive electrode material according to claim 1, characterized in that The mass ratio of the fast ion conductor to the positive electrode active material in the MXene-coated fast ion conductor is (0.01-5):
100.
3. The composite positive electrode material according to claim 1 or 2, characterized in that: The mass ratio of MXene to the positive electrode active material in the MXene-coated fast ion conductor is (0.01-5):
100.
4. The composite positive electrode material according to claim 1 or 2, characterized in that: The particle size of the fast ion conductor in the MXene-coated fast ion conductor is 0.1 to 10 μm.
5. The composite positive electrode material according to claim 1, characterized in that: The positive electrode active material includes LiFePO4, LiNi 0.5 Co 0.3 Mn 0.2 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2 or LiNi 0.8 Co 0.1 Mn 0.1 O2.
6. The composite positive electrode material according to claim 1, characterized in that: The fast ion conductor in the MXene-coated fast ion conductor includes Li 6.4 Ln3Z 1.4 Ta 0.6 O 12 、Li3PO4、Li 1.4 Al 0.4 Ti 1.6 (PO4)3、LiTi 0.5 Zr 1.5 (PO4)3 or Li2AlZr(PO4)3.
7. The method for preparing the composite positive electrode material according to any one of claims 1 to 6, comprising the following steps: (1) mixing a fast ion conductor and MXene with an organic solvent respectively to obtain a fast ion conductor dispersion and a MXene dispersion; (2) mixing the fast ion conductor dispersion obtained in step (1) with the MXene dispersion to obtain a mixed solution; (3) Mixing the positive electrode active material with the mixed solution obtained in step (2) and drying the mixture to obtain a composite positive electrode material.
8. The preparation method according to claim 7, characterized in that: The mass concentrations of the fast ion conductor dispersion and the MXene dispersion in step (1) are independently 1 to 100 mg / mL.
9. The preparation method according to claim 7 or 8, characterized in that: The organic solvent in step (1) includes anhydrous ethanol, N-methylpyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide or dimethyl sulfoxide.
10. An all-solid-state lithium battery, characterized in that: The positive electrode material in the all-solid-state lithium battery is the composite positive electrode material according to any one of claims 1 to 6 or the composite positive electrode material prepared by the preparation method according to any one of claims 7 to 9.
Citation Information
Patent Citations
Lithium titanate / lithium ion conductor / carbon composite material and preparation method and application thereof
CN113937260A
Positive electrode active material, electrochemical device, and electronic apparatus
CN115036503A
Cobalt-based positive electrode material with composite coating layer, preparation method of cobalt-based positive electrode material and lithium ion battery
CN117352736A
Sodium ion battery positive electrode material and application thereof
CN118231587A
Thin film transistor and its fabrication method
KR102189557B1