Anode material of aqueous zinc ion battery, preparation method and application

By using the hydrophobic coating of ZnF2/MXene composite in aqueous zinc ion batteries, problems such as hydrogen evolution reaction and dendrite growth are solved, extending the service life of the battery and improving the safety and performance of the battery.

CN118970007APending Publication Date: 2024-11-15UNIV OF JINAN
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411158580.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

During the charging and discharging process of aqueous zinc ion batteries, there are problems with hydrogen evolution reaction, dendrite growth, corrosion and passivation, resulting in irreversible deposition of zinc negative electrodes and shortening of battery service life.

Method used

Using ZnF2/MXene composite material as the coating of the negative electrode material, connecting ZnF2 and MXene through intermolecular forces to form a hydrophobic layer in the shape of an accordion, combining carbon black and binder to enhance conductivity and protection effect, and reduce the zinc base layer. Corrosion and passivation.

Benefits of technology

It effectively inhibits hydrogen evolution reaction and dendrites growth, extends the service life of the battery, and improves the coulombic efficiency and safety of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970007A_ABST
    Figure CN118970007A_ABST
Patent Text Reader

Abstract

The embodiment of the invention relates to a negative electrode material of an aqueous zinc ion battery, a preparation method and application, the negative electrode material comprises a zinc substrate layer and a coating on the zinc substrate layer, the coating comprises a ZnF2 / MXene composite material and a binder, the ZnF2 / MXene composite material comprises ZnF2 and MXene, the ZnF2 and the MXene are connected through an intermolecular force, the molecular formula of the MXene is MaXb, and the molecular formula of the binder is as shown in the specification. Wherein M is a transition metal element, X is a carbon or nitrogen element, a is 2 or 3, b is 1 or 2, the ZnF2 / MXene composite material has an accordion shape, the negative electrode material can reduce contact between free water and a Zn negative electrode, and the problems of HER (hydrogen evolution reaction), dendritic crystal growth, corrosion, passivation and the like in the charging and discharging process of the aqueous zinc ion battery are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of zinc ion battery materials, and more specifically, to a negative electrode material, a preparation method and an application of an aqueous zinc ion battery. Background Art

[0002] The information disclosed in the background of the present invention is only intended to increase the understanding of the overall background of the present invention and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.

[0003] The growing demand for energy and serious environmental pollution problems force us to promote the transition from fossil fuels to renewable energy. Lithium-ion batteries are the most intensively studied energy storage system. Since their introduction in the 1990s, they have dominated the energy market, from portable electronic products to emerging electric / hybrid vehicles. However, the high cost of lithium and the flammability risk of organic electrolytes restrict the development of lithium-ion batteries. Aqueous zinc-ion batteries are considered to be one of the important energy storage devices to replace lithium batteries because they use aqueous electrolytes, have high safety and high ionic conductivity, and zinc reserves are abundant and low in cost. However, as the negative electrode, metallic zinc will inevitably react with the aqueous solution in the electrolyte due to its high electrochemical activity, causing corrosion and passivation of the zinc negative electrode, thereby further forming zinc "dendrites". These dendrites will continuously consume the electrolyte during their growth, causing irreversible deposition of metallic zinc, making less and less zinc available for the reaction, thereby reducing the coulombic efficiency. In severe cases, the dendrites may even pierce the diaphragm, causing an internal short circuit in the battery and causing an accident. There is also the problem of hydrogen evolution reaction (HER) during the cycle of aqueous zinc-ion batteries. In addition, the surface of pure zinc will be corroded during the charge and discharge process of aqueous electrolytes to generate ZnO and Zn(OH)2 by-products, which affects the electric field distribution on the negative electrode surface. The uneven deposition behavior during multiple charge and discharge processes will accelerate the growth of zinc dendrites, resulting in earlier puncture of the diaphragm, which is further not conducive to improving the battery's service life. Summary of the invention

[0004] The present application is provided to solve the above-mentioned defects existing in the prior art. A negative electrode material, preparation method and application of an aqueous zinc ion battery are needed, and a negative electrode material for an aqueous zinc ion battery is provided, which can reduce the contact between free water and the Zn negative electrode and solve the problems of HER (hydrogen evolution reaction), dendrite growth, corrosion and passivation in the charging and discharging process of the aqueous zinc ion battery.

[0005] In a first aspect of the present application, a negative electrode material for an aqueous zinc ion battery is provided, wherein the negative electrode material comprises a zinc base layer and a coating on the zinc base layer, wherein the coating comprises a ZnF2 / MXene composite material and a binder, wherein the ZnF2 / MXene composite material comprises ZnF2 and MXene, wherein the ZnF2 and MXene are connected by intermolecular forces, and the molecular formula of the MXene is M a X b , wherein M is a transition metal element, X is a carbon or nitrogen element, a is 2 or 3, and b is 1 or 2, and the ZnF2 / MXene composite material has an accordion shape.

[0006] In some embodiments, the thickness of the coating is 15-30 microns, so as to provide better protection for the zinc substrate. The coating can be performed by a scraper method or the like. The coating is performed after the slurry is ground, and the grinding time is 10-30 min.

[0007] In some embodiments, the coating layer further comprises carbon black, which can increase the conductivity of the coating layer and is beneficial to improving the electrical properties of the negative electrode material.

[0008] In some embodiments, the binder includes PVDF (polyvinylidene fluoride) or CMC (sodium carboxymethyl cellulose). In some embodiments, the mass ratio of ZnF2 / MXene composite material, carbon black and PVDF is 6-9: 1-3: 1; preferably 7-8: 2-3: 1.

[0009] In some embodiments, the zinc base layer is made of metallic zinc. The thickness of the zinc base layer is 0.2-1.5 mm. Preferably, the thickness of the coating is 0.2-1 mm, such as 0.2 mm, 0.3 mm, 0.5 mm, 1.0 mm, so as to provide better protection for the zinc base layer.

[0010] The second aspect of the present application provides a method for preparing the negative electrode material of the aqueous zinc ion battery described in any embodiment of the present application, the preparation method comprising: mixing the ZnF2 / MXene composite material with a solvent and a binder to form a slurry; applying the slurry on a zinc base layer, and forming a coating after the slurry is dried to obtain a negative electrode material.

[0011] In some embodiments, the slurry is dried at a temperature of 50-80° C. and for a drying time of 6-24 h.

[0012] In some embodiments, the solvent includes NMP (N-methylpyrrolidone) or water. Preferably, the binder is PVDF and the solvent is NMP. The solvent water causes the ground slurry to be loosely in contact with the zinc foil and is easy to fall off, thereby affecting the performance of the battery.

[0013] In some embodiments, the amount of solvent added is 5% to 30% of the mass of the binder. Specifically, the optimal ratio of solvent to binder can be determined by detecting the viscosity of the mixed slurry. During the drying process, the solvent is evaporated under the condition of a drying time of 6 to 12 hours.

[0014] In some embodiments, the preparation method of the ZnF2 / MXene composite material is as follows: a MAX phase solid material and a fluorine-containing organic matter are placed at different positions in a closed environment, the A layer in the MAX phase material is Zn, and the ZnF2 / MXene composite material is obtained by reaction under protective atmosphere and heating conditions.

[0015] In some embodiments, the reaction temperature is 500-700°C; preferably, the reaction temperature is 580-620°C, such as 590°C, 600°C, etc. In some embodiments, the heating rate is 1-7°C / min; preferably, the heating rate is 4-5°C / min.

[0016] In some embodiments, the M element in the MAX phase material includes one or more of Ti, Zr, Hf, V, Nb, Ta, Cr, Sc, Mo, etc., and the X element includes one or both of C and N.

[0017] In some embodiments, the fluorine-containing organic compound includes one or more mixtures of polyvinylidene fluoride, polytetrafluoroethylene, polychlorotrifluoroethylene, tetrafluoroethylene / hexafluoropropylene copolymer, perfluorinated alkyl vinyl ether copolymer, ethylene and tetrafluoroethylene copolymer, etc., preferably polyvinylidene fluoride.

[0018] In some embodiments, the mass ratio of the MAX phase material to the fluorine-containing organic compound is 1:1-7. Preferably, an excess of fluorine-containing organic compound is used so that the "A" element in the MAX phase (the "A" layer atoms are Zn atoms) material is fully converted into metal fluoride, i.e., ZnF2. Preferably, the mass ratio of the MAX phase material to the fluorine-containing organic compound is 1:4-5. For example, 1:5.

[0019] In some embodiments, a method for preparing a MXene material based on a ZnF2 / MXene composite material is provided, the method comprising: treating the ZnF2 / MXene composite material using a water bath method, then filtering the solution after the water bath treatment to obtain a solid product, and drying the solid product to obtain a MXene material, wherein the molecular formula of the MXene is M a X b , wherein M is a transition metal element, X is a carbon or nitrogen element, a is 2 or 3, and b is 1 or 2. In some embodiments, the temperature for washing the product by water bath method is 60-80° C. The reaction time of water bath method is 2-6 h.

[0020] The product is washed and then vacuum dried to obtain a ZnF2 / MXene composite material. The vacuum drying temperature is 40-80°C and the drying time is 6-12 h.

[0021] In some embodiments, the protective atmosphere is an inert gas and / or nitrogen.

[0022] The third aspect of the present application provides an application of the negative electrode material of an aqueous zinc ion battery and the method for preparing the negative electrode material of an aqueous zinc ion battery described in any embodiment of the present application in an aqueous zinc ion battery.

[0023] The negative electrode material, preparation method and application of an aqueous zinc ion battery provided in each embodiment of the present application, the negative electrode material includes a zinc base layer and a coating on the zinc base layer, the coating includes a ZnF2 / MXene composite material and a binder, the ZnF2 / MXene composite material is better combined with the zinc base layer by the binder to form a protective layer for the zinc base layer, the ZnF2 / MXene composite material includes ZnF2 and MXene, ZnF2 forms a hydrophobic layer, the ZnF2 / MXene composite material has an accordion shape, can inhibit the growth of zinc dendrites, reduce the contact between free water and the Zn negative electrode, thereby solving the problems of corrosion and passivation of the zinc base layer, and greatly extending the service life of the aqueous zinc ion battery. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In the drawings, which are not necessarily drawn to scale, the same reference numerals may describe similar parts in different views. The same reference numerals with letter suffixes or different letter suffixes may represent different instances of similar parts. The accompanying drawings generally illustrate various embodiments by way of example and not limitation, and together with the specification and claims, are used to illustrate the embodiments applied for. When appropriate, the same reference numerals are used throughout the drawings to refer to the same or similar parts. Such embodiments are illustrative and are not intended to be exhaustive or exclusive embodiments of the present apparatus or method.

[0025] Figure 1 A scanning electron microscope image (SEM) of the ZnF2 / V2C MXene composite material of Example 1 of the present application is shown.

[0026] Figure 2 A scanning electron microscope image (SEM) of the V2C MXene material of Example 1 of the present application is shown.

[0027] Figure 3 X-ray diffraction patterns (XRD) of ZnF2 / V2C MXene, V2C MXene, and V2ZnC of Example 1 of the present application are shown.

[0028] Figure 4 The SEM image of the ZnF2 / MXene composite material of Example 5 of the present application is shown.

[0029] Figure 5 The XRD patterns of the ZnF2 / MXene composite materials obtained in Examples 1 and 5 of the present application are shown.

[0030] Figure 6 The long cycle performance diagram of the symmetrical battery assembled from the pole pieces of Example 9 of the present application is shown.

[0031] Figure 7 The cycling performance diagram of the symmetrical battery assembled from the ZnF2 / MXene composite material of Example 5 of the present application is shown.

[0032] Figure 8 The graph showing the cycling performance at high current density of a symmetrical battery assembled with the ZnF2 / V2C MXene composite material negative electrode of Example 1 of the present application.

[0033] Fig. 9 A rate performance diagram of a symmetrical battery assembled from the pole pieces of Example 9 of the present application is shown.

[0034] Fig.10 A comparison chart of the cycle performance of a full battery assembled with the pole piece of Example 9 of the present application and ZVO is shown. DETAILED DESCRIPTION

[0035] In order to enable those skilled in the art to better understand the technical solution of the present application, the present application is described in detail below in conjunction with the accompanying drawings and specific implementation examples. The embodiments of the present application are further described in detail below in conjunction with the accompanying drawings and specific implementation examples, but are not intended to limit the present application.

[0036] The words "first", "second" and similar words used in this application do not indicate any order, quantity or importance, but are only used to distinguish. The words "include" or "comprise" and similar words mean that the elements before the word include the elements listed after the word, and do not exclude the possibility of including other elements.

[0037] According to an embodiment of the present application, a negative electrode material for an aqueous zinc ion battery is provided, wherein the negative electrode material comprises a zinc base layer and a coating on the zinc base layer, wherein the coating comprises a ZnF2 / MXene composite material and a binder, wherein the ZnF2 / MXene composite material comprises ZnF2 and MXene, wherein the ZnF2 and MXene are connected by intermolecular forces, and the molecular formula of the MXene is M a X b, wherein M is a transition metal element, X is a carbon or nitrogen element, a is 2 or 3, and b is 1 or 2, and the ZnF2 / MXene composite material has an accordion shape.

[0038] The ZnF2 in the coating is hydrophobic, and a hydrophobic layer is artificially constructed on the negative electrode side of the aqueous zinc-ion battery to reduce the contact between free water and the Zn negative electrode, thereby effectively inhibiting HER. The high conductivity of MXene enables a uniform electric field to be constructed on the negative electrode side, thereby inducing uniform zinc deposition and reducing the occurrence of the "tip effect", thereby extending the service life of the battery. The ZnF2 and MXene in the ZnF2 / MXene composite material cooperate with each other to form a SEI protective film, which provides a good protection effect for the zinc base layer, can inhibit the corrosion and passivation of the zinc negative electrode, and can inhibit the formation of zinc dendrites.

[0039] The binder enables the ZnF2 / MXene composite material to be firmly attached to the zinc substrate layer.

[0040] In some embodiments, the thickness of the coating is 15-30 microns, so as to provide better protection for the zinc substrate. The coating can be performed by a scraper method or the like. The coating is performed after the slurry is ground, and the grinding time is 10-30 min.

[0041] In some embodiments, the coating layer further comprises carbon black, which can increase the conductivity of the coating layer and is beneficial to improving the electrical properties of the negative electrode material.

[0042] In some embodiments, the binder includes PVDF (polyvinylidene fluoride) or CMC (sodium carboxymethyl cellulose). In some embodiments, the coating further includes a solvent; the solvent includes NMP (N-methylpyrrolidone) or water. Preferably, the binder is PVDF and the solvent is NMP. The solvent water causes the ground slurry to be loosely in contact with the zinc foil and is easy to fall off, thereby affecting the performance of the battery.

[0043] In some embodiments, the mass ratio of ZnF2 / MXene composite material, carbon black and PVDF is 6-9: 1-3: 1; preferably 7-8: 2-3: 1.

[0044] In some embodiments, the amount of solvent added is 5% to 30% of the mass of the binder. Specifically, the optimal ratio of solvent to binder can be determined by detecting the viscosity of the mixed slurry.

[0045] In some embodiments, the zinc base layer is made of metallic zinc. The thickness of the zinc base layer is 0.2-1.5 mm. Preferably, the thickness of the coating is 15-30 microns, such as 15 microns, 18 microns, 20 microns, and 25 microns, so as to provide better protection for the zinc base layer.

[0046] According to an embodiment of the present application, there is also provided a method for preparing a negative electrode material for an aqueous zinc ion battery as described in any embodiment of the present application, the preparation method comprising: mixing a ZnF2 / MXene composite material with a solvent and a binder to form a slurry; applying the slurry on a zinc base layer, and forming a coating after the slurry is dried to obtain a negative electrode material.

[0047] In some embodiments, the slurry is dried at a temperature of 50-80° C. and for a drying time of 6-24 h.

[0048] In some embodiments, the preparation method of the ZnF2 / MXene composite material is as follows: a MAX phase solid material and a fluorine-containing organic substance are placed at different positions in a closed environment, the A layer in the MAX phase material is Zn, and the ZnF2 / MXene composite material is obtained by reaction under a protective atmosphere and heating conditions. In the preparation of traditional MXene materials, the Zn element is etched and dissolved in an acid solution and removed in subsequent steps, and waste liquid is also formed, which not only pollutes the environment but also wastes the Zn element. The preparation method of the present application realizes the atomic-level utilization of the MAX phase to reduce the waste of resources, which can reduce the waste of resources. Compared with existing methods such as electrolysis, electrodeposition, and sputtering, the process operability is greatly improved.

[0049] Fluorine-containing organic matter is thermally decomposed under heating conditions to form fluorine-containing gas (HF, RCF2 and / or CF4). Under protective atmosphere conditions, the fluorine-containing gas and Zn element are etched to generate ZnF2 while also generating accordion-shaped MXene, thereby obtaining a ZnF2 / MXene composite material.

[0050] During the reaction, Zn element combines with F element to form ZnF2.

[0051] In some embodiments, the reaction temperature is 580-620 °C. For example, 590 °C, 600 °C, etc. In some embodiments, the heating rate is 4-5 °C / min. The reaction temperature and heating rate affect the protective effect of the ZnF2 / MXene composite material on the zinc substrate. Because at 600 °C, zinc fluoride is the most; at 500 °C, there are still many MAX phases, and the M element of the MAX phase will be oxidized at higher temperatures. The heating rate will also affect the insulation time. When the insulation time is extended, it will lead to excessive etching of MXene, which will affect its morphology and weaken the performance of the ZnF2 / MXene composite material.

[0052] In some embodiments, the M element in the MAX phase material includes one or more of Ti, Zr, Hf, V, Nb, Ta, Cr, Sc, Mo, etc., and the X element includes one or both of C and N.

[0053] In some embodiments, the fluorine-containing organic compound includes one or more mixtures of polyvinylidene fluoride, polytetrafluoroethylene, polychlorotrifluoroethylene, tetrafluoroethylene / hexafluoropropylene copolymer, perfluorinated alkyl vinyl ether copolymer, ethylene and tetrafluoroethylene copolymer, etc., preferably polyvinylidene fluoride.

[0054] In some embodiments, the mass ratio of the MAX phase material to the fluorine-containing organic compound is 1: 1-7. Preferably, an excess of fluorine-containing organic compound is used so that the "A" element in the MAX phase (the "A" layer atoms are Zn atoms) material is fully converted into metal fluoride, i.e., ZnF2. Preferably, the mass ratio of the MAX phase material to the fluorine-containing organic compound is 1: 4-5. For example, 1: 5.

[0055] In some embodiments, the product after the reaction is washed by a water bath method. In some embodiments, the temperature of the product during the water bath method is 60-80° C. The reaction time of the water bath method is 2-6 h.

[0056] The product is washed and then vacuum dried to obtain a ZnF2 / MXene composite material. The vacuum drying temperature is 40-80°C and the drying time is 6-12 h.

[0057] In some embodiments, the protective atmosphere is an inert gas or nitrogen. The protective atmosphere is mainly used to isolate oxygen and prevent the MAX phase (the "A" layer atoms are Zn atoms) material and the generated MXene material from being oxidized at high temperature.

[0058] According to the embodiments of the present application, there is also provided an application of the negative electrode material of an aqueous zinc ion battery and the method for preparing the negative electrode material of an aqueous zinc ion battery described in any embodiment of the present application in an aqueous zinc ion battery.

[0059] Example 1 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g V2ZnC MAX and 5 g polyvinylidene fluoride at the two ends of a corundum boat.

[0060] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 600 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0061] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0062] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0063] The ZnF2 / MXene composite material and MXene material obtained in Example 1 were observed under a scanning electron microscope. The results were as follows: Figure 1 , Figure 2 As shown. Figure 1 and Figure 2 As can be seen in the figure, these two materials have a typical multi-layer MXene accordion-like structure.

[0064] The ZnF2 / MXene composite material MXene material obtained in this example was subjected to XRD test, and the results are as follows: Figure 3 As shown, combined with Figure 1 , Figure 2 It can be concluded that Example 1 successfully synthesized ZnF2 / MXene composite materials and MXene materials.

[0065] Example 2 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g of V2ZnC MAX and 1 g of polyvinylidene fluoride at the two ends of a corundum boat.

[0066] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 600 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0067] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0068] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0069] Example 3 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g V2ZnC MAX and 3 g polyvinylidene fluoride at the two ends of a corundum boat.

[0070] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 600 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0071] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0072] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0073] Example 4 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g of V2ZnC MAX and 7 g of polyvinylidene fluoride at the two ends of a corundum boat.

[0074] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 600 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0075] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0076] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0077] In Examples 1 to 4, the mass ratios of V2ZnC and polyvinylidene fluoride are different. When the mass ratio is 1: 1 and 1: 3, the amount of polyvinylidene fluoride is insufficient, resulting in insufficient amount of HF gas generated by decomposition, so that the etching is incomplete, and the Zn atoms cannot be completely converted into ZnF2, and MXene with an accordion structure cannot be generated. When the ratio is 1:7, due to the excessive amount of polyvinylidene fluoride, too much HF gas will be generated, resulting in excessive etching, which affects the retention of the MXene accordion structure. When the ratio is 1:5, MXene with an accordion structure can be generated, and Zn atoms can be completely converted into ZnF2. The MXene with an accordion structure and ZnF2 can play a better role in SEI protective film.

[0078] Example 5 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g V2ZnC MAX and 5 g polyvinylidene fluoride at the two ends of a corundum boat.

[0079] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 500 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0080] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0081] (4) After stirring, the solution was filtered using a water filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2CMXene.

[0082] Example 6 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g V2ZnC MAX and 5 g polyvinylidene fluoride at the two ends of a corundum boat.

[0083] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 550 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0084] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0085] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0086] Example 7 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g V2ZnC MAX and 5 g polyvinylidene fluoride at the two ends of a corundum boat.

[0087] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 700 °C at a heating rate of 5 °C / min under a nitrogen atmosphere and kept at this temperature for 30 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0088] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0089] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0090] Example 8 1. A method for preparing a ZnF2 / MXene composite material for an aqueous zinc ion battery negative electrode, comprising: (1) Place 1 g V2ZnC MAX and 5 g polyvinylidene fluoride at the two ends of a corundum boat.

[0091] (2) The corundum boat was placed in a tube furnace, and the temperature was raised to 600 °C at a heating rate of 1 °C / min under a nitrogen atmosphere and kept at this temperature for 60 min. After the temperature dropped to room temperature, the solid product was collected to obtain a ZnF2 / MXene composite material: ZnF2 / V2C MXene.

[0092] 2. A method for preparing MXene material from a ZnF2 / MXene composite negative electrode material, comprising the following steps: (3) Place the ZnF2 / MXene obtained in (2) into a beaker with 200 ml of water and ultrasonicate for 5 min. After the material is evenly dispersed in the water, place the beaker in a water bath and stir at 70 °C for 30 min.

[0093] (4) After stirring, the solution was filtered using a water-based filter paper, and the solid product obtained on the filter paper was vacuum dried at 60 °C for 12 h to obtain the MXene material: V2C MXene.

[0094] In Examples 5 to 8, by adjusting the temperature and the heating rate, it can be found that when the temperature is too low, for example, at 500°C, the Zn atomic layer cannot be completely etched. The SEM image of the ZnF2 / MXene composite material obtained in Example 5 is as follows: Figure 4 As shown, through Figure 4 It can be seen that the ZnF2 / MXene composite material has not yet formed an accordion shape; the XRD patterns of the ZnF2 / MXene composite materials obtained in Example 1 and Example 5 are as follows Figure 5 As shown, through Figure 5 It can be obtained that the ZnF2 / MXene composite material of Example 5 still has a lot of MAX phases when treated at 500°C, and the corresponding zinc fluoride XRD peak is weak. The ZnF2 / MXene composite material of Example 1 has the most zinc fluoride.

[0095] When the temperature is too high, the "M" layer atoms are easily oxidized to form oxides; when the heating rate is too slow and the holding time is extended, for example, 1 ℃ / min, 60 min, it will lead to excessive etching of MXene, affecting its morphology. When the temperature is 600℃, the heating rate is 5 ℃ / min, and the holding time is 30 min, the morphology can be guaranteed and the Zn atomic layer can be completely etched, and the "M" layer atoms are not oxidized.

[0096] Example 9 1. The ZnF2 / MXene composite material, carbon black, PVDF and solvent prepared in Example 1 are mixed and ground into a slurry, the mass ratio of ZnF2 / MXene: carbon black: PVDF is 7:2:1, the solvent is NMP, and the amount of solvent added is 15% of the mass of the binder PVDF.

[0097] 2. The slurry was coated on a glass plate with a 0.2 mm thick zinc foil by a doctor blade method, and the slurry thickness was 100 μm.

[0098] 3. Place the glass plate in a vacuum drying oven at 60 °C and dry for 7 h. Use a 12 mm diameter cutter to cut the glass plate into electrodes.

[0099] The two pole pieces prepared in Example 9 were respectively used as the positive electrode and the negative electrode to assemble a symmetrical battery, and a cycle life test was performed. Symmetric batteries were prepared using zinc foil alone and the MXene material in Example 1 for comparison. The results are shown in FIG. Figure 6 As shown. Figure 6 It can be seen that the symmetrical battery provided with a ZnF2 / MXene composite material coating of the present application exhibits a better service life of more than 1200 h.

[0100] The ZnF2 / MXene composite material prepared in Example 5 was used to obtain a pole piece using the method of Example 9, and was assembled into a symmetrical battery for a cycle life test. The results obtained are as follows: Figure 7 As shown, through Figure 7 The service life can be obtained to be about 160 h.

[0101] The two pole pieces prepared in Example 9 were used as the positive electrode and the negative electrode to assemble a symmetrical battery. -2 ) and a symmetrical battery was prepared using zinc foil alone and the MXene material in Example 1 as a comparison, as shown in the following figure: Figure 8 The results shown by Figure 8 It can be seen that the symmetrical battery provided with a ZnF2 / MXene composite material coating of the present application can still exhibit a good service life.

[0102] The two pole pieces prepared in Example 9 were respectively used as the positive electrode and the negative electrode to assemble a symmetrical battery, and the rate performance test was performed. Symmetric batteries were prepared using zinc foil alone and the MXene material in Example 1 as a comparison, and the results were as follows: Fig. 9 The results shown by Fig. 9 It can be concluded that the symmetrical battery provided with a ZnF2 / MXene composite material coating of the present application has good rate performance.

[0103] The electrode sheet prepared in Example 9 was used as the negative electrode and assembled into a full battery with ZVO (zinc vanadate) for cycle performance test. The MXene material in Example 1 was used as the negative electrode and ZVO (zinc vanadate) was used as the positive electrode to assemble a full battery for comparison. Fig.10 The results shown by Fig.10 It can be obtained that the symmetrical battery provided with a ZnF2 / MXene composite material coating of the present application has a better service life.

[0104] Example 10 1. The ZnF2 / MXene composite material, carbon black, PVDF and solvent prepared in Example 1 are mixed and ground into a slurry, the mass ratio of ZnF2 / MXene: carbon black: PVDF is 6:3:1, the solvent is NMP, and the amount of solvent added is 15% of the mass of the binder PVDF.

[0105] 2. The slurry was coated on a glass plate with a 0.2 mm thick zinc foil pasted on it, and the slurry thickness was 100 μm.

[0106] 3. Place the glass plate in a vacuum drying oven at 60 °C and dry for 7 h. Use a 12 mm diameter cutter to cut the glass plate into electrodes.

[0107] Embodiment 11 1. The ZnF2 / MXene composite material, carbon black, PVDF and solvent prepared in Example 1 are mixed and ground into a slurry, the mass ratio of ZnF2 / MXene: carbon black: PVDF is 8:1:1, the solvent is NMP, and the amount of solvent added is 15% of the mass of the binder PVDF.

[0108] 2. The slurry was coated on a glass plate with a 0.2 mm thick zinc foil pasted on it, and the slurry thickness was 100 μm.

[0109] 3. Place the glass plate in a vacuum drying oven at 60 °C and dry for 7 h. Use a 12 mm diameter cutter to cut the glass plate into electrodes.

[0110] Example 12 1. The ZnF2 / MXene composite material prepared in Example 1, PVDF and a solvent were mixed and ground into a slurry, the mass ratio of ZnF2 / MXene: PVDF was 9:1, the solvent was NMP, and the amount of solvent added was 15% of the mass of the binder PVDF.

[0111] 2. The slurry was coated on a glass plate with a 0.2 mm thick zinc foil pasted on it, and the slurry thickness was 100 μm.

[0112] 3. Place the glass plate in a vacuum drying oven at 60 °C and dry for 7 h. Use a 12 mm diameter cutter to cut the glass plate into electrodes.

[0113] In Examples 9 to 12, the ratios of ZnF2 / MXene, carbon black and PVDF are different. Among the obtained pole pieces, the coating on the pole piece of Example 9 has the best protective effect on the zinc base layer of the negative electrode and the best conductivity. In Example 10, the amount of ZnF2 / MXene composite material added is small, and the amount of carbon black is large, resulting in poor hydrophobic effect of the coating, more serious hydrogen evolution reaction, and poor protective effect on the zinc base layer of the negative electrode. In Examples 11 and 12, there is less or no carbon black, so the conductivity is poor.

[0114] Embodiment 13 1. The ZnF2 / MXene composite material, carbon black, CMC and solvent prepared in Example 1 are mixed and ground into a slurry, the mass ratio of ZnF2 / MXene: carbon black: CMC is 7:2:1, the solvent is water, and the amount of solvent added is 15% of the mass of the binder PVDF.

[0115] 2. The slurry was coated on a glass plate with a 0.2 mm thick zinc foil pasted on it, and the slurry thickness was 100 μm.

[0116] 3. Place the glass plate in a vacuum drying oven at 60 °C and dry for 7 h. Use a 12 mm diameter cutter to cut the glass plate into electrodes.

[0117] Compared with Example 9, Example 13 uses a different type of binder from Example 9. Since the solvent of CMC is water, the contact between the ground slurry and the zinc foil is not tight and is easy to fall off, thus affecting the performance of the battery.

[0118] Embodiment 14 1. The ZnF2 / MXene composite material, carbon black, PVDF and solvent prepared in Example 1 are mixed and ground into a slurry, the mass ratio of ZnF2 / MXene: carbon black: PVDF is 7:2:1, the solvent is NMP, and the amount of solvent added is 15% of the mass of the binder PVDF.

[0119] 2. The slurry was coated on a glass plate with a 0.2 mm thick zinc foil pasted on it, and the slurry thickness was 100 μm.

[0120] 3. Place the glass plate in a vacuum drying oven at 110 °C and dry for 7 h. Use a 12 mm diameter cutter to cut the glass plate into electrodes.

[0121] Compared with Example 9, the drying temperature of Example 14 is different from that of Example 9. At a drying temperature of 110° C., the solvent will evaporate quickly, and the slurry will have slight cracking and small-scale shedding, thereby affecting the life of the battery.

[0122] In addition, although exemplary embodiments have been described herein, the scope includes any and all embodiments based on the present application with equivalent elements, modifications, omissions, combinations (e.g., various embodiments intersecting schemes), adaptations or changes. The elements in the claims are to be interpreted broadly based on the language adopted in the claims, and are not limited to the examples described in this specification or during the practice of this application, and the examples are to be interpreted as non-exclusive. Therefore, this specification and examples are intended to be considered as examples only, and the true scope and spirit are indicated by the following claims and the full scope of their equivalents.

[0123] The above description is intended to be illustrative rather than restrictive. For example, the above examples (or one or more schemes thereof) may be used in combination with each other. For example, a person of ordinary skill in the art may use other embodiments when reading the above description. In addition, in the above-mentioned specific embodiments, various features may be grouped together to simplify the present application. This should not be interpreted as an intention that a feature of an application that does not require protection is necessary for any claim. On the contrary, the subject matter of the present application may be less than all the features of an embodiment of a particular application. Thus, the following claims are incorporated herein in the specific embodiments as examples or embodiments, wherein each claim is independently a separate embodiment, and it is considered that these embodiments may be combined with each other in various combinations or arrangements. The scope of the present invention should be determined with reference to the appended claims and the full scope of equivalent forms granted by these claims.

[0124] The above embodiments are only exemplary embodiments of the present application and are not intended to limit the present invention. The protection scope of the present invention is defined by the claims. Those skilled in the art may make various modifications or equivalent substitutions to the present invention within the essence and protection scope of the present application, and such modifications or equivalent substitutions shall also be deemed to fall within the protection scope of the present invention.

Claims

1. A negative electrode material for an aqueous zinc ion battery, It is characterized in that The negative electrode material comprises a zinc base layer and a coating on the zinc base layer, wherein the coating comprises ZnF 2 / MXene composites and binders, ZnF 2 / MXene composites including ZnF 2 and MXene, the ZnF 2 and MXene are connected by intermolecular forces, and the molecular formula of the MXene is M a X b , wherein M is a transition metal element, X is a carbon or nitrogen element, a is 2 or 3, b is 1 or 2, and the ZnF 2 / MXene composites have an accordion shape.

2. The negative electrode material according to claim 1, It is characterized in that The thickness of the coating is 15 to 30 microns.

3. The negative electrode material according to claim 1, It is characterized in that The binder includes PVDF or CMC.

4. The negative electrode material according to claim 1, It is characterized in that The material of the zinc base layer is metallic zinc; the thickness of the zinc base layer is 0.2-1.5 mm.

5. A method for preparing the negative electrode material of an aqueous zinc ion battery according to any one of claims 1 to 4, It is characterized in that The preparation method comprises: ZnF 2 The / MXene composite material is mixed with a solvent and a binder to form a slurry; the slurry is applied on a zinc base layer, and the slurry is dried to form a coating to obtain a negative electrode material.

6. The preparation method according to claim 5, It is characterized in that The slurry is dried at a temperature of 50-80°C and for a drying time of 6-24 h.

7. The preparation method according to claim 5, It is characterized in that The solvent includes NMP or water.

8. The preparation method according to claim 5, It is characterized in that The amount of solvent added is 5%~30% of the binder mass.

9. The preparation method according to claim 5, It is characterized in that The ZnF 2 The preparation method of the / MXene composite material is as follows: a MAX phase solid material and a fluorine-containing organic substance are placed at different positions in a closed environment, the A layer in the MAX phase material is Zn, and ZnF is obtained by reaction under protective atmosphere and heating conditions. 2 / MXene composites.

10. Use of the negative electrode material for an aqueous zinc ion battery according to any one of claims 1 to 4 and the method for preparing the negative electrode material for an aqueous zinc ion battery according to any one of claims 5 to 9 in an aqueous zinc ion battery.