Corrosion-resistant flow battery collector plate and preparation method thereof
Through multi-step processing of vanadium source, carbon source and graphitization catalyst, corrosion-resistant liquid flow battery current collector plate is prepared, which solves the corrosion problem of conductive current collector plate in the acid-base and oxidation environment in the prior art, and improves the conductivity and mechanical properties, avoiding resistance and leakage risks.
Patent Information
- Application Number
- CN202411297351.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
AI Technical Summary
The existing flow battery conductive current collector plates are prone to corrosion in acid-base and oxidation environments, and the graphite plates are highly brittle and the conductivity of carbon plastic composite materials are low, resulting in increased resistance and contact resistance problems. The existing improvement measures have the risk of leakage.
By mixing vanadium source, carbon source and graphitization catalyst evenly, curing and forming, carbonization, carbon vanadium synthesis and graphitization treatment, corrosion-resistant liquid flow battery current collector plate can be prepared directly in acid-base and strong oxidation environments Contact the electrolyte without corrosion.
The current collector of the current flow battery is realized without corrosion in acid-base and strong oxidation environments, which improves the conductivity and mechanical properties, and avoids the risk of increased resistance and leakage.
Smart Images

Figure CN118970085A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of liquid flow batteries, and in particular relates to a corrosion-resistant liquid flow battery current collecting plate and a preparation method thereof. Background Art
[0002] Copper is usually the first choice for conductive current collectors in flow batteries due to its ultra-high electrical conductivity. However, copper has poor acid, alkali and oxidation resistance, so it cannot be directly exposed to the electrolyte. Existing improvement measures for conductive current collectors in flow batteries include:
[0003] (a) Using bipolar plates made of graphite plates or carbon-plastic composite materials to protect the copper current collector;
[0004] (b) A layer of corrosion-resistant conductive material is sprayed on the copper current collecting plate using a spraying process.
[0005] However, the above methods all have big problems:
[0006] In measure (a), the graphite plate is brittle and easy to break, while the carbon-plastic composite material has poor electrical conductivity, resulting in large resistance. In addition, these two methods will generate contact resistance between the electrode and the current collector.
[0007] In measure (b), the use of a spraying process results in a greater increase in resistance.
[0008] Moreover, both measures (a) and (b) have the potential risk of leakage points corroding the copper plate. Summary of the invention
[0009] In view of the above problems, the present invention provides a corrosion-resistant liquid flow battery current collector and a preparation method thereof.
[0010] The method for preparing a corrosion-resistant liquid flow battery current collector provided by the present invention comprises the following steps:
[0011] S1. Evenly mix the vanadium source, the carbon source and the graphitization catalyst and solidify and shape the mixture in a mold to obtain a sheet material;
[0012] S2, drying the sheet material after demoulding to obtain a dry embryo;
[0013] S3, carbonizing the dried embryo;
[0014] S4, subjecting the dried embryo to carbon-vanadium synthesis;
[0015] S5, graphitizing the dried embryo.
[0016] further,
[0017] The step S1 comprises the following steps:
[0018] S11, weighing the vanadium source, requiring its particle size to be ≤15 μm;
[0019] S12, weighing a carbon source and a curing agent according to the carbon content of the carbon source at a carbon-vanadium ratio of 1 to 2.5:1;
[0020] S13, adding the vanadium source to the carbon source and stirring evenly, then adding 1.5-2.5 wt % of a graphitization catalyst and mixing evenly to obtain a first mixture;
[0021] S14, adding the curing agent to the first mixture and stirring the mixture sufficiently to obtain a second mixture, and pouring the second mixture into a mold and curing the mold to obtain the sheet material.
[0022] further,
[0023] In the step 2, the sheet material is dried naturally, or the sheet material is dried in an oven at 120-180°C.
[0024] further,
[0025] The step S3 comprises the following steps:
[0026] S31, placing the dried embryo into a graphitization furnace, and evacuating the graphitization furnace to a vacuum degree less than 100 Pa;
[0027] S32, heating the graphitization furnace at a heating rate of 3 to 8°C / min;
[0028] S33, heating the graphitization furnace to a carbonization temperature of 300 to 800°C, and maintaining the carbonization temperature for 2 to 4 hours.
[0029] further,
[0030] In the step S4, the graphitization furnace is heated to the carbon-vanadium synthesis temperature at a heating rate of 1 to 5°C / min, the carbon-vanadium synthesis temperature is 1200 to 1800°C, and the carbon-vanadium synthesis temperature is maintained for 1 to 3 hours to perform carbon-vanadium synthesis to obtain vanadium carbide.
[0031] further,
[0032] In the step S5, the graphitization furnace is switched to the protective gas state and then heated to the graphitization temperature at a heating rate of 0.5 to 1.5°C / min. The graphitization temperature is 2100 to 2400°C. The graphitization temperature is maintained for 0.5 to 1.5 hours, and the dry embryo is graphitized under the catalysis of a graphitization catalyst.
[0033] further,
[0034] In step S5, the graphitization furnace is switched to a protective gas state, filled with argon or helium, and then heated.
[0035] further,
[0036] In the step S11, the particle size of the vanadium source is ≤15 μm;
[0037] In the step S12, the carbon to vanadium ratio is 1.5 to 2:1 molar ratio;
[0038] In the step S13, the graphitization catalyst is 2 wt%;
[0039] In the step 2, the sheet is dried in an oven at 150°C;
[0040] In the step S31, the graphitization furnace is evacuated to a vacuum degree less than 50 Pa;
[0041] In step S32, the heating rate is 5°C / min;
[0042] In the step S33, the carbonization temperature is 500° C., and the carbonization temperature is maintained for 3 hours;
[0043] In the step S4, the heating rate is 3°C / min, the carbon-vanadium synthesis temperature is 1500°C, and the carbon-vanadium synthesis temperature is maintained for 2 hours;
[0044] In the step S5, the heating rate is 1°C / min, the graphitization temperature is 2100°C, and the graphitization temperature is preferably maintained for 1 hour.
[0045] further,
[0046] The vanadium source is one of the following materials: vanadium pentoxide, vanadium dioxide, vanadium trioxide, ammonium metavanadate;
[0047] The carbon source is one of the following materials: epoxy resin, phenolic resin, phenolic ketone resin;
[0048] The graphitization catalyst is boric acid or boric anhydride.
[0049] The present invention also provides a corrosion-resistant liquid flow battery current collector plate, which is prepared by the above-mentioned corrosion-resistant liquid flow battery current collector plate preparation method.
[0050] The corrosion-resistant liquid flow battery collector plate provided by the present invention can withstand the acid, alkali and strong oxidation environment of the liquid flow battery and directly contact the electrolyte of the liquid flow battery without corrosion.
[0051] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0053] Figure 1 A flow chart of a method for preparing a corrosion-resistant liquid flow battery current collector plate according to an embodiment of the present invention is shown. DETAILED DESCRIPTION
[0054] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by technicians in the technical field to which this application belongs; the terms used in the specification of the application herein are only for the purpose of describing specific embodiments and are not intended to limit this application; the terms "including" and "having" in the specification and claims of this application and the above-mentioned figure descriptions and any variations thereof are intended to cover non-exclusive inclusions. The terms "first", "second", "third", etc. in the specification and claims of this application or the above-mentioned figures are used to distinguish different objects, not to describe a specific order or a primary and secondary relationship. "Multiple" appearing in this application refers to more than two (including two).
[0056] Reference to "embodiments" herein means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the present application. The appearance of the phrase in various locations in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described herein may be combined with other embodiments.
[0057] Figure 1The present invention provides a flow chart of the method for preparing a corrosion-resistant liquid flow battery current collector plate. The method for preparing a corrosion-resistant liquid flow battery current collector plate comprises the following steps.
[0058] S1, mixing the vanadium source, carbon source and graphitization catalyst uniformly and solidifying and forming the mixture in a mold to obtain a sheet material. This step specifically includes the following steps:
[0059] S11, weighing a certain amount of vanadium source such as vanadium pentoxide, the particle size is required to be ≤15μm, preferably ≤10μm, if the requirement is not met, add a small amount of anhydrous ethanol to grind, dry and set aside, wherein the vanadium source can also be any one of vanadium dioxide, vanadium trioxide, and ammonium metavanadate;
[0060] S12, according to the carbon-vanadium ratio of 1 to 2.5:1, preferably 1.5 to 2:1 molar ratio, weigh the carbon source and the curing agent corresponding to the carbon source according to the carbon content of the carbon source such as epoxy resin, wherein the carbon source can also be any one of phenolic resin and phenolic ketone resin, and the curing agent used for the carbon source is well known to technicians, and the specific materials are not repeated here;
[0061] S13, adding the vanadium source such as vanadium pentoxide obtained in step S11 to a carbon source such as epoxy resin, stirring evenly, and then adding 1.5-2.5wt%, preferably 2wt% of a graphitization catalyst, boric acid or boric anhydride, and mixing evenly to obtain a first mixture;
[0062] S14, adding a curing agent to the first mixture and stirring thoroughly to obtain a second mixture, pouring the second mixture into a mold and curing it to obtain a sheet material, wherein the curing may be natural curing or heating curing, and the latter may be determined by a technician according to the working conditions.
[0063] S2, after demoulding the sheet material, drying it is performed to obtain a dry embryo.
[0064] The sheet material may be dried naturally or in an oven at 120-180°C, preferably 150°C.
[0065] S3, carbonizing the dried embryo. This step specifically includes the following steps:
[0066] S31, placing the dried embryo into a graphitization furnace, and evacuating the graphitization furnace to a vacuum degree of less than 100 Pa (Pa), preferably less than 50 Pa;
[0067] S32, heating the graphitization furnace at a heating rate of 3 to 8°C / min (degrees Celsius per minute), preferably 5°C / min;
[0068] S33, heating the graphitization furnace to a carbonization temperature of 500-800°C, preferably 500°C, and maintaining the carbonization temperature for 2-4 hours, preferably 3 hours, so that the epoxy resin in the dry embryo is fully carbonized, and other gaseous components of carbonization cracking are removed under vacuum conditions to avoid affecting the subsequent carbon-vanadium reaction.
[0069] S4, subjecting the dry embryo to carbon-vanadium synthesis.
[0070] The graphitization furnace is heated to the carbon-vanadium synthesis temperature at a heating rate of 1 to 5°C / min, preferably 3°C / min, the carbon-vanadium synthesis temperature is 1200 to 1800°C, preferably 1500°C, and the carbon-vanadium synthesis temperature is maintained for 1 to 3 hours, preferably 2 hours, to perform carbon-vanadium synthesis to obtain vanadium carbide.
[0071] S5, graphitizing the dry embryo. Considering that after the above steps, there is excess carbon in the dry embryo in the form of amorphous carbon, in order to improve the machining performance and higher conductivity of the current collector, the excess amorphous carbon needs to be further converted into graphite, so the dry embryo needs to be graphitized.
[0072] The graphitization furnace is switched to the protective gas state, filled with argon or helium and heated to the graphitization temperature, the heating rate is 0.5-1.5°C / min, preferably 1°C / min, the graphitization temperature is 1800-2400°C, preferably 2100°C, the graphitization temperature is maintained for 0.5-1.5 hours, preferably 1 hour, and the dry embryo is graphitized under the catalysis of the graphitization catalyst to obtain a liquid flow battery current collector.
[0073] Finally, the graphitization furnace is cooled to room temperature, and the prepared liquid flow battery current collector is taken out.
[0074] The present invention also provides a corrosion-resistant liquid flow battery current collector plate made by the above-mentioned corrosion-resistant liquid flow battery current collector plate preparation method. The current collector plate can withstand the acid, alkali and strong oxidizing environment of the liquid flow battery and directly contact the electrolyte of the liquid flow battery without corrosion.
[0075] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a corrosion-resistant liquid flow battery current collector, characterized in that: Includes steps: S1. Mixing the vanadium source, the carbon source and the graphitization catalyst uniformly and then curing and molding the mixture in a mold to obtain a sheet material; S2, drying the sheet material after demoulding to obtain a dry embryo; S3, carbonizing the dried embryo; S4, subjecting the dried embryo to carbon-vanadium synthesis; S5, graphitizing the dried embryo.
2. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 1, characterized in that: The step S1 comprises the following steps: S11, weighing the vanadium source, requiring its particle size to be ≤15 μm; S12, weighing a carbon source and a curing agent according to the carbon content of the carbon source at a carbon-vanadium ratio of 1 to 2.5:1; S13, adding the vanadium source to the carbon source and stirring evenly, then adding 1.5-2.5 wt % of a graphitization catalyst and mixing evenly to obtain a first mixture; S14, adding the curing agent to the first mixture and stirring the mixture sufficiently to obtain a second mixture, and pouring the second mixture into a mold and curing the mold to obtain the sheet material.
3. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 2, characterized in that: In the step 2, the sheet material is dried naturally or in an oven at 120-180°C.
4. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 3, characterized in that: The step S3 comprises the following steps: S31, placing the dried embryo into a graphitization furnace, and evacuating the graphitization furnace to a vacuum degree less than 100 Pa; S32, heating the graphitization furnace at a heating rate of 3 to 8°C / min; S33, heating the graphitization furnace to a carbonization temperature of 500 to 800°C, and maintaining the carbonization temperature for 2 to 4 hours.
5. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 4, characterized in that: In the step S4, the graphitization furnace is heated to the carbon-vanadium synthesis temperature at a heating rate of 1 to 5°C / min, the carbon-vanadium synthesis temperature is 1200 to 1800°C, and the carbon-vanadium synthesis temperature is maintained for 1 to 3 hours to perform carbon-vanadium synthesis to obtain vanadium carbide.
6. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 5, characterized in that: In the step S5, the graphitization furnace is switched to the protective gas state and then heated to the graphitization temperature at a heating rate of 0.5 to 1.5°C / min. The graphitization temperature is 2100 to 2400°C. The graphitization temperature is maintained for 0.5 to 1.5 hours, and the dry embryo is graphitized under the catalysis of a graphitization catalyst.
7. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 6, characterized in that: In step S5, the graphitization furnace is switched to a protective gas state, filled with argon or helium, and then heated.
8. The method for preparing a corrosion-resistant liquid flow battery current collector according to claim 7, characterized in that: In the step S11, the particle size of the vanadium source is ≤15 μm; In the step S12, the carbon to vanadium ratio is 1.5 to 2:1 molar ratio; In the step S13, the graphitization catalyst is 2 wt%; In the step 2, the sheet is dried in an oven at 150°C; In the step S31, the graphitization furnace is evacuated to a vacuum degree less than 50 Pa; In step S32, the heating rate is 5°C / min; In the step S33, the carbonization temperature is 500° C., and the carbonization temperature is maintained for 3 hours; In the step S4, the heating rate is 3°C / min, the carbon-vanadium synthesis temperature is 1500°C, and the carbon-vanadium synthesis temperature is maintained for 2 hours; In the step S5, the heating rate is 1°C / min, the graphitization temperature is 2100°C, and the graphitization temperature is preferably maintained for 1 hour.
9. The method for preparing a corrosion-resistant liquid flow battery current collector according to any one of claims 1 to 8, characterized in that: The vanadium source is one of the following materials: vanadium pentoxide, vanadium dioxide, vanadium trioxide, ammonium metavanadate; The carbon source is one of the following materials: epoxy resin, phenolic resin, phenolic ketone resin; The graphitization catalyst is boric acid or boric anhydride.
10. A corrosion-resistant liquid flow battery current collector, characterized in that: The corrosion-resistant liquid flow battery collector plate is prepared by the method for preparing the corrosion-resistant liquid flow battery collector plate according to any one of claims 1 to 9.