Solid-state battery polymer electrolyte and preparation method and application thereof

By using carbon nanotubes treated with dielectric resistive discharge plasma in lithium metal batteries to fill PVDF-TRFE-CFE polymer electrolytes, the safety problems of liquid organic electrolytes and poor interface contact of solid inorganic electrolytes in lithium metal batteries are solved. A high-performance solid-state battery polymer electrolyte is realized, improving the cycle stability and energy density of the battery.

CN118970165APending Publication Date: 2024-11-15ZHEJIANG SCI-TECH UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411028218.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

There are safety problems in liquid organic electrolytes in existing lithium metal batteries, such as flammability, explosion risks and lithium dendrites growth, and the interface contact and processing conditions of solid inorganic electrolytes are unfavorable, affecting their application.

Method used

Multi-walled carbon nanotubes treated with dielectric resistive discharge plasma sulfonication are filled with PVDF-TRFE-CFE polymer film to form a high-performance solid-state battery polymer electrolyte. Three-dimensional structural electrolyte is prepared by casting to enhance its ionic conductivity. and lithium dendrites inhibitory ability.

Benefits of technology

It improves the ionic conductivity and mechanical properties of lithium metal batteries, reduces lithium dendrites and electrolyte consumption, improves the interface contact between the electrode and the electrolyte, and improves the cycle stability and energy density of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970165A_ABST
    Figure CN118970165A_ABST
Patent Text Reader

Abstract

The invention discloses a solid-state battery polymer electrolyte as well as a preparation method and application thereof, the polymer electrolyte is a PVDF-TRFE-CFE polymer film taking a carbon nanotube subjected to sulfonation treatment by dielectric barrier discharge plasma as a filler, and the carbon nanotube filler has high ionic conductivity; after dielectric barrier discharge sulfonation treatment, the conductivity and the dispersity in a polymer are enhanced, and the PVDF-based polymer electrolyte with the uniformly dispersed carbon nanotube filler can effectively inhibit lithium dendrites from penetrating an electrolyte membrane, so that a three-dimensional structure polymer electrolyte with stable ion / electron transmission is formed; the interface contact between the electrode and the electrolyte is improved, the problems of low ionic conductivity and high impedance of the polymer electrolyte are greatly improved, and the problems that insufficient interface contact between the electrode and the electrolyte is not beneficial to ion transmission and easy to induce polarization are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of solid-state lithium metal battery polymer electrolytes, and specifically relates to a DBD plasma technology-modified multi-walled carbon nanotube filled in a PVDF-based solid-state battery polymer electrolyte, and a preparation method and application thereof. Background Art

[0002] With the increasing global environmental pollution, energy demand, resource shortage and other problems, green and sustainable alternative energy sources such as solar energy, wind energy and tidal energy have attracted widespread attention. Among them, lithium-ion batteries have been widely used in electric vehicles due to their low self-discharge, high energy density and no memory effect, and they also play an important role in energy storage and conversion. However, the expanding consumer market has put forward higher requirements on the energy density and safety of lithium-ion batteries, which has prompted us to continuously improve and optimize lithium-ion battery systems. High-capacity electrode materials and wide electrochemical windows are the key to obtaining high energy density storage. In recent years, due to the excellent theoretical specific capacity of lithium metal anode, batteries assembled from lithium metal anode and high-capacity cathode or high-voltage cathode have achieved higher energy storage compared with traditional commercial lithium-ion batteries. However, lithium metal batteries have always had safety issues with liquid organic electrolytes. Generally, volatile and flammable liquid organic electrolytes are prone to burn and burst when the battery is subjected to severe impact or damage. Uncontrolled lithium dendrite growth will continuously consume electrolytes and increase the risk of short circuits. In addition, liquid organic electrolytes are unstable under high voltage, which hinders the application of high-voltage cathodes to improve energy density.

[0003] In order to solve the above problems, solid electrolytes are proposed to replace liquid organic electrolytes. Generally speaking, solid electrolytes SSEs have a larger electrochemical stability window than liquid organic electrolytes, can match high-voltage cathodes, and avoid the risk of liquid electrolyte leakage and volatilization. At the same time, combined with excellent mechanical strength, SSE can prevent lithium dendrite growth and electrolyte consumption. Stable lithium transport and deposition can improve the cycle stability of all-solid-state lithium batteries.

[0004] Although solid inorganic electrolytes have excellent conductivity, mechanical properties and safety, poor interface contact and unfavorable processing conditions hinder their further application. Solid polymer electrolytes have excellent flexibility and mechanical properties, and have improved interface contact and processing properties, and have received extensive attention and research in the field of solid electrolytes. Polyethylene oxide-based electrolytes (PEO) have a small dielectric constant and low lithium ion conductivity. However, polyvinylidene fluoride (PVDF) with a high relative dielectric constant increases the dissociation of lithium salts. In addition, the PVDF matrix has other outstanding properties of solid polymer electrolytes, such as: 1) flexibility and mechanical strength; 2) a large electrochemical stability window; 3) good thermal stability. There is still much room for improvement in the combined performance of polyvinylidene fluoride-based solid polymer electrolytes (PVDF-SPE), especially in terms of ionic conductivity. Therefore, it is of great significance to design a high-performance PVDF-based polymer electrolyte. Summary of the invention

[0005] A technical problem to be solved by the present invention is to provide a PVDF-based three-dimensional solid-state battery polymer electrolyte, which mainly solves the problems of low ion conductivity and lithium dendrites in current polymer electrolytes.

[0006] The technical solution adopted by the polymer electrolyte to solve the above technical problems is: a solid-state battery polymer electrolyte, wherein the polymer electrolyte is a PVDF-TRFE-CFE polymer film filled with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation.

[0007] Preferably, the thickness of the polymer electrolyte is 80 μm to 120 μm. Polymer electrolytes of this thickness are most suitable. A larger thickness will limit the energy density of solid-state batteries; a smaller thickness will reduce mechanical properties, weaken the polymer electrolyte's resistance to lithium dendrites, and increase the possibility of short circuits.

[0008] Preferably, the mass fraction of the carbon nanotubes treated by dielectric barrier discharge plasma sulfonation is 1-5 mass %.

[0009] Another technical problem to be solved by the present invention is to provide a method for preparing the above-mentioned solid-state battery polymer electrolyte, which specifically comprises the following steps:

[0010] S1: subjecting the purified carbon nanotubes to dielectric barrier discharge plasma sulfonation treatment to obtain modified carbon nanotubes;

[0011] S2 disperses the modified carbon nanotubes and adds them to the polymer electrolyte solution, which is coated on the mold by casting. After vacuum drying, a PVDF-TRFE-CFE polymer film with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation as filler is obtained.

[0012] Preferably, the processing method for purifying carbon nanotubes in step S1 is:

[0013] A1: The aggregated carbon nanotubes prepared by chemical vapor deposition were calcined at 300°C for 30 min in a muffle furnace, and then heated to 800°C in a quartz tube furnace under argon protection for 10 min at a heating rate of 5°C / min.

[0014] A2: immersing the carbon nanotubes heated in step A1 into an excess of 1 mol / L hydrochloric acid solution at a temperature of 100°C for 2 hours;

[0015] A3: separating the carbon nanotubes treated with acid in step A2 into solid and liquid by centrifugation or filtration, and drying the obtained solid to obtain the purified carbon nanotubes.

[0016] Preferably, the dielectric barrier discharge plasma sulfonation treatment in step S1 is specifically as follows:

[0017] The purified carbon nanotubes were dispersed in a solution with a concentration of 1 mol L -1 H 2 SO 4 Dielectric barrier discharge is carried out in the solution, the discharge power is 50mA / 60V, and the discharge time is 15min~1.5h. Atmospheric pressure dielectric barrier discharge plasma discharge technology can be used to modify the surface properties of various materials, such as 1. Enhance the surface hydrophilicity and wettability of the material; 2. Reduce the friction coefficient of the material surface; 3. Improve the wear resistance of the material; 4. Increase the dispersibility of powder materials; 5. It can also be used to prepare materials with special surface morphology, such as nanostructures, micro-nanostructures, etc.

[0018] Preferably, the polymer electrolyte solution in step S2 is formed by stirring a polymer blend obtained by dissolving PVDF-TRFE-CFE and N,N-dimethylformamide and lithium bis(trifluoromethanesulfonyl)imide at a mass ratio of 1:0.2-1.2 for 48 hours.

[0019] Preferably, in step S2, 0.1 g of PVDF-TRFE-CFE is dissolved in every 1 mL of N,N-dimethylformamide in the polymer blend.

[0020] Preferably, in step S2, the modified carbon nanotubes are dispersed and added to the polymer electrolyte solution, coated on a polytetrafluoroethylene mold, and placed in a vacuum drying oven at 60° C. for 48 hours.

[0021] Compared with the prior art, the advantages of the solid-state battery polymer electrolyte and the preparation method thereof are as follows: the high-performance three-dimensional structure of the carbon nanotubes modified by dielectric barrier discharge plasma makes the solid-state battery polymer electrolyte have excellent ionic conductivity and strong lithium dendrite inhibition ability, solving the problem of unsatisfactory ionic conductivity caused by the high crystallinity of PVDF at room temperature limiting the movement of chain segments and the diffusion ability of ions; the PVDF-TRFE-CFE polymer film inherits the flexibility and mechanical strength of PVDF, and has high mechanical properties when mixed with lithium salts and other plasticizers, and can reduce the generation of dendrites and consumption of electrolyte; because the carbon nanotube filler has high ionic conductivity, its conductivity and dispersibility in the polymer are enhanced after dielectric barrier discharge sulfonation treatment, and the PVDF-based polymer electrolyte with uniformly dispersed carbon nanotube fillers can effectively inhibit lithium dendrites from penetrating the electrolyte membrane, forming a three-dimensional structure electrolyte with stable ion / electron transmission, improving the interface contact between the electrode and the electrolyte, greatly improving the problem of low ionic conductivity and high impedance of the polymer electrolyte, and solving the problem that insufficient interface contact between the electrode and the electrolyte is not conducive to ion transmission and is easy to induce polarization.

[0022] Therefore, a technical problem also solved by the present invention is the application of the above-mentioned solid-state battery polymer electrolyte, which is installed between the positive electrode and the lithium metal negative electrode to form a solid-state lithium metal battery to promote the development of quasi-solid-state lithium metal batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The AC impedance spectrum of the solid-state battery polymer electrolyte of Verification Example 1 of the present invention is obtained by platinum plating as blocking electrodes by magnetron sputtering on both sides;

[0024] Figure 2 This is a scanning electron microscope image of a cross section of a solid-state battery polymer electrolyte of Verification Example 2 of the present invention;

[0025] Figure 3 The AC impedance spectrum of the lithium symmetric battery assembled with the solid-state battery polymer electrolyte of Verification Example 1 of the present invention;

[0026] Figure 4 The AC impedance spectrum of the lithium symmetric battery assembled with the solid-state battery polymer electrolyte of Verification Example 2 of the present invention;

[0027] Figure 5 The lithium symmetric battery assembled with the solid-state battery polymer electrolyte of Verification Example 2 of the present invention is 0.2 mA cm -2 Cyclic test diagram under current density. DETAILED DESCRIPTION

[0028] The following is a description of exemplary verification examples of the present invention in conjunction with the accompanying drawings, including various details of the verification examples of the present invention to facilitate understanding, which should be considered as merely exemplary. Therefore, it should be recognized by those of ordinary skill in the art that various changes and modifications can be made to the verification examples described herein without departing from the scope and spirit of the present invention. Similarly, for clarity and conciseness, the description of well-known functions and structures is omitted in the following description.

[0029] The present invention is a solid-state battery polymer electrolyte, wherein the polymer electrolyte is a polyvinylidene fluoride-trifluoroethylene-chlorofluoroethylene (PVDF-TRFE-CFE) polymer film filled with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation. The thickness of the polymer electrolyte is 80 μm to 120 μm. The mass fraction of the carbon nanotubes treated by dielectric barrier discharge plasma sulfonation is 1 to 5 mass%.

[0030] The preparation method of the solid-state battery polymer electrolyte specifically comprises the following steps:

[0031] S1: subjecting the purified carbon nanotubes to dielectric barrier discharge plasma sulfonation treatment to obtain carbon nanotubes treated with dielectric barrier discharge plasma sulfonation, which are referred to as modified carbon nanotubes;

[0032] S2 disperses the modified carbon nanotubes and adds them to the polymer electrolyte solution, which is coated on the mold by casting. After vacuum drying, a PVDF-TRFE-CFE polymer film with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation as filler is obtained.

[0033] Preferably, the processing method for purifying carbon nanotubes in step S1 is:

[0034] A1: The agglomerated carbon nanotubes prepared by chemical vapor deposition were sintered at 300°C for 30 minutes in a muffle furnace, and then heated to 800°C in a quartz tube furnace under argon protection for 10 minutes at a heating rate of 5°C / min, i.e., solid-phase sintering of carbon nanotubes.

[0035] A2: immersing the carbon nanotubes heated in step A1 into an excess of 1 mol / L hydrochloric acid solution at a temperature of 100°C and an acid treatment time of 2 hours; i.e., hydrochloric acid purification of the carbon nanotubes;

[0036] A3: separating the carbon nanotubes treated with acid in step A2 into solid and liquid by centrifugation or filtration, and drying the obtained solid to obtain the purified carbon nanotubes.

[0037] Preferably, the dielectric barrier discharge (DBD) plasma sulfonation treatment in step S1 is specifically as follows: the purified carbon nanotubes are dispersed in a solution having a concentration of 1 mol L -1H 2 SO 4 The solution was subjected to dielectric barrier discharge at a power of 50 mA / 60 V and a discharge time of 15 min to 1.5 h. After filtration, the solution was washed with deionized water until the pH value of the precipitate reached 7. Then, the purified carbon nanotubes treated by dielectric barrier discharge (DBD) plasma sulfonation were collected and placed in an oven for drying overnight to obtain modified carbon nanotubes.

[0038] Preferably, the polymer electrolyte solution in step S2 is formed by stirring a polymer blend obtained by dissolving PVDF-TRFE-CFE and N,N-dimethylformamide (DMF) and lithium bistrifluoromethanesulfonyl imide (LiTFSI) at a mass ratio of 1:0.2-1.2 for 48 hours.

[0039] Preferably, in step S2, 0.1 g of PVDF-TRFE-CFE is dissolved in every 1 mL of N,N-dimethylformamide in the polymer blend.

[0040] Preferably, in step S2, the modified carbon nanotubes are dispersed and added to the polymer electrolyte solution, coated on a polytetrafluoroethylene mold, and placed in a vacuum drying oven at 60° C. for 48 hours.

[0041] Verification Example 1

[0042] This verification example provides a method for preparing a three-dimensional structured fixed battery polymer electrolyte of a PVDF-TRFE-CFE polymer film with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation as filler, which specifically includes the following steps:

[0043] S1 Preparation of modified carbon nanotubes treated by DBD plasma sulfonation: using purified carbon nanotubes as substrate, sulfuric acid as DBD plasma discharge solution, sulfuric acid concentration of 1 mol / L, solution volume of 10 ml, purified carbon nanotube mass of 1 g, discharge voltage of 60 V, discharge current of 50 mA, discharge time of 15 min.

[0044] S2 prepares a three-dimensional structured fixed battery polymer electrolyte by adding modified carbon nanotube active filler: prepares a blended polymer based on PVDF, the mass of PVDF-TRFE-CFE is 0.2g, and the mass of N,N-dimethylformamide (DMF) is 2ml; the mass of lithium salt LiTFSI mixed in is 0.2g, the mass fraction of modified carbon nanotubes is adjusted to 5mass%, solution casting, vacuum drying, and the thickness of the PVDF-TRFE-CFE polymer film filled with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation is 120μm.

[0045] Verification Example 2

[0046] This verification example provides a second method for preparing a three-dimensional structured fixed battery polymer electrolyte using a PVDF-TRFE-CFE polymer film filled with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation, which specifically includes the following steps:

[0047] S1 Preparation of modified carbon nanotubes treated by DBD plasma sulfonation: using purified carbon nanotubes as substrate, sulfuric acid as DBD plasma discharge solution, sulfuric acid concentration of 1 mol / L, solution volume of 10 ml, purified carbon nanotube mass of 1 g, discharge voltage of 60 V, discharge current of 50 mA, discharge time of 1 h.

[0048] S2 prepares a three-dimensional structured fixed battery polymer electrolyte by adding modified carbon nanotube active filler: prepares a blended polymer based on PVDF, the mass of PVDF-TRFE-CFE is 0.2g, and the mass of N,N-dimethylformamide (DMF) is 2ml; the mass of lithium salt LiTFSI mixed in is 0.2g, the mass fraction of modified carbon nanotubes is adjusted to 5mass%, solution casting, vacuum drying, and the thickness of the PVDF-TRFE-CFE polymer film filled with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation is 80μm.

[0049] Material characterization and performance testing

[0050] Platinum was plated on both sides of the 120 μm fixed battery polymer electrolyte prepared in Verification Example 1 by magnetron sputtering as a blocking electrode, and an AC impedance test was performed at 30°C. The AC impedance spectrum is shown in Figure 1 As shown, the test results show that the ionic conductivity of the prepared three-dimensional structured composite electrolyte is 0.2 -4 S / cm.

[0051] Depend on Figure 2 The scanning electron microscope shown shows that the 80 μm fixed battery polymer electrolyte particles prepared in Verification Example 2 are closely arranged and the carbon nanotubes are evenly distributed.

[0052] Depend on Figure 3 It can be seen that the interface impedance R of the lithium symmetric battery assembled with the 120 μm fixed battery polymer electrolyte of Verification Example 1 at 25°C Li-PVDF1 =157Ω. Figure 4 It can be seen that the interface impedance R of the lithium symmetric battery assembled with the 80μm fixed battery polymer electrolyte of Verification Example 2 at 25°C Li-PVDF2=35Ω. This shows that increasing the DBD time and reducing the film thickness in Verification Examples 1 and 2 greatly reduced the interface impedance between Li and the electrolyte film, and improved the ionic conductivity of the polymer electrolyte. However, due to the short DDB time and large film thickness in Verification Example 1, the dispersion of carbon nanotubes was poor and the film polarization impedance was large. Therefore, an appropriate DBD time will achieve the best dispersion, and a more appropriate film thickness will achieve the best interface impedance effect.

[0053] The lithium symmetric battery assembled with the 80μm fixed battery polymer electrolyte in Verification Example 2 was subjected to cycle testing. The test results are as follows Figure 5 As shown, at a current density of 0.2 mA cm -2 Under this condition, the battery cycle is stable, which proves that the DBD-treated sulfonated modified carbon nanotubes ensure the battery cycle stability performance.

[0054] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions may occur depending on design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A solid-state battery polymer electrolyte, characterized in that: The polymer electrolyte is a PVDF-TRFE-CFE polymer film filled with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation.

2. A solid-state battery polymer electrolyte according to claim 1, characterized in that: The thickness of the polymer electrolyte is 80 μm to 120 μm.

3. A solid-state battery polymer electrolyte according to claim 1 or 2, characterized in that: The mass fraction of the carbon nanotubes treated by dielectric barrier discharge plasma sulfonation is 1 to 5 mass %.

4. The method for preparing a solid-state battery polymer electrolyte according to claim 2 or 3, characterized in that: The specific steps include: S1: subjecting the purified carbon nanotubes to dielectric barrier discharge plasma sulfonation treatment to obtain modified carbon nanotubes; S2 disperses the modified carbon nanotubes and adds them to the polymer electrolyte solution, which is coated on the mold by casting. After vacuum drying, a PVDF-TRFE-CFE polymer film with carbon nanotubes treated by dielectric barrier discharge plasma sulfonation as filler is obtained.

5. The method for preparing a solid-state battery polymer electrolyte according to claim 4, characterized in that: The processing method for purifying carbon nanotubes in step S1 is: A1: The aggregated carbon nanotubes prepared by chemical vapor deposition were calcined at 300°C for 30 min in a muffle furnace, and then heated to 800°C in a quartz tube furnace under argon protection for 10 min at a heating rate of 5°C / min. A2: immersing the carbon nanotubes heated in step A1 into an excess of 1 mol / L hydrochloric acid solution at a temperature of 100°C for 2 hours; A3: separating the carbon nanotubes treated with acid in step A2 into solid and liquid by centrifugation or filtration, and drying the obtained solid to obtain the purified carbon nanotubes.

6. A method for preparing a solid-state battery polymer electrolyte according to claim 5, characterized in that: The dielectric barrier discharge plasma sulfonation treatment in step S1 is specifically as follows: The purified carbon nanotubes were dispersed in a solution with a concentration of 1 mol L -1 Dielectric barrier discharge is carried out in H2SO4 solution with a discharge power of 50mA / 60V and a discharge time of 15min to 1.5h.

7. The method for preparing a solid-state battery polymer electrolyte according to claim 4, characterized in that: The polymer electrolyte solution in step S2 is formed by stirring a blended polymer obtained by dissolving PVDF-TRFE-CFE and N,N-dimethylformamide and lithium bis(trifluoromethanesulfonyl)imide at a mass ratio of 1:0.2-1.2 for 48 hours.

8. The method for preparing a solid-state battery polymer electrolyte according to claim 7, characterized in that: In step S2, 0.1 g of PVDF-TRFE-CFE is dissolved in every 1 mL of N,N-dimethylformamide in the polymer blend.

9. The method for preparing a solid-state battery polymer electrolyte according to claim 8, characterized in that: In step S2, the modified carbon nanotubes are dispersed and added to the polymer electrolyte solution, coated on a polytetrafluoroethylene mold, and placed in a vacuum drying oven at 60° C. for 48 hours.

10. An application of a solid-state battery polymer electrolyte as claimed in claim 2 or 3, characterized in that: Installed between the positive electrode and the lithium metal negative electrode to form a solid-state lithium metal battery.

Citation Information

Cited By

  • Sulfonated C4N nanosheet, preparation method thereof and solid electrolyte

    CN119320124A

  • A sulfonated C4N nanosheet and its preparation method and solid electrolyte

    CN119320124B