In-situ self-polymerization ionic liquid composite solid electrolyte as well as preparation method and application thereof

By using catalysts in lithium-ion batteries to promote click reactions to form a three-dimensional polymer cross-linking structure and coat ionic liquids, the safety hazards of lithium-ion batteries and the problem of low ion conductivity in room temperature are solved, and high conductivity and electrochemical stability are achieved simplifies the process and reduces costs.

CN118970167APending Publication Date: 2024-11-15TONGJI UNIV
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411212474.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The liquid electrolytes in existing lithium-ion batteries have safety hazards during charging and discharging, and the low room temperature ionic conductivity of polymer solid electrolytes limits their application.

Method used

The catalyst promotes the click reaction between the nucleophilic reagent and the electrophilic reagent at room temperature, forming a three-dimensional polymer cross-linking structure, reducing the crystallinity of the polymer, and covering the ionic liquid therein, improving the migration ability and conductivity of lithium ions.

Benefits of technology

The high ionic conductivity and electrochemical stability of lithium-ion batteries are achieved, which improves safety performance and cycle stability, while simplifying the process and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970167A_ABST
    Figure CN118970167A_ABST
Patent Text Reader

Abstract

The invention relates to an in-situ self-polymerization ionic liquid composite solid electrolyte as well as a preparation method and application thereof. The composite solid electrolyte comprises a cross-linked structure formed by in-situ auto-polymerization of a nucleophilic reagent and an electrophilic reagent, and an ionic liquid, a lithium salt and a catalyst dispersed in the cross-linked structure. The preparation process comprises the following steps: mixing an ionic liquid, a catalyst and a lithium salt, and uniformly stirring to obtain an eutectic liquid; mixing a nucleophilic reagent and an electrophilic reagent, and uniformly stirring to obtain a monomer liquid; and mixing the two solutions to obtain the in-situ self-polymerization ionic liquid composite solid electrolyte. Compared with the prior art, the catalyst provided by the invention can promote in-situ cross-linking auto-polymerization of a nucleophilic reagent and an electrophilic reagent through a click reaction to form a three-dimensional polymer cross-linked network and promote rapid transmission of lithium ions. The ionic liquid wrapped by the three-dimensional cross-linked network can effectively improve the ionic conductivity of the solid electrolyte, thereby improving the cycling stability of the solid lithium metal battery at room temperature.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium battery composite solid electrolytes, and in particular to an in-situ self-polymerizing ionic liquid composite solid electrolyte and a preparation method and application thereof. Background Art

[0002] With the acceleration of modernization, the world is facing ecological problems such as the energy crisis of the decreasing traditional fossil energy, serious environmental pollution and the global greenhouse effect. Faced with increasingly prominent environmental and resource problems, it is imperative to accelerate the development of clean energy, establish an efficient, clean, economical and safe energy system, reduce the dependence of the traditional automotive industry and industry on fossil energy, and achieve sustainable development of new energy. Lithium-ion batteries have the advantages of fast charging and discharging and environmental friendliness, and are becoming the focus of attention in the field of new energy.

[0003] Currently, commercial lithium-ion batteries usually use liquid electrolytes. However, this type of battery faces two serious problems: first, during the battery's charge and discharge process, organic solvents may form a solid electrolyte film at the positive electrode, causing electrode polarization and thus reducing battery performance; second, since the organic solvents used in the electrolyte have safety hazards such as leakage, combustion and explosion, safety issues have become a worrying aspect.

[0004] In order to improve the safety performance and cycle life of lithium-ion batteries, the use of solid electrolytes instead of liquid electrolytes can effectively solve the safety problems currently faced by batteries. Polymer solid electrolytes are currently the most promising solid electrolytes, but their low room temperature ionic conductivity limits their application. Compared with traditional liquid electrolytes, ionic liquids have many advantages: higher ionic conductivity, non-flammability, high thermal stability, low toxicity, and higher lithium salt solubility. The composite of ionic liquids and polymer electrolytes can improve the safety performance of solid-state lithium batteries while improving the room temperature ionic conductivity of polymer solid electrolytes. Chinese patent CN114464879B discloses a self-healing block polymer ionic liquid / polyethylene oxide composite solid electrolyte and its preparation method, and uses dissolution, film formation and drying methods to composite ionic liquids with polymers to prepare ionic liquid and polymer composite electrolytes. Chinese patent CN111253521B discloses an organic-inorganic-ionic liquid composite solid electrolyte, its preparation method and application, and an organic-inorganic-ionic liquid composite solid electrolyte prepared by heating or radiation-induced polymerization.

[0005] The ionic liquid polymer composite solid electrolytes prepared by the above patents all have good room temperature ionic conductivity and mechanical strength, and can solve the safety problems of liquid electrolyte lithium-ion batteries and the problem of low room temperature ionic conductivity of all-solid-state batteries. However, their preparation is achieved through dissolution, film formation, drying processes or heating, radiation-induced polymerization, which is time-consuming and energy-consuming, and is not conducive to large-scale applications.

[0006] Therefore, there is an urgent need to study a preparation method that is simple and controllable and can enable polymer solid electrolytes to have high ionic conductivity and cycle stability at room temperature. Summary of the invention

[0007] The purpose of the present invention is to provide an in-situ self-polymerizing ionic liquid composite solid electrolyte and its preparation and application in order to overcome the defects of the above-mentioned prior art. Through the catalytic action of the catalyst, the nucleophilic reagent and the electrophilic reagent undergo a click reaction at room temperature, and the three-dimensional polymer cross-linked structure formed can reduce the crystallinity of the polymer and facilitate the migration of lithium ions; and the ionic liquid coated by the three-dimensional polymer cross-linked structure can improve the ionic conductivity of the polymer electrolyte.

[0008] The purpose of the present invention can be achieved by the following technical solutions:

[0009] The present invention provides an in-situ self-polymerizing ionic liquid composite solid electrolyte, the composite solid electrolyte comprising an in-situ self-polymerizing main body, a lithium salt dispersed in the main body and an ionic liquid wrapped by the main body;

[0010] The in-situ self-polymerization main body is a three-dimensional polymer cross-linked structure formed by in-situ self-polymerization of nucleophilic reagents and electrophilic reagents.

[0011] Furthermore, the composite solid electrolyte also includes a catalyst, which is used to catalyze a click reaction between a nucleophilic reagent and an electrophilic reagent at room temperature to perform in-situ cross-linking self-polymerization;

[0012] The molar ratio of the nucleophile, the electrophile, the ionic liquid, the catalyst and the lithium salt is 1:(2-3):(1-2):(0.10-0.30):(1-2).

[0013] The present invention also provides a method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte, comprising the following steps:

[0014] S1: mixing the ionic liquid, the catalyst and the lithium salt, and stirring them evenly to obtain a eutectic liquid;

[0015] S2: mixing the nucleophile and the electrophile, and stirring them evenly to obtain a monomer liquid;

[0016] S3: The eutectic liquid in S1 and the monomer liquid in S2 are mixed, stirred and allowed to stand at room temperature to obtain an in-situ self-polymerized ionic liquid composite solid electrolyte.

[0017] Furthermore, in S2, the nucleophilic reagent includes one or more of 1,2-ethanedithiol, 1,3-propanedithiol, trimethylolpropane trimercaptopropionate, and pentaerythritol tetrakis-3-mercaptopropionate.

[0018] Furthermore, in S2, the electrophilic reagent includes one or more of acrylate, methacrylate, polyethylene glycol diacrylate, maleimide, and vinyl sulfone.

[0019] Furthermore, in S1, the lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate, and lithium bis(trifluoromethanesulfonyl)imide.

[0020] Furthermore, in S1, the ionic liquid includes one or more of 1-ethyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium perfluoroalkyl phosphate, and 1-alkyl-3-methylimidazolium ionic liquids.

[0021] Furthermore, in S1, the catalyst includes one or more of triethylamine, propylamine, ethylamine, and 4-aminobenzoic acid.

[0022] Furthermore, in S1 to S3, the stirring process is carried out in an inert gas atmosphere for 6 to 8 hours;

[0023] The standing time in S3 is 1 to 2 hours.

[0024] The present invention also provides an application of an in-situ self-polymerizing ionic liquid composite solid electrolyte, wherein the composite solid electrolyte is used to prepare a solid-state lithium metal battery;

[0025] The solid-state lithium metal battery comprises a positive electrode, the above-prepared in-situ self-polymerized ionic liquid composite solid electrolyte and a negative electrode which are stacked in sequence.

[0026] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0027] 1. The present invention self-polymerizes nucleophiles and electrophiles in situ to form a three-dimensional polymer cross-linked structure that can reduce the crystallinity of the polymer, increase the amorphous region, and facilitate the migration of lithium ions; and the ionic liquid coated with the three-dimensional polymer cross-linked structure can improve the ionic conductivity of the polymer electrolyte and has excellent antioxidant properties and flame retardancy. The synergistic effect of the two can improve the ionic conductivity and safety of the polymer solid electrolyte.

[0028] 2. The ionic conductivity of the battery with in-situ self-polymerized ionic liquid composite solid electrolyte in the present invention is as high as 1.1×10 -3 S cm -1 The electrochemical stability window is 5.15V. Compared with traditional polymer solid electrolytes, its ionic conductivity and electrochemical stability are greatly improved.

[0029] 3. The present invention prepares solid electrolytes by in-situ self-polymerization of nucleophiles and electrophiles through click reactions under catalysis. Compared with traditional solution casting methods, thermal initiation or radiation initiation polymerization, this method is simple and controllable, energy-saving and environmentally friendly, improves production efficiency and reduces production costs.

[0030] 4. The present invention coats the precursor solution onto NCM811 and the lithium metal negative electrode to directly self-polymerize the solid electrolyte in situ on the electrode, and the obtained electrolyte has good interface contact with the electrode. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 The impedance test diagram of the solid electrolyte prepared in Examples 1-5 and Comparative Example 1;

[0032] Figure 2 Schematic diagram of the stability test results of the solid electrolyte and the lithium negative electrode prepared in Examples 1-5 and Comparative Example 1;

[0033] Figure 3 This is a cross-sectional view of the precursor solution after in-situ self-polymerization on lithium metal in Example 1.

[0034] Figure 4 Schematic diagram of the electrochemical stability test results of the full battery assembled in Example 1.

[0035] Figure 5 Schematic diagram of the electrochemical stability test results of the full battery assembled based on ionic liquid electrolyte in Comparative Example 2. DETAILED DESCRIPTION

[0036] The specific implementation methods of the present invention are described in detail below through examples. These examples are implemented on the premise of the scheme described in the present invention, and provide detailed implementation methods and specific operating processes, but the protection scope of the present invention is not limited to the following examples.

[0037] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments. Any features such as component models, material names, connection structures, preparation methods, materials, structures or composition ratios not clearly described in this technical solution are deemed to be common technical features disclosed in the prior art.

[0038] Example 1

[0039] This embodiment provides a method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte, comprising the following steps:

[0040] S1: In an argon glove box, 1-ethyl-3-methylimidazolium chloride, triethylamine and lithium bis(trifluoromethanesulfonyl)imide were added into a glass bottle in amounts of 2 g, 0.10 g and 0.60 g, respectively, and stirred for 6 hours to dissolve the solid to obtain a transparent eutectic solution;

[0041] S2: In an argon glove box, 1 g and 1.5 g of trimethylolpropane trimercaptopropionate and polyethylene glycol diacrylate were added into a glass bottle and stirred for 6 hours to obtain a uniformly mixed monomer liquid;

[0042] S3: In an argon glove box, the monomer liquid in S2 and the eutectic solution in S1 are mixed and stirred evenly to obtain a precursor solution, and the precursor solution is allowed to stand at room temperature for 24 hours to obtain an in-situ self-polymerized ionic liquid composite solid electrolyte.

[0043] Figure 3 This is a cross-sectional view of the precursor solution in S3 after in-situ polymerization on the lithium metal negative electrode. It can be seen that the contact between the lithium metal negative electrode and the electrolyte is very close.

[0044] Figure 4 The cycle performance diagram of the solid-state lithium metal button cell at room temperature, which is assembled with the in-situ self-polymerized ionic liquid composite solid electrolyte prepared in this embodiment and uses NCM811 as the positive electrode and lithium metal sheet as the negative electrode. The specific assembly process is: in an argon glove box, the precursor solution obtained in step S3 is evenly coated on NCM811 and the lithium metal negative electrode, and the precursor solution on the electrode is self-polymerized to assemble into a solid-state lithium metal button cell.

[0045] like Figure 4 As shown, the assembled battery exhibited 179.3 mAh g at a current density of 0.1 C after activation. -1 The specific capacity is 165.4 mA hg after 50 cycles. -1 The specific capacity and capacity retention rate are 92.3%, which shows that the solid electrolyte has good cycle stability.

[0046] Example 2

[0047] This embodiment provides a method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte, comprising the following steps:

[0048] S1: In an argon glove box, 1-butyl-3-methylimidazolium tetrafluoroborate, triethylamine and lithium difluorooxalatoborate were added into a glass bottle according to the mass of 2.2 g, 0.15 g and 0.40 g, respectively, and stirred for 6 hours to dissolve the solid to obtain a transparent eutectic solution;

[0049] S2: In an argon glove box, 1 g and 1.5 g of trimethylolpropane trimercaptopropionate and polyethylene glycol diacrylate were added into a glass bottle and stirred for 6 hours to obtain a uniformly mixed monomer liquid;

[0050] S3: In an argon glove box, the monomer liquid in S2 and the eutectic solution in S1 are mixed and stirred evenly, and allowed to stand at room temperature for 24 hours to obtain the in-situ self-polymerized ionic liquid composite solid electrolyte.

[0051] Example 3

[0052] This embodiment provides a method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte, comprising the following steps:

[0053] S1: In an argon glove box, 1-butyl-3-methylimidazolium perfluoroalkyl phosphate, ethylamine and lithium hexafluorophosphate were added into a glass bottle according to the mass of 2.2 g, 0.12 g and 0.50 g, respectively, and stirred for 6 hours to dissolve the solid to obtain a transparent eutectic solution;

[0054] S2: In an argon glove box, 1.2 g of pentaerythritol tetrakis-3-mercaptopropionate and 2 g of acrylate were added into a glass bottle and stirred for 6 hours to obtain a uniformly mixed monomer liquid;

[0055] S3: In an argon glove box, the monomer liquid in S2 and the eutectic solution in S1 are mixed and stirred evenly, and allowed to stand at room temperature for 24 hours to obtain the in-situ self-polymerized ionic liquid composite solid electrolyte.

[0056] Example 4

[0057] This embodiment provides a method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte, comprising the following steps:

[0058] S1: In an argon glove box, 1-alkyl-3-methylimidazole ionic liquid, 4-aminobenzoic acid and lithium bis(trifluoromethanesulfonyl)imide were added into a glass bottle according to mass of 2 g, 0.12 g and 0.60 g, respectively, and stirred for 6 hours to dissolve the solid to obtain a transparent eutectic solution;

[0059] S2: In an argon glove box, 1.2 g and 2.2 g of pentaerythritol tetrakis-3-mercaptopropionate and polyethylene glycol diacrylate were added into a glass bottle and stirred for 6 hours to obtain a uniformly mixed monomer liquid;

[0060] S3: In an argon glove box, the monomer liquid in S2 and the eutectic solution in S1 are mixed and stirred evenly, and allowed to stand at room temperature for 24 hours to obtain the in-situ self-polymerized ionic liquid composite solid electrolyte.

[0061] Example 5

[0062] This embodiment provides a preparation method of an in-situ self-polymerizing ionic liquid composite solid electrolyte, comprising the following steps:

[0063] S1: In an argon glove box, 1.8 g, 0.12 g and 0.50 g of 1-butyl-3-methylimidazolium perfluoroalkyl phosphate, triethylamine and lithium perchlorate were added into a glass bottle and stirred for 6 hours to dissolve the solid to obtain a transparent eutectic solution;

[0064] S2: In an argon glove box, 1.2 g and 1.8 g of pentaerythritol tetrakis-3-mercaptopropionate and methyl methacrylate were added into a glass bottle and stirred for 6 hours to obtain a uniformly mixed monomer liquid;

[0065] S3: In an argon glove box, the monomer liquid in S2 and the eutectic solution in S1 are mixed and stirred evenly, and allowed to stand at room temperature for 24 hours to obtain the in-situ self-polymerized ionic liquid composite solid electrolyte.

[0066] Comparative Example 1

[0067] This comparative example provides a method for preparing a solid electrolyte, comprising the following steps:

[0068] S1: In an argon glove box, lithium difluorooxalatoborate, trimethylolpropane trimercaptopropionate and polyethylene glycol diacrylate were added into a glass bottle according to mass of 0.40 g, 1 g and 1.5 g, respectively, and stirred for 6 hours to obtain a uniformly mixed liquid;

[0069] S2: In an argon glove box, 0.15 g of triethylamine was added to the mixed liquid in S1, stirred evenly, and allowed to stand at room temperature for 24 hours to obtain an in-situ self-polymerizing solid electrolyte.

[0070] Comparative Example 2

[0071] This comparative example provides a method for preparing an ionic liquid electrolyte, comprising the following steps:

[0072] S1: In an argon glove box, 1.8 g and 0.50 g of 1-butyl-3-methylimidazolium tetrafluoroborate and lithium bis(trifluoromethanesulfonyl)imide were added into a glass bottle and stirred for 6 hours to dissolve the lithium salt, thereby obtaining an ionic liquid electrolyte.

[0073] Figure 5 The cycle performance diagram of the liquid lithium metal button battery assembled with the ionic liquid electrolyte prepared in this comparative example, with NCM811 as the positive electrode and lithium metal sheet as the negative electrode, at room temperature. Figure 5As shown in Figure 2, the lithium metal battery assembled with ionic liquid electrolyte exhibited a high efficiency of 183.7 mAh g at a current density of 0.1 C after activation. -1 The specific capacity is 67.3 mAh g after 50 cycles. -1 , the capacity retention rate is 36.6%. It can be seen that the ionic liquid electrolyte lacking a polymer matrix will react with the lithium metal negative electrode, resulting in a significant decrease in the cycle stability.

[0074] Test Example 1

[0075] The composite solid electrolytes prepared in Examples 1 to 5 and Comparative Example 1 were assembled into symmetrical blocking cells in an argon glove box with stainless steel sheets as electrodes to test the ionic conductivity of the composite solid electrolytes. AC impedance tests were performed at 25°C under the conditions of a frequency range of 1 MHz to 0.1 Hz and an AC amplitude of 10 mV. The results are as follows: Figure 1 As shown in Table 1, Figure 1 As shown in Table 1, ionic liquids can effectively improve the ionic conductivity of composite solid electrolytes, which promotes the application of composite solid electrolytes under room temperature conditions.

[0076] Table 1 Ionic conductivity of solid electrolytes prepared in various embodiments and comparative examples

[0077]

[0078] Test Example 2

[0079] The composite solid electrolytes prepared in Examples 1 to 5 and Comparative Example 1 were subjected to linear sweep voltammetry tests. The test conditions / process were as follows: in the voltage range of 0-6 V, 1 mV s -1 The response current changes of different composite solid electrolytes at a scan rate of , the results are shown in Table 2 and Figure 2 As shown in Table 2 and Figure 2 It can be seen that ionic liquids can effectively improve the antioxidant properties of polymer electrolytes.

[0080] Table 2 Electrochemical stability window of solid electrolytes prepared in various embodiments and comparative examples

[0081]

[0082] Test Example 3

[0083] The composite solid electrolyte prepared in Example 1 and the ionic liquid electrolyte prepared in Comparative Example 2 were assembled into a full battery in an argon glove box with NCM811 as the positive electrode and lithium metal sheet as the negative electrode. The cycle stability of the full battery based on different electrolytes was tested at 25°C and 0.1C. The results are as follows: Figure 4 and Figure 5As shown, the ionic liquid with high ionic conductivity effectively improves the ionic conductivity of the polymer substrate, and the polymer substrate can inhibit the reaction between the ionic liquid and the lithium metal negative electrode, thereby improving the cycle stability of the whole battery.

[0084] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. An in-situ self-polymerizing ionic liquid composite solid electrolyte, characterized in that: The composite solid electrolyte comprises an in-situ self-polymerized main body, a lithium salt dispersed in the main body, and an ionic liquid wrapped by the main body; The in-situ self-polymerization main body is a three-dimensional polymer cross-linked structure formed by in-situ self-polymerization of nucleophilic reagents and electrophilic reagents.

2. The in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 1, characterized in that: The composite solid electrolyte further comprises a catalyst, which is used to catalyze a click reaction between a nucleophilic agent and an electrophilic agent at room temperature to perform in-situ cross-linking self-polymerization; The molar ratio of the nucleophile, the electrophile, the ionic liquid, the catalyst and the lithium salt is 1:(2-3):(1-2):(0.10-0.30):(1-2).

3. A method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte as claimed in any one of claims 1 to 2, characterized in that: The following steps are involved: S1: mixing the ionic liquid, the catalyst and the lithium salt, and stirring them evenly to obtain a eutectic liquid; S2: mixing the nucleophile and the electrophile, and stirring them evenly to obtain a monomer liquid; S3: The eutectic liquid in S1 and the monomer liquid in S2 are mixed, stirred and allowed to stand at room temperature to obtain an in-situ self-polymerized ionic liquid composite solid electrolyte.

4. The method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 3, characterized in that: In S2, the nucleophilic reagent includes one or more of 1,2-ethanedithiol, 1,3-propanedithiol, trimethylolpropane trimercaptopropionate, and pentaerythritol tetrakis-3-mercaptopropionate.

5. The method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 3, characterized in that: In S2, the electrophilic reagent includes one or more of acrylate, methacrylate, polyethylene glycol diacrylate, maleimide, and vinyl sulfone.

6. The method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 3, characterized in that: In S1, the lithium salt includes one or more of lithium perchlorate, lithium hexafluorophosphate, lithium difluorooxalatoborate, and lithium bis(trifluoromethanesulfonyl)imide.

7. The method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 3, characterized in that: In S1, the ionic liquid includes one or more of 1-ethyl-3-methylimidazolium chloride, 1-butyl-3-methylimidazolium tetrafluoroborate, 1-butyl-3-methylimidazolium perfluoroalkyl phosphate, and 1-alkyl-3-methylimidazolium ionic liquids.

8. The method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 3, characterized in that: In S1, the catalyst includes one or more of triethylamine, propylamine, ethylamine, and 4-aminobenzoic acid.

9. The method for preparing an in-situ self-polymerizing ionic liquid composite solid electrolyte according to claim 3, characterized in that: In S1 to S3, the stirring process is carried out in an inert gas atmosphere for 6 to 8 hours; The standing time in S3 is 1 to 2 hours.

10. An application of an in-situ self-polymerizing ionic liquid composite solid electrolyte, characterized in that: The composite solid electrolyte is used to prepare a solid-state lithium metal battery; The solid-state lithium metal battery comprises a positive electrode, an in-situ self-polymerizing ionic liquid composite solid electrolyte according to any one of claims 1 to 2, and a negative electrode stacked in sequence.

Citation Information

Cited By

  • Sulfide-based composite solid electrolyte membrane as well as full-dry preparation method and application thereof

    CN121331922A