Quick charge type lithium ion battery electrolyte and application thereof
By adding additives such as coronal ether derivatives to the lithium-ion battery electrolyte, the composition of the electrolyte is optimized, and the problems of low conductivity and large interface impedance are solved, and the good cycle life and fast charging of lithium-ion batteries are achieved at high 6C ratios are achieved. performance.
Patent Information
- Application Number
- CN202411246946.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-09-06
AI Technical Summary
The existing lithium-ion battery electrolyte has low conductivity and large interface impedance during fast charging, resulting in poor cycle life and difficult to meet the requirements of high magnification and long life at the same time.
Using a fast charging electrolyte containing solvents, lithium salts, film-forming additives and multifunctional additives - coronal ethers and their derivatives, to improve conductivity and form a stable and thin SEI film by optimizing composition and proportions, strengthening the Lithium ions conduction capability and interface performance.
It achieves good cycle life and high conductivity of lithium-ion batteries at high 6C, improving the fast charging and cycle performance of the battery.
Smart Images

Figure BDA0005031051230000071 
Figure BDA0005031051230000081
Abstract
Description
Technical Field
[0001] The present invention relates to the field of lithium ions, and in particular to a fast-chargeable lithium ion battery electrolyte and application thereof. Background Art
[0002] Since its advent, lithium-ion batteries have played a very important role in people's daily lives. More and more electrical devices need to use lithium-ion batteries to power them. At present, new energy vehicles are developing rapidly under the advantages of national subsidies and high environmental protection, but they also face many challenges, such as anxiety about battery life, fast charging and safety. In the face of extremely fast charging, the electrolyte plays a key role. The ability of the electrolyte to quickly conduct lithium ions, the low desolvation energy barrier, and the speed of transmission at the interface have a key impact on the fast charging ability of the battery.
[0003] In order to improve the fast charging ability of the electrolyte, a linear carbonate and a cyclic carbonate composite solvent are used in patent CN 117374404 A to increase the lithium ion migration number and conductivity, and reduce the viscosity of the electrolyte. At the same time, trimethyl (methylsulfonylmethyl) silane is added to further assist in the formation of a thin and stable SEI film, which has low impedance, high stability, and high ion conductivity. The patent application with publication number CN113851725A discloses a lithium ion battery fast charging electrolyte, the solvent of which is MF:EC:EMC:DMC=1:3:2:4, the electrolyte is LiPF6:LiClO4=2:1, the total electrolyte content is 2mol / L, and the negative electrode film-forming additive is allyloxytrimethylsilane (AMSL). The formed SEI can passivate the material interface, reduce the lithium ion migration impedance, and improve the battery 5C fast charging performance and cycle life.
[0004] In terms of electrolyte, measures to improve fast charging performance include but are not limited to the use of low-viscosity solvents, solvents with weak solvation ability, and some film-forming additives that form thin SEI films, but commonly used solvents may not meet the requirements of the first two conditions at the same time. Patent CN111293356 A discloses a crown ether electrolyte additive. Studies have shown that the inner cavity diameter of 12-crown-4 is about 120-150pm, while Li + The diameter is 120 pm, which can be + The formation of a stable complex can significantly improve the high-rate performance of the battery and enhance the cycle performance of the battery, but the performance is single and only plays a role in enhancing the conductivity, without improving the modification of the SEI film.
[0005] Although the above schemes have improved the battery performance to a certain extent through the directional selection and combination of additives, there are still some problems such as low electrolyte conductivity and large interface impedance. Therefore, the development of efficient lithium iron phosphate electrolyte and battery development is still a technical point and difficulty that the industry urgently needs to solve. Summary of the invention
[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, one object of the present invention is to provide a fast-charging electrolyte, which has a high ionic conductivity and has the beneficial effect of enabling lithium-ion batteries to maintain a good cycle life at a high rate of 6C.
[0007] In one aspect of the present invention, the present invention provides a fast-charging electrolyte. According to an embodiment of the present invention, the fast-charging electrolyte includes a solvent, a lithium salt, a film-forming additive and a multifunctional additive, and the multifunctional additive is a crown ether and its derivatives. The fast-charging electrolyte has a high ionic conductivity and has the beneficial effect of enabling the lithium-ion battery to maintain a good cycle life at a high rate of 6C.
[0008] According to an embodiment of the present invention, the fast-charging electrolyte may further include at least one of the following additional technical features:
[0009] According to an embodiment of the present invention, the crown ether and its derivatives include one or more selected from 4-vinylbenzo-18-crown-6, 2-(allyloxymethyl)-18-crown-6-ether, eicosine-15-crown-5-ether, benzo-15-crown-5, benzo-18-crown-6-ether, dibenzo-21-crown-7, and dibenzo-24-crown-8.
[0010] According to an embodiment of the present invention, the solvent includes two or more selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, γ-butyrolactone, ethyl acetate, methyl acetate, propyl acetate, methyl propionate, propyl propionate, ethyl propionate, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dimethyl sulfoxide, cyclopentane and dimethyl sulfone.
[0011] According to an embodiment of the present invention, the solvent is ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate.
[0012] According to an embodiment of the present invention, the mass ratio of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate is 2.5:2:5.5.
[0013] According to an embodiment of the present invention, the lithium salt includes at least one selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate.
[0014] According to an embodiment of the present invention, the lithium salt is lithium hexafluorophosphate and / or lithium bis(fluorosulfonyl)imide.
[0015] According to an embodiment of the present invention, the mass fraction of lithium hexafluorophosphate is 8.5%.
[0016] According to an embodiment of the present invention, the mass fraction of the lithium bis(fluorosulfonyl)imide is 5.5%.
[0017] According to an embodiment of the present invention, the film-forming additive is selected from one or more of vinyl sulfite, vinyl sulfate, 1,3-propane sultone, tris(trimethylsilyl)phosphate, lithium difluorooxalatoborate, fluoroethylene carbonate, vinylene carbonate, lithium difluorobisoxalate phosphate, lithium tetrafluorooxalate phosphate, and lithium difluorophosphate (LiPO2F2).
[0018] According to an embodiment of the present invention, the film-forming additives are vinylene carbonate, vinyl sulfate and tris(trimethylsilyl)phosphate.
[0019] According to an embodiment of the present invention, the usage ratio of the vinylene carbonate, the vinyl sulfate and the tris(trimethylsilyl)phosphate is 10:5:1.
[0020] According to an embodiment of the present invention, the weight ratio of the crown ether and its derivatives to the total weight of the fast-charging electrolyte is 0.05% to 0.5%.
[0021] According to an embodiment of the present invention, the ratio of the weight of the solvent to the total weight of the fast-charging electrolyte is 70% to 88%.
[0022] According to an embodiment of the present invention, the ratio of the weight of the solvent to the total weight of the fast-charging electrolyte is 72% to 85%.
[0023] According to an embodiment of the present invention, the ratio of the weight of the lithium salt to the total weight of the fast-charging electrolyte is 10% to 20%.
[0024] According to an embodiment of the present invention, the ratio of the weight of the lithium salt to the total weight of the fast-charging electrolyte is 11% to 16%.
[0025] According to an embodiment of the present invention, the ratio of the weight of the film-forming additive to the total weight of the fast-charging electrolyte is 0.2% to 5%.
[0026] In another aspect of the present invention, the present invention provides a method for preparing the aforementioned fast-charge electrolyte. According to an embodiment of the present invention, the method comprises:
[0027] The lithium salt, the film-forming additive and the multifunctional additive are dissolved in a solvent to obtain the fast-charging electrolyte.
[0028] According to an embodiment of the present invention, the method may further include the following additional technical features:
[0029] According to an embodiment of the present invention, the lithium salt, the film-forming additive and the multifunctional additive are dissolved in the solvent in sequence.
[0030] In another aspect of the present invention, the present invention further provides a battery. According to an embodiment of the present invention, the battery comprises the fast-charging electrolyte described above or the fast-charging electrolyte prepared according to the method described above.
[0031] According to an embodiment of the present invention, the battery may further include at least one of the following additional technical features:
[0032] According to an embodiment of the present invention, the battery is a lithium-ion battery.
[0033] According to an embodiment of the present invention, the battery further includes a positive electrode sheet, a negative electrode sheet and a separator.
[0034] According to the embodiments of the present invention, the present invention has at least one of the following technical effects:
[0035] (1) A mixed system of P salt and F salt is used, wherein lithium bis(fluorosulfonyl)imide and lithium bis(trifluoromethanesulfonyl)imide in the F salt have large anion groups and are easy to dissociate, so that the electrolyte system has high ionic conductivity;
[0036] (2) The use of multifunctional crown ether derivative additives, which have multiple -O-CH2-CH2- fragments in their structure, form a larger ring cavity, while the lone pair of electrons of the O atom on the ring is oriented toward the center of the ring, and Li + The formation of crown ether coordination compounds through dipole-ion interaction increases the Li + The electron transfer number is increased, which improves the conductivity and solubility of lithium ions in the solution;
[0037] (3) Multifunctional crown ether derivative additives compete with EC for Li + The effect of EC and Li + The force of is reduced, which is beneficial to the desolvation at the interface and the improvement of fast charging performance;
[0038] (4) At the same time, the crown ether derivative additive structure is combined with double bonds, fluorine bonds, benzene rings and other functional groups to form a stable and thin SEI film at the negative electrode interface, which is easy for lithium ions to conduct;
[0039] (5) The lithium-ion battery electrolyte of the present invention has the beneficial effect of enabling the lithium-ion battery to maintain a good cycle life at a high rate of 6C. DETAILED DESCRIPTION
[0040] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0041] 1. Preparation of electrolyte
[0042] Example 1
[0043] In an argon-filled glove box (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent and stirred to completely dissolve. 2% vinylene carbonate (VC), 1% vinyl sulfate (DTD), 0.2% tris(trimethylsilyl) phosphate (TMSP) and 0.05% 4-vinylbenzo-18-crown-6 were added to obtain the electrolyte for this experiment.
[0044] Example 2
[0045] This embodiment provides a lithium ion battery electrolyte. The same points as those in Embodiment 1 are not repeated here. The difference from Embodiment 1 is that the amount of 4-vinylbenzo-18-crown ether-6 used is different. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of 4-vinylbenzo-18-crown ether-6 in this embodiment is 0.1%.
[0046] Example 3
[0047] This embodiment provides a lithium ion battery electrolyte. The same points as those in Embodiment 1 are not repeated here. The difference from Embodiment 1 is that the amount of 4-vinylbenzo-18-crown ether-6 used is different. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of 4-vinylbenzo-18-crown ether-6 in this embodiment is 0.5%.
[0048] Example 4
[0049] This embodiment provides a lithium ion battery electrolyte. The same points as those in Embodiment 1 are not repeated here. The difference from Embodiment 1 is that twenty-fluoro-15-crown-5-ether is used as an electrolyte additive. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of twenty-fluoro-15-crown-5-ether in this embodiment is 0.05%.
[0050] Example 5
[0051] This embodiment provides a lithium ion battery electrolyte. The same points as those in Embodiment 1 are not repeated here. The difference from Embodiment 1 is that twenty-fluoro-15-crown-5-ether is used as an electrolyte additive. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of twenty-fluoro-15-crown-5-ether in this embodiment is 0.5%.
[0052] Example 6
[0053] This embodiment provides a lithium ion battery electrolyte. The similarities with Example 1 are not repeated here. The difference from Example 1 is that benzo-15-crown ether-5 is used as an electrolyte additive. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of benzo-15-crown ether-5 in this embodiment is 0.05%.
[0054] Example 7
[0055] This embodiment provides a lithium ion battery electrolyte. The same points as those in Embodiment 1 are not repeated here. The difference from Embodiment 1 is that benzo-15-crown ether-5 is used as an electrolyte additive. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of benzo-15-crown ether-5 in this embodiment is 0.1%.
[0056] Example 8
[0057] This embodiment provides a lithium ion battery electrolyte. The similarities with Example 1 are not repeated here. The difference from Example 1 is that benzo-15-crown ether-5 is used as an electrolyte additive. Based on the total mass of the lithium ion battery electrolyte, the mass percentage of benzo-15-crown ether-5 in this embodiment is 0.5%.
[0058] Comparative Example 1
[0059] In a glove box filled with argon (water content <10ppm, oxygen content <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC) and dimethyl carbonate (DMC) were mixed evenly in a mass ratio of 2.5:2:5.5. Then, 8.5% by mass of lithium hexafluorophosphate (LiPF6) and 5.5% by mass of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent and stirred to completely dissolve.
[0060] Comparative Example 2
[0061] In a glove box filled with argon (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% by mass of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent, stirred to completely dissolve, and 0.5% 4-vinylbenzo-18-crown-6 was added.
[0062] Comparative Example 3
[0063] In a glove box filled with argon (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% by mass of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent, stirred to completely dissolve, and 2% vinylene carbonate (VC) was added.
[0064] Comparative Example 4
[0065] In a glove box filled with argon (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent and stirred to completely dissolve, and 2% of vinylene carbonate (VC) and 1% of vinyl sulfate (DTD) were added.
[0066] Comparative Example 5
[0067] In a glove box filled with argon (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent and stirred to completely dissolve, and 2% of vinylene carbonate (VC), 1% of vinyl sulfate (DTD), and 0.2% of tris(trimethylsilyl) phosphate (TMSP) were added.
[0068] Comparative Example 6
[0069] In a glove box filled with argon (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent and stirred to completely dissolve, and 2% of vinylene carbonate (VC), 1% of vinyl sulfate (DTD), 0.2% of tris(trimethylsilyl) phosphate (TMSP), and 1% of twenty-fluoro-15-crown-5-ether were added.
[0070] Comparative Example 7
[0071] In an argon-filled glove box (water <10ppm, oxygen <10ppm), ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a mass ratio of 2.5:2:5.5, and then 8.5% of lithium hexafluorophosphate (LiPF6) and 5.5% of lithium bis(fluorosulfonyl)imide (LiFSI) were slowly added to the mixed solvent and stirred to completely dissolve, and 2% of vinylene carbonate (VC), 1% of vinyl sulfate (DTD), 0.2% of tris(trimethylsilyl) phosphate (TMSP), and 1% of benzo-15-crown-5 were added.
[0072] The lithium ion battery is prepared by using the electrolyte of the embodiment and the comparative example, which specifically comprises the following steps:
[0073] Preparation of positive electrode sheet: Add positive electrode material (LFP), conductive agent (Super P), carbon tube (CNT) and polyvinylidene fluoride (PVDF) in a mass ratio of 97.5%: 0.5%: 0.5%: 1.5% to N-methylpyrrolidone (NMP), mix evenly to form slurry, and coat the slurry on the aluminum foil current collector. The single surface density of the positive electrode is 18 mg / cm 2 , cold pressed to 2.42g / m 3 , and the positive electrode sheet is obtained after punching.
[0074] Preparation of negative electrode sheet: Graphite, conductive agent (Super P), single-walled carbon tube (SWCNT), sodium carboxymethyl cellulose (CMC) and styrene-butadiene rubber latex (SBR) were added into deionized water at a mass ratio of 96.2%: 0.94%: 0.06%: 2%: 0.8%, and the mixture was stirred and mixed evenly. The slurry was coated on the copper foil current collector, and the negative electrode surface density was determined according to the N / P ratio of 1.15, and the surface density was cold pressed to 1.55 g / m 3 , and then punch out to make the negative electrode sheet.
[0075] Preparation of battery cells: stack the separator, negative electrode plate and positive electrode plate in a "Z" shape to obtain a bare battery cell to be injected with liquid, and then use aluminum-plastic film to package the battery cell to be injected with liquid. After baking, inject the electrolyte in the embodiment or comparative example at an addition amount of 3.5g / Ah to obtain a sodium-lithium ion battery with a nominal capacity of 2Ah to be tested.
[0076] The electrolytes prepared in Examples 1-8 and Comparative Examples 1-7 were tested for conductivity, DCR, 6C fast charge capability, interface lithium deposition, and 6C fast charge cycle. The specific test conditions are as follows:
[0077] Electrolyte conductivity test: In a glove box filled with argon (water content <10ppm, oxygen content <10ppm), the prepared electrolyte is tested for conductivity using a conductivity meter.
[0078] DCR test: Charge the battery to 3.65V with constant current and constant voltage, let it stand for 6 hours, and then test the DC internal resistance of the battery.
[0079] Fast charging capability test: The prepared battery was tested for 2.0-3.65V charging and discharging at room temperature of 25±2℃ and relative humidity of 45%-75%. The test steps are as follows: first, 1C constant capacity was charged three times and the rated capacity was recorded as C0; then, 1C constant current and constant voltage was charged to 3.65V and allowed to stand for 10 minutes; 1C constant current was discharged to 2.0V and allowed to stand for 10 minutes, and then 6C constant current and constant voltage was charged to 3.65V and the charging capacity was recorded as C1.
[0080] 6C fast charge SOC=C1 / C0*100%
[0081] 6C interface lithium plating test: The battery cell is charged to 80% SOC at 6C in a 45℃ constant temperature box, and then the battery is disassembled in a glove box to observe the lithium plating status of the negative electrode.
[0082] 6C rate fast charge cycle test: In a 25℃ constant temperature box, the lithium-ion battery is charged at a constant current of 0.2C to a voltage of 3.65V, and discharged at a constant current of 0.2C to a voltage of 2.0V. The discharge capacity of the lithium-ion battery is tested and recorded as C2; charged to 3.65V at a constant current and constant voltage of 6C, allowed to stand for 10 minutes, and discharged to 2.0V at a constant current of 1C, allowed to stand for 10 minutes; the discharge capacity of the lithium-ion battery after 500 cycles of charge and discharge is recorded as C3.
[0083] 25℃, 500 cycles capacity retention rate = C3 / C2×100%;
[0084] The test data of the embodiments and comparative examples are shown in Table 1.
[0085] Table 1
[0086]
[0087]
[0088] The results show that:
[0089] Comparison of electrical conductivity: Compared with Comparative Examples 1, 3, 4, and 5, the electrical conductivity of Examples 1-8 and Comparative Examples 2, 6, and 7 is significantly improved. The fundamental reason is that the crown ether derivative additive is added to the electrolyte to improve the migration rate of lithium ions.
[0090] The DCR in Comparative Example 1 is lower than that in Examples 1-8 and 2-7. The main reason is that no other film-forming additives are used in the formula of Comparative Example 1, which makes the SEI film thinner and the DCR lower, but the fast charging performance and cycle performance are poor, and there is serious interface lithium precipitation. Compared with Comparative Example 5, Example 1-3 adds different amounts of 4-vinylbenzo-18-crown ether, and the performance is significantly better than the comparative example. The main reason is that the additive improves the conductivity and reduces the interface desolvation energy barrier. At the same time, the molecule contains vinyl groups, which makes the interface produce a thinner SEI layer. In Example 4-5, twenty-fluoro-15-crown-5-ether is used as an additive, which significantly improves the fast charging performance. At the same time, the DCR is smaller than that of Example 1-3. The reason is that the molecule contains F, and the SEI produced at the interface has a smaller impedance than the Li2CO3 generated at the vinyl interface. At the same time, Comparative Example 6 increases the content of twenty-fluoro-15-crown-5-ether, and the conductivity is significantly improved, but the DCR is too large due to the generation of too many LiF layers, resulting in excessive interface impedance and obvious lithium precipitation. In Examples 6-8, 1-benzo-15-crown-5 was selected as an additive. Compared with Comparative Example 5, the performance was also improved a lot. The reason is that the conjugated structure of the benzene ring enhances the force of EC on Li+ through the π orbital, improves the desolvation ability, and the π-π stacking of the benzene ring in the additive can be preferentially adsorbed at the negative electrode interface, thereby inducing anions to form a SEI film at the negative electrode interface. In Comparative Example 7, the content of benzo-15-crown-5 was increased. Although the conductivity was improved, the SEI film was thickened due to the electropolymerization of the benzene ring, the DCR increased, and the performance decreased.
[0091] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
Claims
1. A fast-charging electrolyte, characterized in that: The fast-charging electrolyte comprises a solvent, a lithium salt, a film-forming additive and a multifunctional additive, wherein the multifunctional additive is a crown ether and a derivative thereof.
2. The fast-charging electrolyte according to claim 1, characterized in that: The crown ether and its derivatives include one or more selected from 4-vinylbenzo-18-crown-6, 2-(allyloxymethyl)-18-crown-6-ether, eicosine-15-crown-5-ether, benzo-15-crown-5, benzo-18-crown-6-ether, dibenzo-21-crown-7, and dibenzo-24-crown-8.
3. The fast-charging electrolyte according to claim 1, characterized in that: The solvent comprises two or more selected from ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, γ-butyrolactone, ethyl acetate, methyl acetate, propyl acetate, methyl propionate, propyl propionate, ethyl propionate, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, dimethyl sulfoxide, cyclopentane and dimethyl sulfone; Preferably, the solvent is ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate; Preferably, the mass ratio of ethylene carbonate, ethyl methyl carbonate and dimethyl carbonate is 2.5:2:5.
5.
4. The fast-charging electrolyte according to claim 1, characterized in that: The lithium salt comprises at least one selected from lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide, and lithium tetrafluoroborate; Preferably, the lithium salt is lithium hexafluorophosphate and / or lithium bis(fluorosulfonyl)imide; Preferably, the mass fraction of lithium hexafluorophosphate is 8.5%; Preferably, the mass fraction of the lithium bis(fluorosulfonyl)imide is 5.5%.
5. The fast-charging electrolyte according to claim 1, characterized in that: The film-forming additive is selected from one or more of vinyl sulfite, vinyl sulfate, 1,3-propane sultone, tris(trimethylsilyl)phosphate, lithium difluorooxalatoborate, fluoroethylene carbonate, vinylene carbonate, lithium difluorobisoxalatephosphate, lithium tetrafluorooxalatephosphate, and lithium difluorophosphate (LiPO2F2); Preferably, the film-forming additive is vinylene carbonate, vinyl sulfate and tris(trimethylsilyl)phosphate; Preferably, the usage ratio of the vinylene carbonate, the vinyl sulfate and the tris(trimethylsilyl)phosphate is 10:5:
1.
6. The fast-charging electrolyte according to claim 1, characterized in that: The weight ratio of the crown ether and its derivatives to the total weight of the fast-charging electrolyte is 0.05% to 0.5%; Optionally, the ratio of the weight of the solvent to the total weight of the fast-charging electrolyte is 70% to 88%; Preferably, the ratio of the weight of the solvent to the total weight of the fast-charging electrolyte is 72% to 85%; Optionally, the ratio of the weight of the lithium salt to the total weight of the fast-charging electrolyte is 10% to 20%; Preferably, the ratio of the weight of the lithium salt to the total weight of the fast-charging electrolyte is 11% to 16%; Optionally, the ratio of the weight of the film-forming additive to the total weight of the fast-charging electrolyte is 0.2% to 5%.
7. A method for preparing the fast-charging electrolyte according to any one of claims 1 to 6, characterized in that: include: The lithium salt, the film-forming additive and the multifunctional additive are dissolved in a solvent to obtain the fast-charging electrolyte.
8. The method according to claim 7, characterized in that The lithium salt, the film-forming additive and the multifunctional additive are dissolved in the solvent in sequence.
9. A battery, characterized in that: The invention comprises the fast-charging electrolyte described in any one of claims 1 to 6 or the fast-charging electrolyte prepared by the method described in any one of claims 7 to 8.
10. The method according to claim 9, characterized in that The battery is a lithium-ion battery; Optionally, the battery further comprises a positive electrode sheet, a negative electrode sheet and a separator.
Citation Information
Patent Citations
Lithium ion secondary battery electrolyte and lithium ion battery containing electrolyte
CN104022310A
Lithium ion battery electrolyte and lithium ion battery containing electrolyte
CN107546415A
High-voltage-resistant lithium ion battery electrolyte and lithium ion battery
CN108134138A
Crown ether electrolyte and application thereof
CN111293356A
Lithium secondary battery
JP2000306602A
Cited By
Electrolyte additive, electrolyte and lithium battery
CN122716433A
Electrolyte additive, electrolyte and lithium battery
CN122716433B