Electrolyte and battery

By using electrolyte containing functional additives with disulfide bonds and thiophene structures in lithium-ion batteries, the stability problem of the positive electrode/electrolyte interface at high voltage is solved, and a dense interface film is formed, which significantly improves the circulation of lithium-ion batteries. and storage performance.

CN118970176APending Publication Date: 2024-11-15EVE ENERGY CO LTD

Patent Information

Application Number
CN202410993470.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing technology is difficult to develop a stable positive electrode/electrolyte interface under high voltages. Conventional carbonate electrolytes are easy to oxidize and decompose, resulting in safety problems and collapse of the positive electrode material structure. There are fewer types of high-voltage positive electrode film forming additives, which limits lithium-ion batteries. development.

Method used

An electrolyte is adopted, including lithium salt, organic solvent, carbonate additive and sulfur-containing additive. The first functional additive has a disulfide bond and a thiophene structure, and can form dense CEI and SEI films at the interface between positive and negative electrodes to inhibit side Reaction, improves the cycle stability and high-temperature storage characteristics of the battery.

Benefits of technology

The electrolyte forms a stable interface film at high voltage, which significantly improves the circulation performance and high-temperature storage characteristics of lithium-ion batteries, enhances lithium conductivity, reduces side reactions, and optimizes the battery's room temperature and high-temperature circulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118970176A_ABST
    Figure CN118970176A_ABST
Patent Text Reader

Abstract

The invention provides an electrolyte and a battery. The electrolyte comprises a lithium salt, an organic solvent, a carbonic ester additive, a first functional additive and a second functional additive, the electrolyte has relatively high high-voltage stability, not only can form a stable CEI film on a positive electrode interface, but also can form a stable SEI film on a negative electrode interface, so that the side reaction of the positive electrode interface and the negative electrode interface is effectively inhibited, the service life of the electrolyte is prolonged, and the service life of the electrolyte is prolonged. And the normal-temperature and high-temperature circulation and high-temperature storage characteristics of a high-voltage battery system can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of lithium batteries, and in particular relates to an electrolyte and a battery. Background Art

[0002] Developing high-voltage cathode materials is one of the important ways to develop high-energy-density lithium-ion batteries. The charged electrode material is in a high oxidation state, and the electrolyte is prone to electrochemical oxidation and chemical oxidation reactions on the cathode surface, thereby forming a solid electrolyte interface film (CEI film) on the cathode surface.

[0003] CEI membrane has a dual effect on the performance of positive electrode materials. On the one hand, CEI membrane can prevent the continuous side reaction between electrolyte and electrode materials; on the other hand, CEI membrane has relatively low electronic conductivity and ionic conductivity, which increases the positive electrode interface impedance and causes a decrease in cycle efficiency. Therefore, a dense and stable CEI membrane is of great significance to the performance of positive electrode materials.

[0004] However, conventional carbonate electrolytes will continue to oxidize and decompose under high voltage, generating a large amount of gas and heat that may cause safety issues; and the dissolution of transition metal ions causes the collapse of the cathode material structure, which seriously restricts the performance of high-voltage cathode materials and the development of lithium-ion batteries. Therefore, the development of high-voltage electrolytes, especially the study of stable cathode / electrolyte interfaces under high voltage, is urgent.

[0005] At present, there are two main ways to achieve high voltage of electrolyte: 1. Improve the oxidation resistance of the solvent itself: through design, use substitution, grafting and other methods to reduce the HOMO value of the solvent molecule and broaden its electrochemical stability window. 2. Use electrolyte additives. Film-forming additives: Additives can lose electrons and oxidize before carbonate solvents, forming a passivation film on the surface of the positive electrode, inhibiting the dissolution of transition metal ions and preventing the electrolyte from reacting with the electrode; Adsorption additives: Additives complex with transition metal ions on the surface of the electrode to ensure the charge balance of the electrode surface and passivate the catalytic active sites, thereby stabilizing the system. Considering the cost, process difficulty and performance improvement, the mainstream path to achieve high pressure of the electrolyte and improve the stability of the electrolyte is still to add electrolyte additives.

[0006] However, at present, there are relatively few types of high-voltage positive electrode film-forming additives that can be used on the market. Therefore, the development of new practical positive electrode film-forming high-voltage electrolyte positive electrode additives to further improve the electrolyte stability and optimize the cycle performance of lithium batteries is still an urgent problem to be solved. Summary of the invention

[0007] In order to solve the problems and deficiencies in the prior art, the present invention provides an electrolyte and a battery. The electrolyte has high high-voltage stability, can not only form a stable CEI film at the positive electrode interface, but also can form a stable SEI film at the negative electrode interface, effectively inhibit the side reactions at the positive and negative electrode interfaces, and can improve the normal temperature, high temperature cycle and high temperature storage characteristics of the high-voltage battery system.

[0008] According to a first aspect of the present invention, an electrolyte is provided, comprising a lithium salt, an organic solvent, a carbonate additive, a first functional additive, and a second functional additive; the structural formula of the first functional additive is as follows:

[0009] Wherein R1, R2, R3, R4, R5, and R6 are each independently selected from hydrogen, C1-C10 straight chain or branched alkyl or alkoxy, C1-C10 straight chain or branched alkyl or alkoxy substituted by halogen, C3-C10 straight chain or branched alkenyl, C3-C10 straight chain or branched alkynyl, C6-C26 unsubstituted aryl, C6-C26 aryl substituted by alkyl, and / or hydroxyl, and / or halogen, C7-C27 unsubstituted aryl, C7-C27 benzyl substituted by alkyl, and / or hydroxyl, and / or halogen; the second functional additive is a sulfur-containing additive, and the sulfur-containing additive includes vinyl sulfate and 1,3-propane sultone.

[0010] In the electrolyte provided by the present invention, the carbonate additive and the second functional additive (sulfur-containing additive) are mainly involved in forming a good SEI film at the negative electrode, while the first functional additive can participate in the film formation of the positive electrode and the negative electrode, which can not only further improve the interface stability of the negative electrode, but also have a more obvious effect on further improving the interface stability of the positive electrode. Therefore, these three additives are used together to form a dense and uniform CEI and SEI film at the interface of the positive and negative electrodes, further optimize the interface stability of the positive and negative electrodes, reduce the side reactions at the interface of the positive and negative electrodes, and further optimize the cycle stability of the battery using it, especially for the normal temperature, high temperature cycle and high temperature storage characteristics of the battery.

[0011] Specifically, it should be emphasized that the first additive structure contains disulfide bonds, which are easy to oxidize and reduce, and also has a thiophene structure, so it is easy to participate in the dense film formation of the positive electrode CEI and the negative electrode SEI, which can improve the interfacial stability and lithium conductivity of the CEI and SEI films, and optimize the battery cycle performance. In particular, the special structure of the first additive has a more obvious effect on participating in the film formation of the positive electrode CEI and further improving the stability of the positive electrode interface, so it can have a more obvious improvement in the performance optimization of the final battery, such as high-temperature storage characteristics and room temperature / high temperature cycle performance. In addition, sulfur-containing additives include vinyl sulfate (DTD) and 1,3-propane sultone (PS). These two sulfur-containing additives not only do not have obvious adverse reactions with the first additive, but also can produce a certain synergistic effect when used in combination, thereby further enhancing the interfacial stability and lithium conductivity of the CEI and SEI films, and effectively improving the room temperature and high temperature cycle and storage performance of high-voltage battery systems such as ternary systems.

[0012] Preferably, the mass proportion of the first functional additive in the electrolyte is 0.3-1.0%. If the first additive is too little, the density and uniformity of the interface film formed at the interface of the positive and negative electrodes will deteriorate, and it cannot effectively improve the interface stability of the positive and negative electrodes with other additives, resulting in a reduction in the degree of optimization of the battery performance. If the first additive is too much, on the one hand, it will limit the role of other electrolyte additives or other components of the electrolyte, and deteriorate the overall performance of the electrolyte. Therefore, if the first functional additive is too much, it will also deteriorate the stability of the electrolyte, that is, it will not be conducive to further improving the interface stability of the positive and negative electrodes, and the cycle performance of the battery will be reduced. At the same time, too much of the first additive will also transition to film formation, which is not conducive to the deintercalation and insertion of lithium ions, and therefore is not conducive to the cycle performance of the battery.

[0013] Preferably, the mass proportion of sulfur-containing additives in the electrolyte is 0.5-2.0%. Sulfur-containing additives mainly assist film formation at the negative electrode and have high thermal stability. Too little addition is not conducive to the formation of a dense SEI film at the negative electrode, and too much addition will result in excessive film formation, which is not conducive to the deintercalation of lithium ions and leads to decreased cycle performance. And too much addition is not conducive to its interaction with other electrolyte additives, affecting the performance of other electrolyte additives or other components of the electrolyte.

[0014] Preferably, the sulfur-containing additive further includes propenyl-1,3-sultone. Further adding the sulfur-containing additive can further coordinate the performance of the sulfur-containing additive. At the same time, under such a combination, the sulfur-containing additive can further work together with the first additive to exert a more excellent performance, which is more conducive to the interface stability of the positive and negative electrodes and reduces side reactions, thereby further optimizing the performance of the battery.

[0015] Preferably, the first functional additive includes at least one of bis(2-thienyl) disulfide, 2-chloro-5-[(5-chlorothien-2-yl) disulfide]thiophene, 5,5'-disulfonyldiylbis(2-acetylamino-4-methylthiophene-3-carboxylic acid diethyl ester), and N,N'-(disulfodi-5,2-thienyldiyl)bisacetamide. The structural formula of bis(2-thienyl) disulfide is The structural formula of 2-chloro-5-[(5-chlorothien-2-yl)disulfide]thiophene is The structural formula of 5,5'-disulfonyldiylbis(2-acetylamino-4-methylthiophene-3-carboxylic acid diethyl ester) is The structural formula of N, N'-(dithiodi-5,2-thiophenediyl)bisacetamide is

[0016] Preferably, the carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate; the mass proportion of the carbonate additive in the electrolyte is 0.2-1.0%. Carbonate additives such as vinylene carbonate (VC) and fluoroethylene carbonate (FEC) form a film at the negative electrode, but too little addition will not form a dense SEI film, and too much addition will lead to high impedance and high-temperature gas production. At the same time, too much addition is not conducive to its interaction with other electrolyte additives, affecting the performance of other electrolyte additives or other components of the electrolyte, which is not conducive to the comprehensive performance of the electrolyte.

[0017] Preferably, the electrolyte provided by the present invention also includes a lithium salt additive, and the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate); the mass proportion of the lithium salt additive in the electrolyte is 0.5-1.0%. The lithium salt additive also has the function of forming positive and negative electrodes, and can further improve the density of the generated CEI film and SEI film, inhibit the dissolution of positive electrode metal ions, reduce the damage of metal ions to the negative electrode SEI film, and improve the thermal stability of the film. If the amount of addition is too small, a dense SEI film cannot be formed, and if the amount of addition is too large, gas production and electrical performance will be reduced.

[0018] Preferably, the lithium salt includes lithium hexafluorophosphate, and the concentration of the lithium salt in the electrolyte is 1.0 to 1.3 mol / L.

[0019] Preferably, the organic solvent includes at least two of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

[0020] Preferably, when the organic solvent includes ethylene carbonate and ethyl methyl carbonate, calculated by volume fraction, the volume fractions of ethylene carbonate, dimethyl carbonate, diethyl carbonate and ethyl methyl carbonate in the organic solvent are 20-40%, 0-20%, 0-20% and 30-50%, respectively.

[0021] According to the second aspect of the present invention, a battery is provided, comprising the above-mentioned electrolyte. By using the electrolyte provided by the present invention, a uniform and dense CEI film and SEI film can be formed on both sides of the positive electrode and the negative electrode of the battery, which greatly optimizes the stability of the positive and negative electrode interfaces, while enhancing the lithium conductivity of the positive and negative electrodes, and improving the lithium ion transmission efficiency, thereby significantly optimizing the normal temperature and high temperature cycle and storage performance of the battery using the electrolyte. In particular, the introduction of the first additive containing a disulfide bond and a thiophene structure and the sulfur-containing additive plays a key role in further improving the density and uniformity of the positive electrode CEI film, greatly improving the stability of the positive electrode interface, and making the cycle performance optimization effect of the battery more obvious. DETAILED DESCRIPTION

[0022] In order to enable those skilled in the art to better understand the solutions of the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below. Obviously, the described embodiments are only embodiments of a part of the present invention, rather than all embodiments.

[0023] Example 1

[0024] 1. Electrolyte and preparation of electrolyte

[0025] The electrolyte in this embodiment is composed of an organic solvent, a lithium salt and an additive, and the lithium salt is an electrolyte salt. The additives are carbonate additives, lithium salt additives, first functional additives, and second functional additives (sulfur-containing additives). The carbonate additive is fluoroethylene carbonate (FEC), and its mass fraction in the electrolyte is 0.5%. The lithium salt additive is lithium difluorophosphate (LiPO2F2), and its mass fraction in the electrolyte is 1.0%. The sulfur-containing additives are 1,3-propane sultone (PS) and vinyl sulfate (DTD), and their mass fractions in the electrolyte are 0.7% and 0.3% respectively (total 1.0%). The first additive is bis(2-thienyl) disulfide The mass fraction in the electrolyte is 0.5%. The lithium salt is lithium hexafluorophosphate (LiPF6), and its concentration in the electrolyte is 1.0 mol / L. The organic solvent is composed of ethylene carbonate, diethyl carbonate, and ethyl methyl carbonate. Taking the total volume of the organic solvent as 100%, the volume fraction of ethylene carbonate is 30%, the volume fraction of diethyl carbonate is 20%, and the volume fraction of ethyl methyl carbonate is 50%.

[0026] The preparation of the electrolyte follows the following steps: in an argon atmosphere, add the carbonate additive, lithium salt additive, first additive and sulfur-containing additive to an organic solvent, and finally add lithium hexafluorophosphate (lithium salt) and stir at low temperature to mix evenly.

[0027] 2. Preparation of the battery

[0028] The battery of this embodiment includes a positive electrode, a negative electrode, an electrolyte, and a separator.

[0029] In the preparation of the positive electrode sheet, the positive electrode active material is a nickel-cobalt-manganese ternary material (Li(Ni x Co y Mn z )O2) (where 0.5 ≤ x < 0.8, 0 < y ≤ 0.3, 0 < z ≤ 0.3 and x + y + z = 1). And the preparation method of the positive electrode sheet is as follows: Prepare a slurry by mixing the positive electrode active material (NCM523 in this embodiment), the conductive agent acetylene black, and the binder PVDF in a mass ratio of 94:3:3, coat it on an aluminum foil current collector, and dry it in vacuum to obtain the positive electrode sheet.

[0030] In the preparation of the negative electrode sheet, the negative electrode active material is graphite. And the preparation method of the negative electrode sheet is as follows: Prepare a slurry by mixing the negative electrode active material graphite, the conductive agent acetylene black, and the binders CMC and SBR in a mass percentage of 94:1:2:3, coat it on a copper foil current collector, and dry it in vacuum to obtain the negative electrode sheet.

[0031] After assembling the positive and negative electrode sheets prepared above with a Celgard 2400 separator to obtain an electric core, transfer the electric core into a casing, and then inject the electrolyte prepared in this embodiment, and perform formation and constant volume to obtain the battery of this embodiment.

[0032] Example 2

[0033] 1. Electrolyte and preparation of the electrolyte

[0034] The difference between the electrolyte in this embodiment and that in Example 1 is that: adjust the mass fraction of the first functional additive in the electrolyte to 0.3%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as that in Example 1.

[0035] And the preparation of the electrolyte in this embodiment is the same as that in Example 1.

[0036] 2. Preparation of the battery

[0037] The preparation of the battery in this embodiment is the same as that in Example 1.

[0038] Example 3

[0039] 1. Electrolyte and preparation of the electrolyte

[0040] The difference between the electrolyte in this embodiment and that in Example 1 is that: adjust the mass fraction of the first functional additive in the electrolyte to 0.7%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as that in Example 1.

[0041] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0042] 2. Preparation of batteries

[0043] The preparation of the battery in this example is consistent with that in Example 1.

[0044] Example 4

[0045] 1. Electrolyte and preparation of electrolyte

[0046] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the first functional additive in the electrolyte is adjusted to 0.2%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Embodiment 1.

[0047] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0048] 2. Preparation of batteries

[0049] The preparation of the battery in this example is consistent with that in Example 1.

[0050] Example 5

[0051] 1. Electrolyte and preparation of electrolyte

[0052] The electrolyte in this embodiment is different from that in Embodiment 1 in that the mass fraction of the first functional additive in the electrolyte is adjusted to 1.2%, which can be obtained by adaptively adjusting the amount of the organic solvent (one or more of the organic solvents can be adjusted). The rest is the same as in Embodiment 1.

[0053] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0054] 2. Preparation of batteries

[0055] The preparation of the battery in this example is consistent with that in Example 1.

[0056] Example 6

[0057] 1. Electrolyte and preparation of electrolyte

[0058] The electrolyte in this embodiment is different from that in Embodiment 1 in that the composition of the sulfur-containing additive is adjusted to 1,3-propane sultone (PS), vinyl sulfate (DTD) and propenyl-1,3-sultone (PST), and the mass fractions of these three additives in the electrolyte are 0.5%, 0.3% and 0.2% (total 1.0%) respectively. The rest is the same as in Embodiment 1.

[0059] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0060] 2. Preparation of batteries

[0061] The preparation of the battery in this example is consistent with that in Example 1.

[0062] Example 7

[0063] 1. Electrolyte and preparation of electrolyte

[0064] The electrolyte in this embodiment is different from that in embodiment 1 in that the first additive is adjusted to 2-chloro-5-[(5-chlorothiophene-2-yl)disulfide]thiophene The rest is consistent with Example 1.

[0065] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0066] 2. Preparation of batteries

[0067] The preparation of the battery in this example is consistent with that in Example 1.

[0068] Example 8

[0069] 1. Electrolyte and preparation of electrolyte

[0070] The electrolyte in this embodiment is different from that in embodiment 1 in that the first additive is adjusted to 5,5'-disulfonyldiylbis(2-acetylamino-4-methylthiophene-3-carboxylic acid diethyl ester) The rest is consistent with Example 1.

[0071] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0072] 2. Preparation of batteries

[0073] The preparation of the battery in this example is consistent with that in Example 1.

[0074] Example 9

[0075] 1. Electrolyte and preparation of electrolyte

[0076] The electrolyte in this embodiment is different from that in embodiment 1 in that the first additive is adjusted to 5,5'-disulfonyldiylbis(2-acetylamino-4-methylthiophene-3-carboxylic acid diethyl ester) The rest is consistent with Example 1.

[0077] The preparation of the electrolyte in this embodiment is consistent with that in Example 1.

[0078] 2. Preparation of batteries

[0079] The preparation of the battery in this example is consistent with that in Example 1.

[0080] Example 10

[0081] 1. Electrolyte and preparation of electrolyte

[0082] The electrolyte in this embodiment is different from that in embodiment 6 in that the first additive is adjusted to 2-chloro-5-[(5-chlorothiophene-2-yl)disulfide]thiophene The rest is consistent with Example 6.

[0083] The preparation of the electrolyte in this embodiment is consistent with that in Example 6.

[0084] 2. Preparation of batteries

[0085] The preparation of the battery in this example is consistent with that in Example 6.

[0086] Embodiment 11

[0087] 1. Electrolyte and preparation of electrolyte

[0088] The electrolyte in this embodiment is different from that in embodiment 6 in that the first additive is adjusted to 5,5'-disulfonyldiylbis(2-acetylamino-4-methylthiophene-3-carboxylic acid diethyl ester The rest is consistent with Example 6.

[0089] The preparation of the electrolyte in this embodiment is consistent with that in Example 6.

[0090] 2. Preparation of batteries

[0091] The preparation of the battery in this example is consistent with that in Example 6.

[0092] Example 12

[0093] 1. Electrolyte and preparation of electrolyte

[0094] The electrolyte in this embodiment is different from that in embodiment 6 in that the first additive is adjusted to N, N'-(dithiodi-5,2-thiophenediyl)bisacetamide The rest is consistent with Example 6.

[0095] The preparation of the electrolyte in this embodiment is consistent with that in Example 6.

[0096] 2. Preparation of batteries

[0097] The preparation of the battery in this example is consistent with that in Example 6.

[0098] Comparative Example 1

[0099] 1. Electrolyte and preparation of electrolyte

[0100] The electrolyte in this comparative example is different from that in Example 1 in that the first functional additive is not added. The rest is the same as that in Example 1.

[0101] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0102] 2. Preparation of batteries

[0103] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0104] Comparative Example 2

[0105] 1. Electrolyte and preparation of electrolyte

[0106] The electrolyte in this comparative example is different from that in Example 1 in that no second functional additive is added, that is, no sulfur-containing additive is added. The rest is the same as in Example 1.

[0107] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0108] 2. Preparation of batteries

[0109] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0110] Comparative Example 3

[0111] 1. Electrolyte and preparation of electrolyte

[0112] The electrolyte in this comparative example is different from that in Example 1 in that the second functional additive (sulfur-containing additive) is only 1,3-propane sultone (PS), and the mass fraction of PS in the electrolyte is 1%. The rest is the same as in Example 1.

[0113] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0114] 2. Preparation of batteries

[0115] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0116] Comparative Example 4

[0117] 1. Electrolyte and preparation of electrolyte

[0118] The electrolyte in this comparative example is different from that in Example 1 in that no carbonate additive is added (ie, no FEC is added). The rest is the same as in Example 1.

[0119] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0120] 2. Preparation of batteries

[0121] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0122] Comparative Example 5

[0123] 1. Electrolyte and preparation of electrolyte

[0124] The electrolyte in this comparative example is different from that in Example 1 in that no carbonate additive (ie, no FEC) and no second functional additive (ie, no sulfur-containing additives PS and DTD) are added. The rest is the same as in Example 1.

[0125] The preparation of the electrolyte in this comparative example is consistent with that in Example 1.

[0126] 2. Preparation of batteries

[0127] The preparation of the battery in this comparative example is consistent with that in Example 1.

[0128] Test Case

[0129] 1. Experimental Construction Method

[0130] The batteries (lithium-ion batteries) prepared in all the above embodiments and comparative examples were subjected to electrochemical tests using a Xinwei charge and discharge test cabinet.

[0131] (1) Cycle performance test of lithium-ion batteries:

[0132] At 25 or 45°C, charge the lithium-ion battery at a constant current of 1.0C (nominal capacity) to a voltage of 4.4V, then charge at a constant voltage of 4.4V to a current ≤0.05C. After standing for 10 minutes, discharge at a constant current of 1C to 2.8V. The above is one charge and discharge cycle.

[0133] The capacity retention rate (%) of a lithium-ion battery after N cycles = (discharge capacity at the Nth cycle / initial discharge capacity) × 100%, where N is the number of cycles of the lithium-ion battery.

[0134] (2) High temperature storage performance test of lithium-ion batteries:

[0135] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. The volume of the tested lithium-ion battery was V0, and the initial capacity was C0. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 90 days, and the volume of the tested lithium-ion battery was taken out and recorded as V1, the capacity remained C1, and the capacity recovered to C2.

[0136] The volume expansion ratio (%) of a lithium-ion battery after storage at 60°C for 90 days = (V1-V0)V0×100%.

[0137] The capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C1 / C0)×100%, and the capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C2 / C0)×100%.

[0138] The batteries obtained from the above examples and comparative examples were tested as follows:

[0139] (a) High temperature storage performance test of lithium-ion batteries:

[0140] At 25°C, the lithium-ion battery was charged at a constant current of 1C to a voltage of 4.4V, and then charged at a constant voltage of 4.4V to a current of 0.05C. The volume of the tested lithium-ion battery was V0, and the initial capacity was C0. The lithium-ion battery was then placed in a constant temperature box at 60°C and stored for 90 days, and the volume of the tested lithium-ion battery was taken out and recorded as V1, the capacity remained C1, and the capacity recovered to C2.

[0141] The volume expansion rate (%) of a lithium-ion battery after storage at 60°C for 90 days = (V1-V0) / V0×100%.

[0142] The capacity retention rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C1 / C0)×100%, and the capacity recovery rate (%) of the lithium-ion battery after storage at 60°C for 90 days = (C2 / C0)×100%.

[0143] (b) High temperature storage experiment:

[0144] Carry out 5 charge and discharge cycle tests at room temperature at a charge and discharge rate of 1C, and then charge to full charge at a rate of 1C. Record the 1C capacity Q0 and battery volume V0 respectively. Store the fully charged battery at 60°C for 90 days, record the battery volume V1 and 1C discharge capacity Q1, then charge and discharge the battery at room temperature at a rate of 1C for 5 weeks, record the 1C discharge capacity Q2, and calculate the experimental data such as the battery's high temperature storage capacity retention rate, capacity recovery rate and volume change rate. The recorded results are shown in Table 1 below. The calculation formulas used are as follows: Capacity retention rate (%) = Q1 / Q0×100%; Capacity recovery rate (%) = Q2 / Q0×100%; Volume change rate (%) = (V1-V0) / V0×100%.

[0145] (c) Normal temperature cycle test:

[0146] Place the battery at 25°C, record the initial capacity as A1, the capacity after 5C / 5C cycle to 2000 weeks as A2, and calculate the capacity retention rate of the battery after 2000 weeks of high-temperature cycle by the following formula: Cycle capacity retention rate (%) = A2 / A1×100%.

[0147] (d) High temperature cycle test:

[0148] Place the battery at 45°C, record the initial capacity as A1, the capacity after 5C / 5C cycle to 2000 cycles as A2, and calculate the capacity retention rate of the battery after 2000 cycles of high-temperature cycle by the following formula: Cycle capacity retention rate (%) = A2 / A1×100%, and record the result.

[0149] 2. Experimental results

[0150] The test results of the battery performance of the above examples and comparative examples are shown in Table 1 below.

[0151] Table 1. Test results of relevant performance of batteries in the embodiments and comparative examples

[0152]

[0153]

[0154] As can be seen from Table 1, the electrolyte provided by the present invention has high high-voltage stability, and can not only form a stable CEI film at the positive electrode interface, but also form a stable SEI film at the negative electrode interface, effectively inhibiting the side reactions at the positive and negative electrode interfaces, and can improve the room temperature, high temperature cycle and high temperature storage characteristics of the high-voltage battery system. For details, refer to Examples 1 to 12.

[0155] In Comparative Example 1, the first functional additive is not added, that is, the functional additive containing both a disulfide bond and a thiophene structure is not added, and the room temperature cycling performance deteriorates, which ultimately leads to poor high-temperature storage and cycle performance, obvious gas production during high-temperature storage, and a large volume change rate.

[0156] In Comparative Example 2, no second functional additive is added, that is, no sulfur-containing additive is added (that is, no PS and DTD are added), and the room temperature cycling performance deteriorates, which ultimately leads to poor high-temperature storage and cycling performance, obvious gas production during high-temperature storage, and a large volume change rate.

[0157] In Comparative Example 3, the second functional additive (sulfur-containing additive) is only 1,3-propane sultone PS, and the room temperature cycling performance deteriorates, which ultimately leads to poor high-temperature storage and cycle performance. The high-temperature storage produces obvious gas and has a large volume change rate.

[0158] In Comparative Example 4, no carbonate additives were added (ie, no FEC was added), and the room temperature cycling performance deteriorated, which ultimately led to poor high temperature storage and cycling performance, obvious gas production during high temperature storage, and a large volume change rate.

[0159] In Comparative Example 5, no carbonate additives (i.e., no FEC) and no second functional additives (i.e., no sulfur-containing additives PS and DTD) were added, and the room temperature cycling performance deteriorated, which ultimately led to poor high-temperature storage and cycling performance, and obvious gas production during high-temperature storage.

[0160] Further comparing Example 1 with Examples 2 to 5, the mass fractions of the first functional additive (bis(2-thienyl) disulfide) in the electrolyte in Examples 4 and 5 are 0.2% and 1.2%, respectively. If the mass fraction is too little or too much, the interface film formed will be thicker, which will increase the impedance, and the battery cycle performance and storage performance will decrease to a certain extent. And further comparing Examples 1 to 3, it can be found that when the mass fraction of the first functional additive (bis(2-thienyl) disulfide) in the electrolyte is 0.5%, the high temperature storage performance, room temperature cycle performance and high temperature cycle performance of the battery are better.

[0161] Comparing Example 1 and Example 6, it can be found that when the sulfur content increases with propenyl-1,3-sultone (PST), the battery has better cycle and storage performance. This shows that the addition of PST can further improve the high-voltage stability of the electrolyte, optimize the positive and negative interface stability, and further optimize the high-temperature storage performance, room-temperature cycle performance, and high-temperature cycle performance of the battery.

[0162] At the same time, it can be further observed from Example 1 and Examples 7 to 9 that when the type of the first functional additive is changed, the battery can also maintain good or even better performance. It can also be known that when used in combination with the sulfur-containing additive, the battery performance is better.

[0163] In addition, further observations can be made in Example 6 and Examples 10 to 12. Compared with Example 1 and Examples 7 to 9, PST is added to the sulfur-containing additives in Examples 6 and Examples 10 to 12, so the high-voltage stability of the electrolyte is better, and the positive and negative electrode interface stability can be further optimized, and the high-temperature storage performance, room-temperature cycle performance, and high-temperature cycle performance of the battery can be optimized. It can also be seen that when used in combination with PST, the battery performance is better.

[0164] The above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit the protection scope of the present invention. Although the present invention is described in detail with reference to the above embodiments, ordinary technicians in the relevant field should understand that the technical solutions of the present invention can be modified or equivalently replaced, but these modifications or replacements are all within the protection scope of the present invention.

Claims

1. An electrolyte, characterized in that: Including lithium salt, organic solvent, carbonate additive, first functional additive, second functional additive; The structural formula of the first functional additive is as follows: wherein R1, R2, R3, R4, R5, and R6 are each independently selected from hydrogen, C1-C10 straight or branched alkyl or alkoxy, C1-C10 straight or branched alkyl or alkoxy substituted with halogen, C3-C10 straight or branched alkenyl, C3-C10 straight or branched alkynyl, C6-C26 unsubstituted aryl, C6-C26 aryl substituted with alkyl, and / or hydroxyl, and / or halogen, C7-C27 unsubstituted aryl, and C7-C27 benzyl substituted with alkyl, and / or hydroxyl, and / or halogen; The second functional additive is a sulfur-containing additive, and the sulfur-containing additive includes vinyl sulfate and 1,3-propane sultone.

2. The electrolyte according to claim 1, characterized in that: The mass proportion of the first functional additive in the electrolyte is 0.3-1.0%.

3. The electrolyte according to claim 1, characterized in that: The sulfur-containing additive accounts for 0.5-2.0% by mass in the electrolyte.

4. The electrolyte according to claim 1, characterized in that: The sulfur-containing additive further includes propenyl-1,3-sultone.

5. The electrolyte according to claim 1, characterized in that: The first functional additive includes at least one of bis(2-thienyl)disulfide, 2-chloro-5-[(5-chlorothien-2-yl)disulfide]thiophene, 5,5'-disulfonyldiylbis(2-acetylamino-4-methylthiophene-3-carboxylic acid diethyl ester), and N,N'-(disulfodi-5,2-thienyl)bisacetamide.

6. The electrolyte according to claim 1, characterized in that: The carbonate additive includes at least one of vinylene carbonate and fluoroethylene carbonate; The carbonate additive accounts for 0.2-1.0% by weight in the electrolyte.

7. The electrolyte according to claim 1, characterized in that: Also included is a lithium salt additive, wherein the lithium salt additive includes at least one of lithium bis(fluorosulfonyl)imide, lithium difluorophosphate, lithium bis(oxalatoborate), and lithium difluorobis(oxalatophosphate); The lithium salt additive accounts for 0.5-1.0% by mass in the electrolyte.

8. The electrolyte according to claim 1, characterized in that: The lithium salt includes lithium hexafluorophosphate, and the concentration of the lithium salt in the electrolyte is 1.0 to 1.3 mol / L.

9. The electrolyte according to claim 1, characterized in that: The organic solvent includes at least two of ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.

10. A battery, characterized in that: Comprising the electrolyte as claimed in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Non-aqueous electrolyte of high-voltage lithium ion batteries

    CN103384017A

  • Lithium ion battery electrolyte suitable for NCM811 and SiO-C material system and preparation method

    CN110600804A

  • Electrolyte and preparation method and application thereof

    CN113381071A

  • Nonaqueous electrolyte solution for electricity storage devices, and electricity storage device using same

    CN114008830A

  • Silicon-based lithium ion battery electrolyte and battery thereof

    CN116632347A

Cited By

  • Electrolyte and battery

    CN119764558A

  • Electrolyte for high and low temperature resistant sodium ion battery as well as preparation method and application of electrolyte

    CN120637603A

  • High and low temperature resistant electrolyte for sodium ion battery and preparation method and application thereof

    CN120637603B