Secondary liquid injection electrolyte, liquid injection method and lithium ion battery
By adopting a secondary injection electrolyte solution in lithium-ion batteries and using a combination design of fluorovinyl carbonate and unsaturated phosphate, the structural instability and expansion of lithium-ion batteries under high voltage/high temperature conditions is solved. It improves the battery's fast charging and high-temperature cycling performance and avoids the disadvantages of increasing battery DC internal resistance.
Patent Information
- Application Number
- CN202411015674.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-15
- Estimated Expiration
- 2044-07-26
AI Technical Summary
Prior Art Under high voltage/high temperature conditions, the unstable positive electrode structure of lithium-ion batteries and the expansion of silicon-based negative electrodes lead to insufficient cycle performance and calendar life, especially the low utilization rate of borate and unsaturated phosphate additives. Increase the DC internal resistance of the battery, making it difficult to take into account the high-efficiency electrolyte design of both positive and negative electrodes.
Using the secondary injection electrolyte solution, the additive combination design of electrolyte A and electrolyte B, where electrolyte A contains fluorovinyl carbonate and lithium difluorophosphate, and electrolyte B contains unsaturated phosphate and unsaturated phosphite. The ester is concentratedly added with unsaturated additives through the secondary injection design to avoid its participation in the negative electrode film formation, and improve the positive electrode film formation efficiency and electrolyte cost.
It significantly improves the performance of lithium-ion batteries under fast charging and high-temperature circulation, avoids the problem of increased DC resistance of the battery, and improves the overall performance of the battery, especially the circulation performance under high temperature conditions.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of battery electrolytes, and in particular to a secondary injection electrolyte, an injection method and a lithium ion battery. Background Art
[0002] Range anxiety has always been a key factor restricting the large-scale promotion of new energy vehicles, which is mainly determined by the energy density of power batteries. The energy density of power batteries is directly related to the selection of positive and negative electrode materials. According to the different positive electrode materials, the current commercial power batteries are divided into lithium iron phosphate batteries and ternary batteries. Among them, ternary batteries occupy the high-end car market with their energy density advantages. To further improve the energy density of batteries, the more mature route is to use high-nickel or high-voltage positive electrode materials (LiNi x Co y Mn (1-x-y) O2) matches silicon-based negative electrode materials (SiO x , SiC, etc.), but the problems of positive electrode instability and negative electrode silicon expansion under high voltage / high nickel seriously limit the cycle performance and calendar life of the battery, especially under high temperature conditions.
[0003] The optimization of positive and negative material structures and the design of electrolyte formula are two key ways to solve the shortcomings of ternary battery high temperature performance. Among them, the direction of material optimization strategy is relatively clear, and the main purpose is to improve the structural stability of the battery during high temperature cycling or storage, such as single crystallization, metal ion doping, surface coating and gradient structure design of the positive electrode, carbon coating, pre-lithiation of silicon oxide, porous carbon deposition silicon, etc. for the negative electrode. In terms of electrolyte formulation strategy, the design difficulty and challenge are greater because it is necessary to take into account both positive and negative electrode factors. For power batteries using silicon negative electrode materials, the most critical factor restricting their electrical performance is the repeated destruction and formation of the solid electrolyte interface (SEI) caused by the expansion of the silicon-based negative electrode during the cycle. The electrolyte design mainly improves the battery cycle performance by adding fluoroethylene carbonate (FEC) as a sacrificial additive, but FEC itself has a long thermal stability and is easy to decompose to produce HF, which will cause further deterioration of the battery's high temperature performance. In view of the problem of unstable positive electrode structure under high voltage / high temperature, the main strategy in electrolyte design is to add boron or phosphorus additives to form a stable and dense electrochemical interface (CEI) to inhibit the positive electrode interface side reaction. Unsaturated B / P acid ester additives can form a dense and stable CEI on the positive electrode surface, which has a significant effect on improving the dissolution of positive electrode metal ions and interface side reactions. However, due to the presence of unsaturated bonds, this type of additive often also participates in the positive electrode film formation. The existing process adopts a one-time injection method. If too much is added, the battery DC internal resistance (DCR) will be seriously deteriorated; if too little is added, it will be consumed in the negative electrode film formation and the amount of participation in the CE I reaction will be insufficient. Therefore, the application of this type of additive in power batteries is seriously restricted.
[0004] In the prior art, some use borates and unsaturated phosphate compounds in high-voltage nickel-manganese-oxide lithium battery systems to maintain the stability of the positive electrode structure and oxidation resistance, inhibit the decomposition of the electrolyte, and improve the battery cycle life. Others use a combination of multiple additives such as fluorinated cyclic carbonates, phosphate compounds containing unsaturated hydrocarbon groups, boron-containing lithium salt additives and second additives to significantly improve the high-temperature performance of the battery, wherein the second additive is at least one of a trinitrile compound and a cyclic carboxylic anhydride.
[0005] Although the above schemes have improved battery performance to a certain extent through the directional selection and combination of additives, there are still some problems such as low additive utilization and increased DCR. Therefore, the development of efficient electrolytes and batteries that take into account both silicon-based negative electrodes and high-nickel / high-voltage ternary positive electrodes is still a technical point and difficulty that the industry urgently needs to solve. Summary of the invention
[0006] In view of the problems existing in the prior art, the present invention provides a secondary injection electrolyte, an injection method and a lithium ion battery, including an electrolyte A for primary injection and an electrolyte B for secondary injection. The additive combination of electrolyte A and electrolyte B is improved, and the secondary battery prepared with the obtained electrolyte shows excellent performance in fast charging, high-temperature cycling and other aspects.
[0007] The technical solution of the present invention is as follows:
[0008] In a first aspect of the present invention, a secondary injection electrolyte is provided, comprising an electrolyte A for primary injection and an electrolyte B for secondary injection; wherein the electrolyte A accounts for 78% to 92% of the total injection mass of the battery, and the electrolyte B accounts for 8% to 22% of the total injection mass of the battery, and the electrolyte A and the electrolyte B both include lithium salt, solvent and additives;
[0009] The first additive in the electrolyte A is fluoroethylene carbonate, and the second additive comprises lithium difluorophosphate and at least one selected from vinyl sulfate and methylene methanedisulfonate;
[0010] The first additive in the electrolyte B includes at least one of unsaturated phosphate and unsaturated phosphite or unsaturated borate, and the second additive is one or two of lithium difluorophosphate, lithium difluorobisoxalate phosphate and lithium tetrafluorooxalate phosphate.
[0011] In view of the several problems in cycling and high temperature in high energy density batteries, especially high nickel or high voltage positive electrode matching silicon-based negative electrode system, a secondary injection electrolyte design scheme is proposed, which can solve the application problem of unsaturated phosphates, unsaturated phosphites or unsaturated borates in the electrolyte under this system.
[0012] In some embodiments of the present invention, in the electrolyte A, the first additive fluoroethylene carbonate accounts for 1% to 15% of the total mass of the electrolyte A; preferably 6% to 8%.
[0013] The second additive lithium difluorophosphate accounts for 0.5% to 1.2% of the total mass of the electrolyte, and the second additive vinyl sulfate and / or methylene disulfonate accounts for 0.5% to 2.5% of the total mass of the electrolyte A; preferably 0.8% to 1%.
[0014] Specifically, the amount of the first additive fluoroethylene carbonate (FEC) added is directly related to the type and proportion of the silicon base in the negative electrode.
[0015] Specifically, the amount of the first additive fluoroethylene carbonate (FEC) added is positively correlated with the amount of silicon-based addition in the negative electrode; if silicon oxide (SiOx) is used as the negative electrode, the ratio of the mass fraction of FEC in the electrolyte A to the mass fraction of SiOx in the negative electrode is 2:1 to 1:2; if porous carbon-deposited silicon is used as the negative electrode, the ratio of the mass fraction of FEC in the electrolyte A to the mass fraction of porous carbon-deposited silicon in the negative electrode is 1:2 to 1:5; if the mass fraction of SiOx in the negative electrode is 5%, the mass fraction of FEC in the electrolyte A accounts for 2.5% to 10%, preferably 4% to 7%.
[0016] In some embodiments of the present invention, the additives in the electrolyte A also include one or more of ethylene sulfite (ES), 1,3-propane sultone (PS), tris(trimethylsilyl) phosphate (TMSP), lithium difluorooxalatoborate (LiODFB), lithium difluorobis(oxalatophosphate), lithium tetrafluorooxalatophosphate, succinonitrile (SN), adiponitrile (ADN), 1,3,6-hexanetrinitrile (HTCN) and 1,2-bis(2-cyanoethoxy)ethane (DENE), and the added amount is 0.2% to 2% of the total mass of the electrolyte A.
[0017] In some embodiments of the present invention, the first additive in the electrolyte B is at least one of tripropargyl phosphate (TPP), triallyl phosphate, tris(2-cyanoethyl) phosphate, tripropargyl phosphite, triallyl phosphite, tris(2-cyanoethyl) phosphite, tripropargyl borate, triallyl borate and tris(2-cyanoethyl) borate, and the amount of the first additive added is 0.2% to 2% of the total mass of the electrolyte B, preferably 0.2% to 0.8%.
[0018] Specifically, the unsaturated functional group of the first additive in electrolyte B is an alkynyl, alkenyl or cyano group. This type of additive can form a dense CEI film at the positive electrode, alleviate the dissolution of transition metal ions at the positive electrode and the decomposition of FEC at the positive electrode under high temperature and high pressure conditions, and improve the cycle performance of the battery, especially the high temperature cycle performance. However, this type of additive not only participates in the formation of CEI, but also participates in the formation of SEI at the negative electrode, thereby deteriorating the battery DCR. In the electrolyte design, if the content is too little, it will preferentially participate in the formation of SEI, resulting in a significant reduction in the amount of participation in CEI generation, and it is difficult to exert its beneficial effect; if the content increases, it will seriously deteriorate the SEI impedance and affect the fast charging and cycle performance of the battery. It is known that SEI generation is mainly in the first charging to 3.4V before the stage, through the two-injection design, this type of unsaturated additive is concentrated in the two-injection electrolyte, so as to avoid the main disadvantage of the existing one-injection solution that causes the increase of battery DCR due to the use of this type of additive, while greatly improving its participation in CEI generation efficiency and reducing the cost of the electrolyte.
[0019] In some embodiments of the present invention, the amount of the second additive added to the electrolyte B is 0.2% to 1.5% of the total mass of the electrolyte B; preferably 0.3% to 0.7%;
[0020] Preferably, the additive in the electrolyte B further includes fluoroethylene carbonate (FEC), and the added amount is 1% to 15%, preferably 3% to 7%.
[0021] The use of phosphorus-containing lithium salt compounds as the second additive of the secondary injection electrolyte B can work synergistically with the above-mentioned unsaturated additives to increase the content of lithium phosphate-rich structural components in CEI. The structure has superconducting lithium ion characteristics and further reduces the battery DCR.
[0022] In some embodiments of the present invention, the lithium salt is at least one of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) and lithium tetrafluoroborate (LiBF4);
[0023] Preferably, the lithium salt is one or both of lithium hexafluorophosphate (LiPF6) and lithium bis(fluorosulfonyl)imide (LiFSI).
[0024] In some embodiments of the present invention, the lithium salt accounts for 10% to 20% of the total mass of electrolyte A or electrolyte B, preferably 12% to 16%.
[0025] In some embodiments of the present invention, the solvent is two or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, γ-butyrolactone, ethyl acetate, methyl acetate, propyl acetate, methyl propionate, propyl propionate, and ethyl propionate;
[0026] The amount of solvent added to the electrolyte A accounts for 70% to 88% of the total mass of the electrolyte A, preferably 75% to 85%; the amount of solvent added to the electrolyte B accounts for 75% to 88% of the total mass of the electrolyte B, preferably 82% to 87%.
[0027] In a second aspect of the present invention, a method for injecting a secondary injection electrolyte is provided, comprising:
[0028] Determine the total electrolyte injection volume required for the battery according to the battery capacity and injection coefficient, and inject electrolyte A with a mass of "m*total injection volume" into the battery to be injected, and soak for ≥24h at 45℃; where m represents the proportion of electrolyte A to the total injection volume of the battery;
[0029] Set the formation step current to 3.4V or above (e.g. 0.05C charging for 36min, 0.1C charging to 3.4V cut-off), and the aging time is ≥3h;
[0030] The electrolyte B of the mass of "(1-m)*total injection volume" is injected into the formed and aged battery to complete the secondary injection, wherein 1-m represents the proportion of electrolyte B in the total injection volume of the battery.
[0031] In a third aspect of the present invention, a lithium-ion battery is provided, comprising a positive electrode plate, a negative electrode plate, a separator and an electrolyte, wherein the electrolyte is the secondary injection electrolyte described in the first aspect.
[0032] One or more technical solutions of the present invention have the following beneficial effects:
[0033] (1) The present invention realizes "targeted" film formation of additives through the composition design of electrolyte A and electrolyte B, takes advantage of the advantages and avoids the disadvantages, improves the film formation efficiency of positive electrode additives, and avoids the problem of a sharp increase in battery DCR caused by the participation of bidirectional film-forming additives in negative electrode film formation. The high energy density ternary battery prepared by the secondary injection electrolyte has significantly improved its comprehensive performance, especially the high temperature performance.
[0034] (2) The present invention uses a two-injection design to add such unsaturated additives to the two-injection electrolyte, thereby avoiding the main drawback of the existing one-injection solution that the use of such additives leads to an increase in the battery DCR, while greatly improving its efficiency in participating in the generation of CEI and reducing the cost of the electrolyte. At the same time, the phosphorus-containing lithium salt compound is used as the second additive of the two-injection electrolyte of this solution, which can synergize with the above-mentioned unsaturated additives to increase the content of lithium phosphate-rich structural components in CEI. The structure has superconducting lithium ion characteristics, which further reduces the battery DCR.
[0035] (3) The present invention has conducted extensive verification of the electrolyte A formula based on the electrolyte B formula and screened out a combination of additives with a strong match. The secondary battery prepared using the secondary injection electrolyte of the present invention exhibits excellent performance in terms of fast charging, high-temperature cycling, etc. DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with the embodiments.
[0037] The secondary injection electrolyte provided by the present invention is used to prepare a lithium-ion battery with an embedded multi-layer structure negative electrode plate. The specific preparation process is as follows:
[0038] Preparation of positive electrode sheet: polyvinylidene fluoride (PVDF), conductive agent (Super P) and carbon tube (CNT), positive electrode material (NMC, nickel content 90%) are added to N-methylpyrrolidone (NMP) at a mass ratio of 1.5%: 0.5%: 0.5%: 97.5%, mixed evenly to form slurry, and coated on aluminum foil current collector. The single surface density of the positive electrode is 180 ± 3g / m 2 , cold pressed to 3.5g / m 3 , and the positive electrode sheet is obtained after punching.
[0039] Preparation of negative electrode: sodium carboxymethyl cellulose (CMC), polyacrylic acid (PAA), styrene-butadiene rubber latex (SBR), conductive agent (Super P), single-walled carbon nanotube (SWCNT), silicon dioxide (SiO x ) and graphite are added into deionized water in a mass ratio of 0.4%:1.6%:0.8%:0.94%:0.06%:96.2%, and the mixture is stirred and mixed thoroughly. The slurry is coated on the copper foil current collector, and the negative electrode surface density is determined according to the N / P ratio of 1.12, and the surface density is cold pressed to 1.55g / m 3 , and then punch out to make the negative electrode sheet.
[0040] Configuration of the reference electrolyte:
[0041] Electrolyte A is prepared according to the mass ratio of LiPF6:LiFSI:EC:DMC:EMC:FEC:DTD:LiODFB:LiPO2F2:TPP of 10.0%:4.5%:19.5%:37.0%:19.5%:7.0%:1.0%:0.5%:0.8%:0.2%, ensuring strict moisture control (<1ppm) during the entire preparation process and the temperature below 30°C;
[0042] Electrolyte B is prepared according to the mass ratio of LiPF6:LiFSI:EC:DMC:EMC:DTD:LiPO2F2:LiODFP:TPP:tri(2-cyanoethyl)phosphate of 10.0%:4.5%:19.5%:37.5%:19.5%:7%:1.0%:0.5%:0.5%.
[0043] Comparative Examples 1 to 4 are one-time injection schemes; Examples 1 to 10 keep the above-mentioned reference electrolyte A liquid formula unchanged, and only adjust the B liquid formula; Examples 11 to 14 keep the above-mentioned reference electrolyte B liquid formula unchanged, and only adjust the A liquid formula. The specific electrolyte schemes are shown in Table 1. Table 1
[0044]
[0045]
[0046] Preparation of the battery to be filled with liquid: stack the separator, negative electrode plate and positive electrode plate in a "Z" shape to obtain a bare battery cell to be filled with liquid, then use aluminum-plastic film to package the battery cell to be filled with liquid, and after baking, obtain the battery to be filled with liquid. The designed capacity of the battery to be filled with liquid is 2Ah.
[0047] Implementation of the two-injection plan: The electrolyte injection coefficient is calculated as 2.5g / Ah, and liquid A is calculated as 90% of the total injection volume, that is, 4.5g.
[0048] Inject 4.5g of liquid A into the cell to be filled, seal it and soak it at 45℃ for 36h;
[0049] The soaked battery was charged at 0.2C (0.4A) to a voltage cutoff of 3.4V and aged at 45°C for 12h.
[0050] 0.5 g of solution B was injected into the battery after formation aging, and then placed at 25°C for 36 hours and then normally charged and discharged to obtain a battery to be tested.
[0051] Lithium-ion battery testing:
[0052] DCR test: Charge the battery to 4.0V with constant current and constant voltage, let it stand for 6 hours, and then test the DC internal resistance of the battery.
[0053] Rate charging performance test: Charge the battery to 4.25V at 1C and 3C constant current and constant voltage, with a cut-off current of 0.05C, and discharge it to 2.8V at 1C, and calculate the constant current charging capacity ratio. Prepare three soft-pack electrodes, test the charging time at different rates, and determine the maximum charging current at different SOCs through data integration. Determine the optimal step charging scheme (6 stages) for different batteries, and determine the shortest charging time for batteries from 10% to 90% SOC.
[0054] Normal temperature / high temperature cycle performance test: The capacity retention rate under different number of 1C charge and discharge cycles was tested at 25℃ and 45℃ respectively. The charge and discharge cut-off voltage was 2.8V~4.25V, and the constant voltage charge cut-off current was 0.05C.
[0055] Negative electrode transition metal deposition test: After the battery is cycled at 45°C for 1000 times, it is discharged to 2.8V, the battery is disassembled, the negative electrode powder is collected, the ICP is tested, and the Ni element content is recorded.
[0056] The test data of the embodiments and comparative examples are shown in Table 2.
[0057] Table 2
[0058]
[0059] The results show that compared with Comparative Example 1, Comparative Example 2 increases the amount of TPP added by 0.3%, and the high temperature performance of the battery cell is improved, mainly due to the increase in the TPP content involved in the positive electrode film formation, but the DCR and fast charging performance of the battery cell are seriously deteriorated, which is directly related to the deterioration of the negative electrode film formation impedance caused by the increase in TPP content. Compared with Comparative Example 1, Comparative Example 3 effectively reduces the battery DCR and improves the battery fast charging and cycle performance by increasing the composite film formation of LiODFP and TPP at the positive electrode, but LiODFP also has the problem of participating in the consumption of negative electrode film formation, which greatly affects its improvement effect. Compared with Comparative Example 3, Comparative Example 4 further increases tris (2-cyanoethyl) phosphate in the electrolyte formula, and uses cyano complexation to inhibit the dissolution of metal ions to a certain extent, thereby improving the high temperature performance of the battery. However, due to the relatively high viscosity of tris (2-cyanoethyl) phosphate, the battery DCR and fast charging performance are deteriorated to a certain extent.
[0060] Electrolyte A is a reference electrolyte solution. The reference electrolyte formula is used as a reference. Examples 1-3 conducted a single variable experiment on the TPP content in electrolyte B. Compared with the reference examples, it can be found that the two-injection solution can significantly improve the battery fast charging and high-temperature cycle performance. Among them, Example 2 has the best comprehensive performance, proving that under this solution, the optimal addition amount of TTP in the electrolyte is 0.5%. Further analysis of the battery performance comparison results shows that compared with the reference examples, Example 3 has the highest TPP content in liquid B, but the cell DCR is still low, which also proves that the increase in battery DCR caused by TPP is mainly due to its participation in the negative electrode film formation. At the same time, compared with the reference examples 1-3, the improvement in the high-temperature cycle performance and metal dissolution of the cell further proves that the directional control of the film-forming additives for both the positive and negative electrodes can be achieved through two-injection combined with formation voltage control.
[0061] Compared with Example 2, Example 4-6 adds a lithium salt additive to the electrolyte, and conducts a single factor variable experiment on its content. It can be found that the use of a compounding scheme of LiODFB and TPP in electrolyte B can effectively reduce the battery DCR and thus improve the battery fast charging performance. Overall, 0.5% addition has the best effect. Compared with Example 5, Example 7 uses LiODFP to replace LiODFB, and it is found that the high temperature cycle performance and metal dissolution of the battery will be slightly deteriorated, but the battery DCR and rate performance are significantly improved. The main reason is that the increase in the P component in CEI is more conducive to improving the interface impedance, and the increase in the electrolyte B component is more obvious because of its stronger complexing ability. The inhibitory effect on the dissolution of metal ions is more obvious. In Example 8-10, the electrolyte B formula adds tris (2-cyanoethyl) phosphate on the basis of Example 7. The purpose is to utilize the complexing effect of low-impedance polycyano compounds to alleviate the problem of transition metal ion dissolution during the cycle of the ternary system battery, especially during the high temperature cycle. The experimental results also prove the effectiveness of this design. Compared with other embodiments, the Ni element content deposited at the negative electrode after high-temperature cycling is significantly reduced, and the corresponding high-temperature cycling performance of the battery is also significantly improved. However, due to the high viscosity of tri(2-cyanoethyl) phosphate, the battery DCR will be slightly deteriorated. As the amount of addition increases, the degree of deterioration will also increase. Overall, Example 9 (i.e., the amount of tri(2-cyanoethyl) phosphate added is 0.5%) The comprehensive performance of the battery cell is the best.
[0062] The electrolyte B of Example 9, which has been verified to have better comprehensive performance, is selected as the reference electrolyte, and the formula of liquid A is adjusted to further verify the optimal solution of the two-injection scheme. Example 11 and Example 12 verify the effect of the amount of FEC added in liquid A on battery performance. The results show that high FEC content is beneficial to improving room temperature cycles, while low FEC content is more beneficial to high temperature cycles. This is mainly related to the instability of FEC at high temperatures. In practical applications, the amount of FEC added can also be adjusted according to the different requirements of the terminal for battery cycles. Example 13 and Example 14 respectively investigate the effects of DTD and LiPO2F2 on battery performance. The results show that in a battery system with high nickel to silicon negative electrode, both are indispensable. The lack of any one of them in liquid A will cause serious deterioration in the battery cycle performance. In short, combined with the examples, the present invention has verified the design of the two-injection scheme in many aspects. Compared with the existing scheme, the use effect of unsaturated phosphate / borate / phosphite additives focusing on improving the positive electrode interface has been greatly improved, so that the comprehensive performance of the battery has been significantly improved.
[0063] Although the above describes the specific implementation methods of the present invention, it is not intended to limit the scope of protection of the present invention. Those skilled in the art should understand that various modifications or variations that can be made by those skilled in the art on the basis of the technical solution of the present invention without creative work are still within the scope of protection of the present invention.
Claims
1. A secondary injection electrolyte, characterized in that: It includes an electrolyte A for primary injection and an electrolyte B for secondary injection; wherein the electrolyte A accounts for 78% to 92% of the total injection mass of the battery, and the electrolyte B accounts for 8% to 22% of the total injection mass of the battery, and the electrolyte A and the electrolyte B both include lithium salt, solvent and additives; The first additive in the electrolyte A is fluoroethylene carbonate, and the second additive comprises lithium difluorophosphate and at least one selected from vinyl sulfate and methylene methanedisulfonate; The first additive in the electrolyte B includes at least one of unsaturated phosphate and unsaturated phosphite or unsaturated borate, and the second additive is one or two of lithium difluorophosphate, lithium difluorobisoxalate phosphate and lithium tetrafluorooxalate phosphate.
2. The secondary injection electrolyte according to claim 1, characterized in that: In the electrolyte A, the first additive fluoroethylene carbonate accounts for 1% to 15% of the total mass of the electrolyte A; preferably 6% to 8%; The second additive lithium difluorophosphate accounts for 0.5% to 1.2% of the total mass of the electrolyte, and the second additive vinyl sulfate and / or methylene disulfonate accounts for 0.5% to 2.5% of the total mass of the electrolyte A; preferably 0.8% to 1%.
3. The secondary injection electrolyte according to claim 2, characterized in that: The additives in the electrolyte A also include one or more of vinyl sulfite, 1,3-propane sultone, tris(trimethylsilyl)phosphate, lithium difluorooxalatoborate, lithium difluorobisoxalatophosphate, lithium tetrafluorooxalatophosphate, succinonitrile, adiponitrile, 1,3,6-hexanetrinitrile and 1,2-bis(2-cyanoethoxy)ethane, and the added amount is 0.2% to 2% of the total mass of the electrolyte A.
4. The secondary injection electrolyte according to claim 1, characterized in that: The first additive in the electrolyte B is at least one of tripropargyl phosphate, triallyl phosphate, tris(2-cyanoethyl) phosphate, tripropargyl phosphite, triallyl phosphite, tris(2-cyanoethyl) phosphite, tripropargyl borate, triallyl borate and tris(2-cyanoethyl) borate, and the amount of the first additive added is 0.2% to 2% of the total mass of the electrolyte B, preferably 0.2% to 0.8%.
5. The secondary injection electrolyte according to claim 1, characterized in that: The amount of the second additive added to the electrolyte B is 0.2% to 1.5% of the total mass of the electrolyte B, preferably 0.3% to 0.7%; Preferably, the additive in the electrolyte B also includes fluoroethylene carbonate, and the addition amount is 1% to 15%, preferably 3% to 7%.
6. The secondary injection electrolyte according to claim 1, characterized in that: The lithium salt is at least one of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium bis(trifluoromethanesulfonyl)imide and lithium tetrafluoroborate; Preferably, the lithium salt is one or both of lithium hexafluorophosphate and lithium bis(fluorosulfonyl)imide.
7. The secondary injection electrolyte according to claim 2, characterized in that: The lithium salt accounts for 10% to 20% of the total mass of electrolyte A or electrolyte B, preferably 12% to 16%.
8. The secondary injection electrolyte according to claim 1, characterized in that: The solvent is two or more of ethylene carbonate, propylene carbonate, dimethyl carbonate, ethyl methyl carbonate, diethyl carbonate, γ-butyrolactone, ethyl acetate, methyl acetate, propyl acetate, methyl propionate, propyl propionate and ethyl propionate; The amount of solvent added to the electrolyte A accounts for 70% to 88% of the total mass of the electrolyte A, preferably 75% to 85%; the amount of solvent added to the electrolyte B accounts for 75% to 88% of the total mass of the electrolyte B, preferably 82% to 87%.
9. A method for injecting a secondary injection electrolyte according to any one of claims 1 to 8, characterized in that: include: Determine the total electrolyte injection volume required for the battery according to the battery capacity and injection coefficient, and inject electrolyte A with a mass of "m*total injection volume" into the battery to be injected, and soak for ≥24h at 45℃; where m represents the proportion of electrolyte A to the total injection volume of the battery; Set the voltage to 3.4V or above according to the forming step current, and the aging time should be ≥3h; Inject electrolyte B of the mass of "(1-m)*total injection volume" into the formed and aged battery to complete the secondary injection; where 1-m represents the proportion of electrolyte B in the total injection volume of the battery.
10. A lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte, characterized in that: The electrolyte adopts the secondary injection electrolyte as described in any one of claims 1 to 8.
Citation Information
Patent Citations
Liquid injection formation process of lithium iron phosphate battery
CN115000546A
Non-aqueous electrolyte and fast-charging type secondary battery
CN117293391A
Combined electrolyte for secondary liquid injection, lithium ion battery and secondary liquid injection method of lithium ion battery
CN117594874A
Electrolyte injection method for lithium ion battery, and use
WO2023030537A1
High-nickel ternary lithium ion battery electrolyte and lithium ion battery containing electrolyte
WO2023035298A1