Preparation method of miniature insensitive glass sealing connector
By using graphite molds and pretreatment technology in the preparation process of micro connectors, the insensitivity problems caused by electrostatic discharge are solved, the product accuracy and yield rate are improved, the cost is reduced, and it is suitable for mass production.
Patent Information
- Application Number
- CN202411232929.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-15
AI Technical Summary
During the preparation process, the micro connector is insensitized due to electrostatic discharge shock, which affects product reliability, and the integrity of the electrostatic tank is difficult to guarantee, resulting in low yield.
Graphite molds and pretreatment technology are used to limit the floating of the metal shell through step-shaped graphite pressing tables to ensure the flowability of the glass exhaust gas. Combined with sintering and post-treatment steps, the sealed glass is flush and bubble-free, and the electrostatic overflow phenomenon is reduced.
It improves the product dimensional accuracy and yield rate, reduces costs, is suitable for mass production, effectively suppresses the overflow of the electrostatic tank glass, and extends the service life of the mold.
Smart Images

Figure CN118970589A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of micro connectors, and in particular to a method for preparing a micro insensitive glass sealing connector. Background Art
[0002] Connectors often encounter static electricity during storage, transportation, testing, and use, which may cause the connector to experience multiple electrostatic discharge shocks. Multiple electrostatic discharge shocks may cause the connector to become insensitive to a certain degree, thus affecting the reliability of the product. Therefore, the "discharge" electrostatic design technology is generally used on connectors, and an electrostatic air discharge channel, namely, an electrostatic slot, is designed on the shell and the foot line. The integrity of the electrostatic slot has a direct impact on the use of the connector, so the quality of the electrostatic slot must be guaranteed during the preparation process.
[0003] In the actual preparation process of micro connectors, due to the small size of the product, the low rigidity of the foot line, and the electrostatic groove of only 0.2mm, the assembly process is difficult, and the electrostatic groove is easily filled with glass during the sealing process, resulting in a low yield. Summary of the invention
[0004] In view of the deficiencies in the prior art, the purpose of the present invention is to provide a method for preparing a miniature insensitive glass sealed connector, which has high product dimensional accuracy, high yield rate, and low cost, and meets the requirements of enterprise mass production.
[0005] The technical solution adopted by the present invention to solve the technical problem is: a method for preparing a miniature insensitive glass sealing connector, the connector comprising a metal shell, a sealing glass, and a metal foot line; the sealing glass is arranged in the metal shell, the upper surface of the sealing glass is flush with the upper surface of the metal shell, and the lower surface of the sealing glass is flush with the lower bottom surface inside the metal shell; the metal foot line passes through the sealing glass, and the upper end of the metal foot line is flush with the upper end surface of the sealing glass and the metal shell;
[0006] The preparation method of the connector is as follows: assembling the pre-treated metal shell, sealing glass and metal foot line in a graphite mold; sintering the assembled sintered parts, taking out and disassembling the mold after sintering to obtain a semi-finished product; post-processing the obtained semi-finished product to obtain a finished connector.
[0007] Furthermore, the graphite mold includes a graphite lower mold and a graphite press plate; each component of the connector is embedded in the graphite lower mold, and the graphite press plate is pressed on top of each component of the connector.
[0008] Furthermore, the middle part of the graphite lower mold is provided with a first lower mold boss, a second lower mold boss and a foot line hole in sequence from the outside to the inside; the first lower mold boss is higher than the second lower mold boss; a lower mold groove is formed between the first lower mold boss and the second lower mold boss, and the lower mold groove is embedded with the metal shell; the metal foot line is inserted into the foot line hole.
[0009] Furthermore, the second lower die boss is embedded between the metal shell and the metal foot line; the upper surface of the second lower die boss is flush with the inner bottom surface of the metal shell.
[0010] Furthermore, a press platform groove is provided below the graphite press platform, and a press platform through hole is provided in the middle of the press platform groove; the aperture of the press platform through hole is equivalent to the inner diameter of the upper end surface of the metal shell, and the graphite press platform fixes the upper end of the metal shell.
[0011] Furthermore, the pretreatment is specifically as follows: degreasing and cleaning the metal shell and metal foot line, ultrasonic cleaning with a cleaning agent for 10 to 30 minutes, and then pre-oxidation treatment for 1 to 2 hours at 700 to 800° C. in a wet nitrogen atmosphere.
[0012] Furthermore, the sintering is carried out in a chain furnace, the sintering temperature is 900-960° C., the belt speed is 30-70 mm / min, and the atmosphere is nitrogen.
[0013] Furthermore, the post-processing is specifically as follows: grinding the upper end surface of the semi-finished product until the upper end surfaces of the metal shell, the metal foot line and the sealing glass are overall flush; pickling the connector to remove the oxide layer on the surface of the metal shell and the metal foot line, and then drying; finally, gold plating the surface of the exposed metal shell and metal foot line.
[0014] Furthermore, the metal shell and the metal baseboard are both made of Kovar alloy; and the sealing glass is iron sealing glass.
[0015] The beneficial effects of the present invention are as follows: compared with the prior art, in a preparation method for a miniature insensitive glass sealing connector provided by the present invention, a stepped graphite press plate with a through hole is selected to limit the floating phenomenon of a metal shell that is too light during the sintering process, thereby effectively suppressing the overflow of glass from the electrostatic trough; the exhaust flowability during the glass sintering process is ensured, and the glass has no obvious bubble defects after sintering; during the preparation method, the sealing glass is not subjected to the vertical pressure of the graphite press plate, and the sealing glass will not be filled to the position of the second lower mold boss of the graphite lower mold. During the sampling process after sintering, it is easy to demold and the graphite lower mold boss is not easily damaged, thereby effectively improving the service life of the mold and reducing the cost; according to a preparation method for a miniature insensitive glass sealing connector provided by the present invention, the product has high dimensional accuracy, high yield, and low cost, which meets the requirements of mass production of enterprises. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The components and assembly diagram of the micro connector provided by the present invention.
[0017] Figure 2 It is a schematic diagram of the assembly between the micro connector and the graphite mold in the present invention.
[0018] Among them, 1-metal shell; 2-sealing glass; 3-metal foot line; 4-connector; 5-graphite press plate; 6-graphite lower mold; 7-first lower mold boss; 8-second lower mold boss; 9-foot line hole; 10-lower mold groove; 11-press plate groove; 12-press plate through hole. DETAILED DESCRIPTION
[0019] The present invention is further described below by specific examples, but these examples are only used to illustrate the present invention and are not used to limit the scope of the present invention.
[0020] Example
[0021] like Figures 1-2 As shown, a method for preparing a micro passive glass sealing connector, the connector comprises a metal shell 1, a sealing glass 2, and a metal foot line 3; the sealing glass 2 is arranged in the metal shell 1, the upper surface of the sealing glass 2 is flush with the upper surface of the metal shell 1, and the lower surface of the sealing glass 2 is flush with the lower bottom surface inside the metal shell 1; the metal foot line 3 passes through the sealing glass 2, and the upper end of the metal foot line 2 is flush with the upper end surfaces of the sealing glass 2 and the metal shell 1;
[0022] The preparation method of the connector is as follows: assembling the pre-treated metal shell 1, the sealing glass 2, and the metal foot line 3 in a graphite mold; sintering the assembled parts to be sintered, and after the sintering is completed, taking out and disassembling the mold to obtain a semi-finished product; post-processing the obtained semi-finished product to obtain a finished connector.
[0023] The graphite mold includes a graphite lower mold 6 and a graphite press 5; each component of the connector is embedded in the graphite lower mold 6, and the graphite press 5 is pressed on top of each component of the connector. The middle part of the graphite lower mold 6 is provided with a first lower mold boss 7, a second lower mold boss 8 and a foot line hole 9 from outside to inside; the first lower mold boss 7 is higher than the second lower mold boss 8; a lower mold groove 10 is formed between the first lower mold boss 7 and the second lower mold boss 8, and the lower mold groove 10 is embedded with the metal shell 1; the metal foot line 2 is inserted into the foot line hole 9. The second lower mold boss 8 is embedded between the metal shell 1 and the metal foot line 2; the upper surface of the second lower mold boss 8 is flush with the inner bottom surface of the metal shell 1.
[0024] Among them, a press groove 11 is provided below the graphite press 5, and a press through hole 12 is provided in the middle of the press groove 11; the aperture of the press through hole 12 is equivalent to the inner diameter of the upper end surface of the metal shell 1, and the graphite press 5 fixes the upper end of the metal shell 1.
[0025] The pretreatment specifically includes: degreasing and cleaning the metal shell 1 and the metal foot line 3, ultrasonic cleaning with a cleaning agent for 10 to 30 minutes, and then pre-oxidation treatment for 1 to 2 hours at 700 to 800° C. in a wet nitrogen atmosphere.
[0026] The sintering is carried out in a chain furnace, the sintering temperature is 900-960° C., the belt speed is 30-70 mm / min, and the atmosphere is nitrogen.
[0027] Among them, the post-processing is specifically as follows: grinding the upper end surface of the obtained semi-finished product until the upper end surfaces of the metal shell 1, the metal foot line 3, and the sealing glass 2 are overall flush; pickling the obtained connector 4 to remove the oxide layer on the surface of the metal shell 1 and the metal foot line 3, and then drying; finally, gold plating is performed on the exposed surface of the metal shell 1 and the metal foot line 3.
[0028] The metal shell 1 and the metal foot line 3 are made of Kovar alloy; the sealing glass 2 is iron sealing glass. In this embodiment, the metal shell 1 has a wall thickness of 0.2 mm, an outer diameter of 2.0 mm, and a height of 0.8 mm; the metal foot line 3 has a diameter of 0.3 mm and a length of 35 mm; the sealing glass 2 has a diameter of 1.6 mm and a height of 2.0 to 2.3 mm.
[0029] As a preferred embodiment, the preparation method of the connector is specifically as follows: first, the metal shell 1 and the metal foot line 3 are degreased and cleaned, and a cleaning agent is selected to perform ultrasonic cleaning for 20 minutes, and then a pre-oxidation treatment is performed at 750°C in a wet nitrogen atmosphere for 1.5 hours; the oxidized metal shell 1 and the metal foot line 3 are assembled with the sealing glass 2 in a graphite mold, and the lower mold groove 10 in the middle of the graphite lower mold 6 is embedded with the metal shell 1, and the second lower mold boss 8 in the middle of the graphite lower mold 6 is embedded with the groove between the metal shell 1 and the metal foot line 3; the upper surface of the second lower mold boss 8 is flush with the inner bottom surface of the metal shell 1; the pressing platform groove 11 below the graphite pressing platform 5 is respectively embedded with the sealing glass 2 and the metal shell 1; the metal foot line 3 passes through the sealing glass 2 and the foot line hole 9 on the graphite lower mold 6, and the graphite pressing platform 5 fixes the upper end of the metal shell 1 to obtain an assembled part to be sintered.
[0030] Then put the assembled parts to be sintered into a chain atmosphere furnace for sintering, with a sintering temperature of 900-960°C, a belt speed of 30-70 mm / min, and a nitrogen atmosphere. After sintering, take out and disassemble the mold to obtain a semi-finished product. Grind the upper end surface of the metal shell 1 of the semi-finished connector until the upper end surfaces of the metal shell 1, the sealing glass 2, and the metal foot line 3 are flush as a whole. Then pickle the obtained connector 4 to remove the oxide layer on the surface of the metal shell 1 and the metal foot line 3, and then dry it. Finally, gold is plated on the exposed surface of the metal shell 1 and the metal foot line 3, and the coating thickness is 5μm.
[0031] The micro connector prepared in this embodiment is composed of a metal shell 1, a metal foot line 3, and a sealing glass 2. The diameter of the metal shell 1 is only 2 mm, and a very small air gap of about 0.2 mm is reserved between the metal foot line 3 and the metal shell 1, and the air gap between two metal foot lines 3 is about 0.2 mm.
[0032] The above implementation modes are only used to illustrate the present invention, but not to limit the present invention. Ordinary technicians in the relevant technical field can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, all equivalent technical solutions also belong to the scope of the present invention. The patent protection scope of the present invention should be defined by the claims.
Claims
1. A method for preparing a micro insensitive glass sealing connector, Features: The connector comprises a metal shell (1), a sealing glass (2), and a metal foot line (3); the sealing glass (2) is arranged in the metal shell (1), the upper surface of the sealing glass (2) is flush with the upper surface of the metal shell (1), and the lower surface of the sealing glass (2) is flush with the lower bottom surface inside the metal shell (1); the metal foot line (3) passes through the sealing glass (2), and the upper end of the metal foot line (2) is flush with the upper end surfaces of the sealing glass (2) and the metal shell (1); The preparation method of the connector comprises: assembling the pre-treated metal shell (1), the sealing glass (2), and the metal foot line (3) in a graphite mold; Then the assembled parts to be sintered are sintered. After the sintering is completed, the mold is taken out and disassembled to obtain a semi-finished product; the obtained semi-finished product is post-processed to obtain a finished connector.
2. A method for preparing a micro passive glass sealed connector as claimed in claim 1, Features: The graphite mold comprises a graphite lower mold (6) and a graphite pressing platform (5); each component of the connector is embedded in the graphite lower mold (6), and the graphite pressing platform (5) is pressed on top of each component of the connector.
3. A method for preparing a micro passive glass sealed connector as claimed in claim 2, Features: The middle part of the graphite lower die (6) is provided with a first lower die boss (7), a second lower die boss (8) and a foot line hole (9) in sequence from the outside to the inside; the first lower die boss (7) is higher than the second lower die boss (8); a lower die groove (10) is formed between the first lower die boss (7) and the second lower die boss (8), and the lower die groove (10) is embedded in the metal shell (1); the metal foot line (2) is inserted into the foot line hole (9).
4. A method for preparing a micro passive glass sealed connector as claimed in claim 3, Features: The second lower die boss (8) is embedded between the metal shell (1) and the metal foot line (2); the upper surface of the second lower die boss (8) is flush with the inner bottom surface of the metal shell (1).
5. A method for preparing a micro passive glass sealed connector as claimed in claim 2, Features: A press platform groove (11) is provided below the graphite press platform (5), and a press platform through hole (12) is provided in the middle of the press platform groove (11); the aperture of the press platform through hole (12) is equivalent to the inner diameter of the upper end surface of the metal shell (1), and the graphite press platform (5) fixes the upper end of the metal shell (1).
6. A method for preparing a micro passive glass sealed connector as claimed in claim 1, It is characterized in that The pretreatment specifically comprises: degreasing and cleaning the metal shell (1) and the metal foot line (3), ultrasonic cleaning with a selected cleaning agent for 10 to 30 minutes, and then pre-oxidation treatment for 1 to 2 hours at 700 to 800° C. in a wet nitrogen atmosphere.
7. A method for preparing a micro passive glass sealed connector as claimed in claim 1, Features: The sintering is carried out in a chain furnace, the sintering temperature is 900-960° C., the belt speed is 30-70 mm / min, and the atmosphere is nitrogen.
8. A method for preparing a micro passive glass sealed connector as claimed in claim 1, It is characterized in that The post-processing specifically comprises: grinding the upper end surface of the semi-finished product until the upper end surfaces of the metal shell (1), the metal leg line (3) and the sealing glass (2) are flush as a whole; pickling the connector (4) to remove the oxide layer on the surface of the metal shell (1) and the metal leg line (3), and then drying; and finally gold plating the exposed surfaces of the metal shell (1) and the metal leg line (3).
9. A method for preparing a micro passive glass sealed connector as claimed in claim 1, Features: The metal shell (1) and the metal foot line (3) are both made of Kovar alloy; the sealing glass (2) is iron sealing glass.