Electron transport composite material, electron transport layer and preparation method thereof
By using the composite material of TiO2 and SnO2 nanocrystals as the electron transport layer in perovskite solar cells and adjusting its molar ratio, the problem of insufficient performance of the electron transport layer is solved, and the battery performance of perovskite solar cells is significantly improved.
Patent Information
- Application Number
- CN202411044436.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-31
- Publication Date
- 2024-11-15
AI Technical Summary
The electron transport layer in perovskite solar cells has low electron mobility and strong photocatalytic activity, which limits the improvement of cell performance.
The composite material of TiO2 nanocrystal and SnO2 nanocrystals is used as the electron transport layer. By adjusting its molar ratio to 4: (0.75~2.25), a smooth surface is formed, interface defects are reduced, DC conductivity is improved, and the rapid extraction of electrons is promoted. transmission.
The short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells are improved, and the non-radiative recombination of charge carriers and interface defects are reduced.
Smart Images

Figure BDA0004973120790000111 
Figure BDA0004973120790000121 
Figure HDA0004973120800000011
Abstract
Description
Technical Field
[0001] The present application relates to the field of solar cell technology, and in particular, to an electron transport composite material, an electron transport layer and a preparation method thereof, and more particularly, to a perovskite solar cell and an electrical device. Background Art
[0002] Organic-inorganic halide perovskite solar cells (PSCs) are a promising type of solar cell due to their excellent optoelectronic properties and potential low-cost manufacturing characteristics. Currently, perovskite solar cells have attracted increasing attention due to their advantages such as simple structure and low-temperature preparation process. However, the electron transport layer in perovskite solar cells usually has the problems of low electron mobility and strong photocatalytic activity, which is not conducive to the realization of efficient and stable perovskite solar cells.
[0003] Therefore, it is urgent to prepare new electron transport layers to improve the performance of perovskite solar cells. Summary of the invention
[0004] In the first aspect of the present application, the present application proposes an electron transport composite material. According to an embodiment of the present application, the electron transport composite material comprises: titanium dioxide (TiO2) nanocrystals and tin dioxide (SnO2) nanocrystals, and the molar ratio of the TiO2 nanocrystals to the SnO2 nanocrystals is 4:(0.75-2.25). The electron transport composite material of the present application combines the advantages of both TiO2 nanocrystals and SnO2 nanocrystals, provides a smoother surface, helps the uniform deposition of the perovskite layer, reduces interface defects, and has a higher DC conductivity, which is conducive to the rapid extraction and transmission of electrons. Among them, a too high molar ratio of TiO2 nanocrystals to SnO2 nanocrystals will increase the resistance to electron transfer, interface defects and cause band bending or gap changes. A too low molar ratio of TiO2 nanocrystals to SnO2 nanocrystals will reduce the electron capture rate and increase the recombination loss. Therefore, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is moderate, and the electron transport composite material can better realize electron extraction and transmission, thereby improving the charge transfer efficiency, reducing the non-radiative recombination of charge carriers and reducing interface defects.
[0005] In the second aspect of the present application, the present application proposes an electron transport layer. According to an embodiment of the present application, the electron transport layer includes: the electron transport composite material described in the first aspect of the present application. The electron transport layer of the present application is a TiO2 and SnO2 bimolecular composite layer, which has a smooth surface, is conducive to the uniform deposition of the perovskite layer, reduces interface defects and has a high DC conductivity, which is conducive to the rapid extraction and transmission of electrons. Among them, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is too high, which will increase the resistance of electron transmission, interface defects and cause band bending or gap changes. The molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is too low, which will reduce the capture rate of electrons and increase the composite loss. Therefore, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is moderate, and the electron transport layer can better realize electron extraction and transmission, thereby improving the charge transfer efficiency, reducing the non-radiative recombination of charge carriers and reducing interface defects, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.
[0006] In some embodiments, the thickness of the electron transport layer is 20-30 nm.
[0007] In the third aspect of the present application, the present application proposes a method for preparing the electron transport composite material described in the first aspect of the present application. According to an embodiment of the present application, the method comprises: dispersing tin dioxide nanocrystals in a solvent to form a dispersion, adding a titanium source to the dispersion, and heating to obtain the electron transport composite material described in the first aspect of the present application. Thus, the method can prepare an electron transport composite material that can better achieve electron extraction and transmission, thereby improving charge transfer efficiency, reducing non-radiative recombination of charge carriers, and reducing interface defects.
[0008] In some embodiments, the solvent includes ethanol, the titanium source includes titanium tetrachloride, the heating temperature is 60 to 80° C., and the heating time is 20 to 40 minutes.
[0009] In the fourth aspect of the present application, the present application proposes a method for preparing the electron transport layer described in the second aspect of the present application. According to an embodiment of the present application, the electron transport composite material prepared by the method described in the third aspect of the present application is coated on a transparent conductive substrate to obtain the electron transport layer. Thus, the method can prepare an electron transport layer that can better achieve electron extraction and transmission, thereby improving charge transfer efficiency, reducing non-radiative recombination of charge carriers, and reducing interface defects.
[0010] In some embodiments, the spin coating speed of the coating process is 3000 rpm to 5000 rpm, and the coating process time is 20 to 40 seconds.
[0011] In some embodiments, after the coating process, the process further includes: annealing process.
[0012] In some embodiments, the annealing treatment is performed at a temperature of 140 to 160° C., and the annealing treatment time is 10 to 30 minutes.
[0013] In the fifth aspect of the present application, the present application proposes a perovskite solar cell. According to an embodiment of the present application, the perovskite solar cell comprises: the electron transport layer described in the second aspect of the present application. As a result, the perovskite solar cell has higher short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency.
[0014] In the sixth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device includes: the perovskite solar cell described in the fifth aspect of the present application.
[0015] Additional aspects and advantages of the present application will be given in part in the description below, and in part will become apparent from the description below, or will be learned through the practice of the present application. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:
[0017] Figure 1 The present invention is a flow chart of a method for preparing an electron transport composite material according to an embodiment of the present application.
[0018] Figure 2 Schematic diagram of the structure of a positive-type perovskite solar cell according to an embodiment of the present application.
[0019] Figure 3 Schematic diagram of the structure of an inversion perovskite solar cell according to an embodiment of the present application.
[0020] Figure 4 Schematic diagram of the structure of a positive-type perovskite solar cell according to an embodiment of the present application.
[0021] Figure 5 The diffraction patterns are obtained by transmission electron microscopy (TEM) and X-ray diffraction (XRD) tests according to the embodiments of the present application.
[0022] Description of reference numerals:
[0023] Positive-type perovskite solar cell 101; Inverted-type perovskite solar cell 102;
[0024] Hole transport layer 01; perovskite thin film layer 02; electron transport layer 03; electrode 04; transparent conductive substrate 05. DETAILED DESCRIPTION
[0025] The embodiments of the present application are described in detail below. Examples of the embodiments are shown in the drawings, but unnecessary detailed descriptions may be omitted. For example, detailed descriptions of well-known matters and repeated descriptions of actually identical structures may be omitted. This is to avoid the following description from becoming unnecessarily lengthy and to facilitate understanding by those skilled in the art. In addition, the drawings and the following description are provided for those skilled in the art to fully understand the present application and are not intended to limit the subject matter described in the claims.
[0026] Unless otherwise defined, all technical and scientific terms used in this application have the same meanings as those commonly understood by technicians in the technical field to which this application belongs; the terms used in this application are only for the purpose of describing specific embodiments and are not intended to limit this application; unless otherwise specified, the numerical values of the parameters mentioned in this application can be measured using various measurement methods commonly used in the art (for example, they can be tested according to the methods given in the embodiments of this application).
[0027] The terms "including" and "having" in the specification and claims of the present application and any modifications thereof are open expressions, that is, including the contents specified in the present application but not excluding other contents.
[0028] In the description of the present application, it should be understood that the terms "width", "thickness", etc. indicate orientation or positional relationships based on the orientation or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0029] In the description of this application, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. "First feature" and "second feature" may include one or more of the features.
[0030] In the description of the present application, it should be understood that the terms "center", "longitudinal", "lateral", "length", "width", "thickness", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", "clockwise", "counterclockwise", "axial", "radial", "circumferential" and the like indicate orientations or positional relationships based on the orientations or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore should not be understood as a limitation on the present application.
[0031] In the description of the present application, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may mean that the first and second features are in direct contact, or the first and second features are in indirect contact through an intermediate medium. Moreover, a first feature being “above”, “above”, and “above” a second feature may mean that the first feature is directly above or obliquely above the second feature, or simply means that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature may mean that the first feature is directly below or obliquely below the second feature, or simply means that the first feature is lower in level than the second feature.
[0032] In the description of the present application, “plurality” means two or more.
[0033] In the description of the present application, "A and / or B" may include the case of A alone, the case of B alone, or any of the cases of A and B, where A and B are only used for examples and may be any technical feature connected by "and / or" in the present application.
[0034] Unless otherwise specified, all embodiments and optional embodiments of the present application can be combined with each other to form a new technical solution.
[0035] Perovskite solar cells (PSCs) have developed rapidly due to their high efficiency and low cost. Planar structure PSCs have attracted attention due to their simple preparation process and low temperature requirements. However, the commonly used electron transport material titanium dioxide (TiO2) has problems such as low mobility and strong photocatalytic activity, which limits the improvement of cell performance.
[0036] To solve this problem, the present application proposes a new type of electron transport composite material, which includes: TiO2 nanocrystals and SnO2 nanocrystals, and the molar ratio of the TiO2 nanocrystals to the SnO2 nanocrystals is 4:(0.75-2.25). Based on the composite material, a composite electron transport layer hybridized with SnO2 nanocrystals and TiO2 nanocrystals is developed. The electron transport composite material of the present application and the composite electron transport layer prepared based on the electron transport composite material can effectively improve the performance of perovskite solar cells.
[0037] Based on this, in the first aspect of the present application, the present application proposes an electron transport composite material. According to an embodiment of the present application, the electron transport composite material includes: TiO2 nanocrystals and SnO2 nanocrystals, and the molar ratio of the TiO2 nanocrystals to the SnO2 nanocrystals is 4:(0.75-2.25). According to an embodiment of the present application, the composite material formed by the hybridization of SnO2 nanocrystals and TiO2 nanocrystals is a mixture of two different nano-sized particles. Each nanocrystal (SnO2 and TiO2) has its own specific crystal structure, but in the composite material, they are physically mixed. The electron transport composite material of the present application combines the advantages of TiO2 nanocrystals and SnO2 nanocrystals, provides a smoother surface, helps the uniform deposition of the perovskite layer, reduces interface defects and has a higher DC conductivity, improves the electron dynamics at the interface, and increases the extraction and transport speed of electrons from the perovskite layer to the electron transport layer, which is beneficial to the rapid extraction and transport of electrons; in addition, the electron transport composite material is beneficial to the perovskite film to show high crystallinity. Among them, a too high molar ratio of TiO2 nanocrystals to SnO2 nanocrystals will increase the resistance to electron transfer, interface defects and cause band bending or gap changes. A too low molar ratio of TiO2 nanocrystals to SnO2 nanocrystals will reduce the electron capture rate and increase the recombination loss. Therefore, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is moderate, and the electron transport composite material can better realize electron extraction and transmission, thereby improving the charge transfer efficiency, reducing the non-radiative recombination of charge carriers and reducing interface defects.
[0038] In the second aspect of the present application, the present application proposes an electron transport layer. According to an embodiment of the present application, the electron transport layer includes: the electron transport composite material described in the first aspect of the present application. According to an embodiment of the present application, the electron transport layer formed by hybridization of SnO2 nanocrystals and TiO2 nanocrystals is a mixture of two different nano-sized particles. Each nanocrystal (SnO2 and TiO2) itself has its own specific crystal structure, but in the electron transport layer, they are physically mixed. The electron transport layer of the present application is a bimolecular composite layer of TiO2 and SnO2, which has a smooth surface, contributes to the uniform deposition of the perovskite layer, reduces interface defects and has a higher DC conductivity, improves the electron dynamics at the interface, and increases the extraction and transport speed of electrons from the perovskite layer to the electron transport layer, which is beneficial to the rapid extraction and transport of electrons; in addition, the electron transport composite material is beneficial to the perovskite film to show high crystallinity. Among them, a too high molar ratio of TiO2 nanocrystals to SnO2 nanocrystals will increase the resistance to electron transmission, interface defects and cause band bending or gap changes. A too low molar ratio of TiO2 nanocrystals to SnO2 nanocrystals will reduce the electron capture rate and increase the recombination loss. Therefore, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is moderate, and the electron transport layer can better realize electron extraction and transmission, thereby improving the charge transfer efficiency, reducing the non-radiative recombination of charge carriers and reducing interface defects, thereby improving the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of perovskite solar cells.
[0039] In some embodiments, the thickness of the electron transport layer is 20-30 nm, for example, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm and range values between any two of them, such as 20-29 nm, 20-28 nm and 20-27 nm. Thus, the thickness of the electron transport layer is moderate, which can improve the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.
[0040] In a fourth aspect of the present application, the present application proposes a method for preparing the electron transport composite material described in the first aspect of the present application. According to an embodiment of the present application, Figure 1 As shown, the method includes:
[0041] S100: Dispersing tin dioxide (SnO2) nanocrystals in a solvent to form a dispersion.
[0042] S200: adding a titanium source to the dispersion and heating to obtain the electron transport composite material described in the first aspect of the present application. Thus, the method can prepare an electron transport composite material that can better achieve electron extraction and transmission, thereby improving charge transfer efficiency, reducing non-radiative recombination of charge carriers, and reducing interface defects.
[0043] In some embodiments, tin dioxide (SnO2) nanocrystals are prepared by a sol-gel method. For example, tin tetrachloride pentahydrate (SnCl4·5H2O) is dissolved in ethylene glycol and stirred and aged for 2 days, and acetic acid (HAc) and ammonia water are slowly added thereto while stirring. Then, heating and stirring are performed at 150°C for 30 minutes to obtain SnO2 nanocrystals. Among them, tin tetrachloride pentahydrate (SnCl4·5H2O) is dissolved in ethylene glycol (used as a solvent), which is a step to prepare the starting solution for the reaction; the solution is stirred and aged for 2 days, which helps to ensure uniform dispersion and dissolution of the precursor; acetic acid (HAc) and ammonia water are slowly added to the solution under continuous stirring. Acetic acid is used to adjust the pH value of the solution, while ammonia water, as a base, can promote the hydrolysis reaction of SnCl4 to generate SnO2. After adding HAc and ammonia water, SnCl4 is hydrolyzed under alkaline conditions to generate SnO2 nanocrystals. The chemical equation is as follows: SnCl4+2H2O+4OH - →SnO2+4H2O+4Cl - .
[0044] In some embodiments, the solvent includes ethanol, the titanium source includes titanium tetrachloride, the heating temperature is 60-80°C, and the heating time is 20-40 minutes. For example, first, the TiCl4 solution is slowly dripped onto the frozen deionized water ice cube, and the ice cube is completely melted after the dripping is completed. At this time, the prepared SnO2 nanocrystals are added to the suspension, and then heated at 70°C for 30 minutes to obtain a hybrid nanocrystalline solution of SnO2 and TiO2. Among them, titanium tetrachloride (TiCl4) is dissolved in an appropriate solvent, usually deionized water or other suitable solvents; frozen deionized water: deionized water is frozen into ice cubes, which helps to control the subsequent chemical reaction rate; dripping TiCl4: TiCl4 solution is slowly dripped onto the frozen deionized water ice cube, and as the ice cube melts, TiCl4 gradually reacts with water to generate a precursor of TiO2, in which a hydrolysis reaction occurs, and TiCl4 reacts with water to generate a TiO2 nanocrystalline suspension. The chemical equation is as follows: TiCl4+2H2O→TiO2+4HCl. The prepared SnO2 nanocrystals are added to the TiO2 nanocrystal suspension, and then heated at 70°C for 30 minutes to obtain a hybrid nanocrystal solution of SnO2 and TiO2.
[0045] In the fourth aspect of the present application, the present application proposes a method for preparing the electron transport layer described in the second aspect of the present application. According to an embodiment of the present application, the electron transport composite material prepared by the method described in the third aspect of the present application is coated on a transparent conductive substrate to obtain the electron transport layer. Thus, the method can prepare an electron transport layer that can better achieve electron extraction and transmission, thereby improving charge transfer efficiency, reducing non-radiative recombination of charge carriers, and reducing interface defects.
[0046] In some embodiments, the spin coating speed of the coating process is 3000 rpm to 5000 rpm, and the coating process time is 20 to 40 seconds.
[0047] In some embodiments, after the coating process, the process further includes: annealing process.
[0048] In some embodiments, the annealing treatment is performed at a temperature of 140 to 160° C., and the annealing treatment time is 10 to 30 minutes.
[0049] In a fifth aspect of the present application, the present application proposes a perovskite solar cell. According to an embodiment of the present application, the electron transport layer described in the second aspect of the present application. Thus, the perovskite solar cell has higher short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency.
[0050] According to an embodiment of the present application, the perovskite solar cell includes but is not limited to an inverted perovskite solar cell, a positive perovskite solar cell and a perovskite tandem solar cell.
[0051] According to the embodiments of the present application, reference Figure 2 and Figure 4 , the positive-type perovskite solar cell 101 comprises:
[0052] Electrode 04;
[0053] A hole transport layer 01, wherein the hole transport layer 01 is disposed on one side of the electrode 04;
[0054] A perovskite film layer 02, wherein the perovskite film layer 02 is disposed on a side of the hole transport layer 01 away from the electrode 04;
[0055] The electron transport layer 03 described in the second aspect of the present application is disposed on a side of the perovskite thin film layer 02 away from the hole transport layer 01;
[0056] A transparent conductive substrate 05 is disposed on a side of the electron transport layer 03 away from the perovskite thin film layer 02 .
[0057] According to the embodiments of the present application, reference Figure 3 , the inverted perovskite solar cell 102 comprises:
[0058] Transparent conductive substrate 05;
[0059] A hole transport layer 01, wherein the hole transport layer 01 is disposed on one side of the transparent conductive substrate 05;
[0060] A perovskite thin film layer 02, wherein the perovskite thin film layer 02 is disposed on a side of the hole transport layer 01 away from the transparent conductive substrate 05;
[0061] The electron transport layer 03 described in the second aspect of the present application is disposed on a side of the perovskite thin film layer 02 away from the hole transport layer 01;
[0062] The electrode 04 is disposed on a side of the electron transport layer 03 away from the perovskite thin film layer 02 .
[0063] In the embodiments of the present application, it is preferred that Figure 2 and Figure 4 The positive-type perovskite solar cell shown has higher short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency.
[0064] In some embodiments, the thickness of the electron transport layer is 20 to 30 nm, for example, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm, and ranges between any two of these values, such as 20-29 nm, 20-28 nm, and 20-27 nm. Thus, the thickness of the electron transport layer is moderate, which can further improve the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the perovskite solar cell.
[0065] In some embodiments, the thickness of the perovskite film layer is 500-600nm, for example, it can be 500nm, 510nm, 520nm, 530nm, 540nm, 550nm, 560nm, 570nm, 580nm, 590nm, 600nm and the range between any two of them, such as 500-590nm, 500-580nm and 500-570nm. Thus, the thickness of the perovskite film layer is moderate, which can further improve the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.
[0066] In some embodiments, the thickness of the hole transport layer is 15 to 30 nm, for example, 15 nm, 16 nm, 17 nm, 18 nm, 19 nm, 20 nm, 21 nm, 22 nm, 23 nm, 24 nm, 25 nm, 26 nm, 27 nm, 28 nm, 29 nm, 30 nm and ranges between any two of them, such as 16-30 nm, 17-30 nm and 18-30 nm. Thus, the thickness of the hole transport layer is moderate, which can further improve the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.
[0067] In some embodiments, the thickness of the electrode is 105-115 nm, for example, 105 nm, 106 nm, 107 nm, 108 nm, 109 nm, 110 nm, 111 nm, 112 nm, 113 nm, 114 nm, 115 nm and ranges between any two of them, such as 106-115 nm, 107-115 nm and 108-115 nm. Thus, the thickness of the electrode is moderate, which can further improve the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell.
[0068] In some embodiments, the perovskite thin film layer includes ABX3, wherein A includes but is not limited to methylamine cation (FA + ), methylammonium cation (MA + ), cesium cation (Cs + ), rubidium cation (Rb + ) and potassium cation (K + ) at least one of; B includes but is not limited to lead cations (Pb 2+ ), tin cation (Sn 2+ ) and copper cations (Cu 2+ ), zinc cation (Zn 2+ ), gallium cation (Ga 2+ ) and calcium cations (Ca 2+ ) at least one of; X includes but is not limited to fluoride anion (F - ), chloride anion (Cl - ), bromide anion (Br - ) and iodide anion (I - )
[0069] In some embodiments, and / or the material of the hole transport layer includes [2-(9H-carbazole-9-yl)ethyl]phosphonic acid, [2-(3,6-dimethoxy-9H-carbazole-9-yl)ethyl]phosphonic acid, [4-(3,6-dimethyl-9H-carbazole-9-yl)butyl]phosphonic acid (Me-4PACZ), benzoic acid, 4-[bis(2,4-dimethoxybiphenyl-4-yl)amino]-biphenyl-4-carboxylic acid, 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene), poly Ethylene terephthalate, poly(3-hexylthiophene) (P3HT), poly(3,4-ethylenedioxythiophene)-poly(styrenesulfonate) (PEDOT:PSS), spirobis(terthiophene)benzodithiophene (Spiro-TTB), tetrafluoro-7,7,8,8-tetracyanoquinolinium (F4-TCNQ), hexafluoro-7,7,8,8-tetracyanoquinodimethane (F6TCNNQ), 2,2'-(1,4-phenylene)bis-4-(2-ethylhexyloxy)phenyl-1-phenyloctanone (TAPC), nickel oxide (NiO x ), copper thiocyanate (CuSCN), copper aluminum oxide (CuAlO2), vanadium pentoxide (V2O5), cadmium sulfide (CdS), cadmium selenide (CdSe) and poly (9,9-di-n-decylfluorene) bromide (PFN-Br), and at least one of x is 0.5 to 1.5.
[0070] In some embodiments, the electrode includes at least one of copper (Cu), silver (Ag), and gold (Au).
[0071] In the sixth aspect of the present application, the present application proposes an electrical device. According to an embodiment of the present application, the electrical device includes: the perovskite solar cell described in the fifth aspect of the present application.
[0072] The scheme of the present application will be explained below in conjunction with the embodiments. It will be appreciated by those skilled in the art that the following embodiments are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the literature in this area or the product specification are carried out. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.
[0073] Embodiment 1:
[0074] This embodiment provides a method for preparing a high-efficiency perovskite solar cell based on a composite nanocrystalline electron transport layer, and the preparation steps are as follows:
[0075] S1. Preparation of SnO2 nanocrystalline solution:
[0076] First, tin tetrachloride pentahydrate (SnCl4·5H2O) was dissolved in ethylene glycol and stirred for aging for 2 days. Then, the solution was transferred to a round-bottom flask, and acetic acid (HAc) and ammonia water were slowly added to it while stirring. After stirring, the round-bottom flask was placed in an oil bath, and a condensation reflux device was installed and heated and stirred at 150°C for 30 minutes to obtain SnO2 nanocrystals. Then, ethanol was used for centrifugal washing and separation, and finally the centrifugal product was dispersed in ethanol to form a SnO2 nanocrystal dispersion solution with a concentration of 10 mg / mL.
[0077] S2. Preparation of hybrid nanocrystalline solution of SnO2 and TiO2:
[0078] First, the TiCl4 solution is slowly dripped onto the frozen deionized water ice cube. After the dripping is completed, the ice cube is completely melted. At this time, the prepared SnO2 nanocrystals are added to the suspension (the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is 4:1.5, corresponding to a volume fraction of SnO2 nanocrystals of 10%), and then heated at 70°C for 30 minutes to obtain a hybrid nanocrystal solution of SnO2 and TiO2.
[0079] S3. Preparation of composite electron transport layer:
[0080] First, the prepared SnO2 and TiO2 hybrid nanocrystal solution was spin-coated on a transparent conductive substrate (the transparent conductive substrate was made of transparent conductive indium oxide (FTO)) at a speed of 4000 rpm for 30 seconds. After the spin coating, it was transferred to a hot stage for annealing at 150°C for 20 minutes, and the thickness of the composite electron transport layer was 25nm.
[0081] S4. Preparation of perovskite thin film layer:
[0082] After filtering the prepared 1.5M FAPbI3-based perovskite solution, the perovskite solution was statically spin-coated on FTO coated with tin dioxide (SnO2) at a speed of 5000 rpm. After spinning for 30 seconds, VCD treatment was performed for 15 seconds and then moved to a hot stage for annealing at 150°C for 30 minutes. The thickness of the perovskite film layer was 550nm.
[0083] S5. Preparation of hole transport layer:
[0084] After filtering the prepared 2,2',7,7'-tetrakis[N,N-di(4-methoxyphenyl)amino]-9,9'-spirobifluorene) (Spiro-OMeTAD) solution, the perovskite solution was dynamically spin-coated on the perovskite-coated FTO at a speed of 5000 rpm for 30 seconds, and the thickness of the hole transport layer was 30 nm.
[0085] S6. Preparation of electrodes:
[0086] On the surface of the hole transport layer, a copper electrode (thickness of about 110 nm) was deposited using a thermal evaporation evaporator. The vacuum degree of the thermal evaporation chamber was 10 -5 Pa, and the metal evaporation rate was 5 nm / min.
[0087] Embodiment 2:
[0088] The present embodiment provides a method for preparing a high-efficiency perovskite solar cell based on a composite nanocrystal electron transport layer. The preparation steps are the same as those in Example 1, except that the volume fraction of SnO2 nanocrystals in the hybrid nanocrystal solution of SnO2 and TiO2 is 5%, and the molar ratio of the corresponding TiO2 nanocrystals to SnO2 nanocrystals in the prepared hybrid nanocrystal solution is 4:0.75.
[0089] Embodiment 3:
[0090] The present embodiment provides a method for preparing a high-efficiency perovskite solar cell based on a composite nanocrystal electron transport layer. The preparation steps are the same as those in Example 1, except that the volume fraction of SnO2 nanocrystals in the hybrid nanocrystals of SnO2 and TiO2 prepared in S2 is 14.5%, and the molar ratio of the corresponding TiO2 nanocrystals to SnO2 nanocrystals in the prepared hybrid nanocrystal solution is 4:2.25.
[0091] Embodiment 4:
[0092] The experimental process of this embodiment is basically the same as that of Embodiment 1. The functional layers of the perovskite battery provided in this embodiment are basically the same as the functional layers of the perovskite battery in Embodiment 1. The main difference is that the concentration of SnO2 nanocrystals used in this embodiment is 5 mg / mL.
[0093] Embodiment 5:
[0094] The experimental process of this embodiment is basically the same as that of Embodiment 1. The functional layers of the perovskite battery provided in this embodiment are basically the same as the functional layers of the perovskite battery in Embodiment 1. The main difference is that the concentration of SnO2 nanocrystals used in this embodiment is 15 mg / mL.
[0095] Embodiment 6:
[0096] The preparation steps of this embodiment are basically the same as the experimental process of Example 1, except that tin tetrachloride pentahydrate (SnCl4·5H2O) is dissolved in ethanol and stirred for aging for 2 days. The other steps are the same as Example 1.
[0097] Embodiment 7:
[0098] The preparation steps of this embodiment are basically the same as the experimental process of embodiment 1, except that tin tetrachloride pentahydrate (SnCl4·5H2O) is dissolved in propanol and stirred for aging for 2 days. The other steps are the same as embodiment 1.
[0099] Comparative Example 1:
[0100] The preparation steps of this comparative example are basically the same as the experimental process of Example 1, except that in step S2, the TiCl4 solution is not dripped into the SnO2 nanocrystals, and the prepared electron transport layer is only composed of SnO2 nanocrystals as the electron transport material. The other steps are the same as Example 1.
[0101] Comparative Example 2:
[0102] The preparation steps of this comparative example are basically the same as the experimental process of Example 1, except that, SnO2 nanocrystals are not prepared, and TiCl4 solution is only slowly dripped onto the frozen deionized water ice cube. After the dripping is completed, the ice cube is completely melted, and then TiO2 nanocrystals are obtained after heating at 70°C for 30 minutes. The prepared electron transport layer is only composed of TiO2 nanocrystals, an electron transport material, and the other steps are the same as Example 1.
[0103] Comparative Example 3:
[0104] The preparation steps of this comparative example are basically the same as the experimental process of Example 1, except that:
[0105] (1) Preparation of TiO2 dense layer (c-TiO2 layer):
[0106] The cleaned conductive substrate (FTO) was placed in a coater, and a certain amount of dense layer precursor solution was taken with a pipette and dropped on the substrate. A 20-25 nm thick TiO2 thin layer was formed by spin coating dilution (spin coating at 500 rpm for 5 s and 2000 rpm for 30 s, respectively) with 0.15 μm diisopropoxy diacetylacetonate titanium (acetylacetonate) in n-butanol, followed by heat treatment on a hot plate at 135°C for 10 min and annealing at 500°C in air for 30 min.
[0107] (2) Preparation of TiO2 mesoporous layer (m-TiO2 layer): The mesoporous layer slurry was spin-coated on the prepared thin film sample by a spin coating process. In the case of a mesoporous structure, a 200 nm thick mesoporous TiO2 layer was further deposited on the dense TiO2 layer by spin coating a commercially available TiO2 slurry (Dyesol 18NR-T). The TiO2 slurry was diluted in anhydrous ethanol at a weight ratio of 1:10 at a rotation speed of 4000 rpm for 30 s and then sintered in air at 500 °C for 30 min. The obtained FTO / c-TiO2 layer / m-TiO2 substrate was further subjected to UV-ozone treatment for 20 min.
[0108] (3) Preparation of SnO2 nanoparticles (NP-SnO2): 0.5 mL of SnO2 colloidal dispersion (15 wt%) was diluted in 3-5 mL of ultrapure water, and then spin-coated on a FTO / c-TiO2 / m-TiO2 substrate at 3000 rpm for 30 s, and then annealed at 150°C for 30 min. FTO / c-TiO2 / m-TiO2+NP-SnO2 was formed, and subjected to UV-ozone treatment for 20 min; the other steps were the same as in Example 1.
[0109] The electron transport layer prepared in this comparative example is prepared by first spin-coating a TiO2 layer, then spin-coating a TiO2 mesoporous layer, and finally spin-coating a SnO2 layer to prepare a double-layer stack of SnO2 and TiO2.
[0110] Comparative Example 4:
[0111] The preparation steps of this comparative example are basically the same as the experimental process of Example 1, except that, in S2, in the preparation of the hybrid nanocrystal solution of SnO2 and TiO2, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is 4:0.5, corresponding to a volume fraction of SnO2 nanocrystals of 3.6%, and the other steps are the same as Example 1.
[0112] Comparative Example 5:
[0113] The preparation steps of this comparative example are basically the same as the experimental process of Example 1, except that in the hybrid nanocrystalline solution of SnO2 and TiO2 prepared in step S2, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is 4:2.5, corresponding to a volume fraction of SnO2 nanocrystals of 15.9%, and the other steps are the same as Example 1.
[0114] Test Example 1:
[0115] The performance of the perovskite solar cells prepared in Examples 1 to 7 was compared with that of the perovskite solar cells in Comparative Examples 1 to 5, and their parameters are shown in Table 1.
[0116] Table 1
[0117]
[0118]
[0119] Compared with Examples 1 to 7 and Comparative Examples 1 to 3, the perovskite solar cell with the electron transport layer of the present application has higher short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency, which indicates that the composite electron transport layer hybridized with TiO2 nanocrystals and SnO2 nanocrystals is beneficial to improving the performance of perovskite solar cells.
[0120] Compared with Comparative Examples 4 to 5, in Example 1, the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is 4:(0.75 to 2.25), corresponding to a volume fraction of SnO2 nanocrystals of 5% to 14.5%, and the short-circuit current, open-circuit voltage, filling factor and photoelectric conversion efficiency of the perovskite solar cell are higher. When the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is higher than 4:0.75 or the molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is lower than 4:2.25, the short-circuit current, open-circuit voltage, filling factor and photoelectric conversion efficiency of the perovskite solar cell are lower. This indicates that a moderate molar ratio of TiO2 nanocrystals to SnO2 nanocrystals is more conducive to improving the performance of perovskite solar cells.
[0121] Compared with Example 1 and Examples 4 to 5, when the concentration of SnO2 nanocrystals is about 8 to 12 mg / mL, the short-circuit current, open-circuit voltage, fill factor, and photoelectric conversion efficiency of the perovskite solar cell are higher, which indicates that a moderate concentration of SnO2 nanocrystals is beneficial to improving the performance of the perovskite solar cell.
[0122] Compared with Example 1 and Examples 6 to 7, the short-circuit current, open-circuit voltage, fill factor and photoelectric conversion efficiency of the perovskite solar cell prepared with SnO2 nanocrystals dissolved in ethylene glycol are improved compared with the perovskite solar cells prepared with SnO2 nanocrystals dissolved in ethanol and propanol, respectively, indicating that SnO2 nanocrystals prepared with SnO2 nanocrystals dissolved in ethylene glycol as electron transport layers are more beneficial to improving the performance of perovskite solar cells.
[0123] Test Example 2:
[0124] The SnO2 nanocrystals prepared in Example 1 were subjected to TEM and XRD tests. Figure 5 As shown. Figure 5 The left picture shows a series of obviously broadened diffractions, indicating that they are diffractions of tetragonal rutile SnO2. Figure 5 The right figure shows a uniform SnO2 nanocrystal morphology with an average diameter of about 3 nm, which indicates that the method of the present application improves the crystallinity of SnO2 nanocrystals prepared.
[0125] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0126] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.
Claims
1. An electron transport composite material, characterized in that include: TiO2 nanocrystals and SnO2 nanocrystals, wherein the molar ratio of the TiO2 nanocrystals to the SnO2 nanocrystals is 4:(0.75-2.25).
2. An electron transport layer, characterized in that include: The electron transport composite material according to claim 1.
3. The electron transport layer according to claim 2, characterized in that The thickness of the electron transport layer is 20-30 nm.
4. A method for preparing the electron transport composite material according to claim 1, characterized in that: include: Tin dioxide nanocrystals are dispersed in a solvent to form a dispersion, a titanium source is added to the dispersion, and the dispersion is heated to obtain the electron transport composite material according to claim 1.
5. The method according to claim 4, characterized in that The solvent includes ethanol, the titanium source includes titanium tetrachloride, the heating temperature is 60 to 80° C., and the heating time is 20 to 40 minutes.
6. A method for preparing the electron transport layer according to claim 2 or 3, characterized in that: The electron transport composite material prepared by the method according to claim 4 or 5 is coated on a transparent conductive substrate to obtain the electron transport layer.
7. The method according to claim 6, characterized in that The spin coating speed of the coating process is 3000 rpm to 5000 rpm, and the coating time is 20 to 40 seconds; And / or, after the coating process, further comprising: annealing process.
8. The method according to claim 7, characterized in that The annealing treatment is performed at a temperature of 140 to 160° C., and the annealing treatment time is 10 to 30 minutes.
9. A perovskite solar cell, characterized in that: include: The electron transport layer according to claim 2 or 3.
10. An electrical device, characterized in that: include: The perovskite solar cell according to claim 9.