Heat-sensitive recording medium

The existing thermal recording bodies are solved by using inorganic pigments, hollow particles and specific binders in the thermosensitive recording bodies, combined with N,N'-diarylurea compounds and diphenylsulfone derivatives, at high temperatures, are The problem of fading in wet environments achieves higher water resistance, water plasticizer resistance and alcohol resistance, ensuring long-term clearness of the image.

CN118973826APending Publication Date: 2024-11-15OJI HLDG CORP
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202380031697.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-07
Filing Date
2023-04-06
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing thermally sensitive recording bodies fade in high temperature and high humidity environments and are sensitive to alcohol, and have insufficient water resistance, water-resistant plasticizer and alcohol resistance, which makes it difficult for images to maintain for a long time.

Method used

Using a thermosensitive recording body containing inorganic pigments, hollow particles and specific binders, N,N'-diarylurea compound and diphenylsulfone derivative are used as color developers in the thermosensitive recording layer, and optimized The composition of the primer layer and the thermal recording layer improves the color development density and image quality.

Benefits of technology

The water resistance, water plasticizer and alcohol resistance of the thermal recording body are significantly improved, ensuring that the image remains clear for a long time under different environmental conditions and the color development concentration is improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118973826A_ABST
    Figure CN118973826A_ABST
Patent Text Reader

Abstract

The present disclosure provides a heat-sensitive recording body including, in order on a support body, at least an undercoat layer containing an inorganic pigment, hollow particles, and a binder, and a heat-sensitive recording layer containing a leuco dye, a developer, and a binder, the heat-sensitive recording layer being characterized by containing, as the developer, a first developer and a second developer, and contains an N, N '-diarylurea compound represented by general formula (1). (In the formula, each R2 represents an alkyl group having 1-12 carbon atoms, an aralkyl group having 7-12 carbon atoms, or an aryl group having 6-12 carbon atoms; the aralkyl group and the aryl group may be substituted by an alkyl group having 1-12 carbon atoms, an alkoxy group having 1-12 carbon atoms, an aryl group having 6-12 carbon atoms, or a halogen atom; the plurality of R2 may be the same as or different from each other, each A1 represents a hydrogen atom or an alkyl group having 1-4 carbon atoms, and the plurality of A1 may be the same as or different from each other. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a thermosensitive recording material. Background Art

[0002] Thermosensitive recording media in widespread practical use record color images by utilizing a heating color development reaction between a colorless or light-colored leuco dye and a phenol or an organic acid. Such thermosensitive recording media have advantages in that, for example, a color image can be formed only by applying heat, and further, a recording device for these can be compact, can be easily maintained, and generates less noise. For this reason, thermosensitive recording media have been used in a wide range of technical fields as various information recording materials for various printing devices such as label printers, automatic ticket machines, CD / ATMs, order output devices used in restaurants, data output devices in scientific research equipment, and the like.

[0003] Because this type of color development reaction is a reversible reaction, it is known that color images fade over time. This fading reaction is accelerated in a high temperature and high humidity environment, and further rapidly progresses by contacting with oil, plasticizers, etc., and the color may fade to the extent that the recorded image becomes difficult to recognize. In recent years, disinfection and sterilization with alcohol have become a common practice in general life, especially for the prevention of infectious diseases. Therefore, the demand for improved performance of thermosensitive recording bodies such as the following is increasing day by day: even when they are in contact with alcohol, there is no color development in the blank paper portion, and there is no fading in the printing portion.

[0004] For example, Patent Document 1 proposes a thermosensitive recording material containing a diaryl urea derivative as a developer. However, the thermosensitive recording material described in Patent Document 1 is insufficient in water resistance, water plasticizer resistance, and alcohol resistance, and has room for improvement.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: WO2019 / 044462 Summary of the invention

[0008] Problem that the invention aims to solve

[0009] A main object of the present invention is to provide a thermosensitive recording medium having excellent water resistance and water-plasticizer resistance in a recorded area and excellent alcohol resistance in a recorded area and a background area.

[0010] Solutions for solving problems

[0011] The present inventors conducted intensive studies in view of the prior art and found a solution to the problem. More specifically, the present invention provides the following thermosensitive recording material.

[0012] Project 1.

[0013] A thermosensitive recording medium comprising at least an undercoat layer and a thermosensitive recording layer in this order on a support,

[0014] The base coating contains inorganic pigments, hollow particles and a binder.

[0015] The heat-sensitive recording layer contains a leuco dye, a developer and a binder.

[0016] The thermosensitive recording layer contains a first developer and a second developer as developers, and

[0017] The thermosensitive recording layer contains an N,N'-diaryl urea compound represented by formula (1) as a second developer:

[0018]

[0019] in

[0020] R2 means C 1-12 Alkyl, C 7-12 Arylalkyl or C 6-12 Aryl, aralkyl and aryl groups can be C 1-12 Alkyl, C 1-12 Alkoxy, C 6-12 An aryl group or a halogen atom is substituted, and multiple R2 may be the same or different; and

[0021] A1 represents a hydrogen atom or C 1-4 alkyl, and multiple A1 may be the same or different.

[0022] Project 2.

[0023] The thermosensitive recording material according to item 1, wherein the N,N'-diaryl urea compound represented by formula (1) is selected from N,N'-di-[3-(p-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(o-toluenesulfonyloxy)phenyl]urea, N,N'-di-[3-(benzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(mesitylenesulfonyloxy)phenyl]urea, N,N'-di-[3-(4-ethylbenzenesulfonyloxy)phenyl]urea, N,N'-di-[3-(2-naphthalenesulfonyloxy)phenyl]urea, N,N'-di-[3 -(p-methoxybenzenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(benzylsulfonyloxy)phenyl]urea, N,N'-bis-[3-(ethanesulfonyloxy)phenyl]urea, N,N'-bis-[3-(p-toluenesulfonyloxy)-4-methyl-phenyl]urea, N,N'-bis-[4-(p-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[4-(benzenesulfonyloxy)phenyl]urea, N,N'-bis-[4-(ethanesulfonyloxy)phenyl]urea and N,N'-bis-[2-(p-toluenesulfonyloxy)]phenylurea.

[0024] Project 3.

[0025] The thermosensitive recording material according to item 1, wherein the N,N'-diaryl urea compound represented by formula (1) is N,N'-di-[3-(p-toluenesulfonyl)oxy]phenyl urea.

[0026] Project 4.

[0027] The thermosensitive recording material according to any one of items 1 to 3, comprising a diphenyl sulfone derivative represented by formula (2) as the first developer:

[0028]

[0029] Wherein R3 and R4 are the same or different and each represents C 1-4 Alkyl, C 2-4 Alkenyl, C 1-4 Alkoxy, C 2-4 Alkenyloxy, C 7-12 an aralkyloxy group or a halogen atom;

[0030] m is an integer from 0 to 2;

[0031] n is an integer from 1 to 3; and

[0032] p and q are the same or different and each represents an integer of 0 to 2.

[0033] Item 5.

[0034] The thermosensitive recording material according to item 4, wherein the diphenyl sulfone derivative represented by formula (2) is at least one selected from the group consisting of 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(3-allyl-4-hydroxy)diphenyl sulfone, 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone, 4-allyloxy-4'-hydroxydiphenyl sulfone and 4-hydroxy-4'-benzyloxydiphenyl sulfone.

[0035] Item 6.

[0036] The thermosensitive recording material according to any one of items 1 to 3, wherein the first developer is N-p-toluenesulfonyl-N′-3-(p-toluenesulfonyloxy)phenylurea.

[0037] Item 7.

[0038] The thermosensitive recording material according to any one of items 1 to 3, wherein the first developer is N-[2-(3-phenylureido)phenyl]benzenesulfonamide.

[0039] Item 8.

[0040] The thermosensitive recording material according to any one of items 1 to 3, wherein the first developer is 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide.

[0041] Item 9.

[0042] The thermosensitive recording material according to any one of items 1 to 8, wherein the second color developer is contained in an amount of 0.1 to 3 parts by mass relative to 1 part by mass of the first color developer.

[0043] Item 10.

[0044] The thermosensitive recording material according to any one of items 1 to 8, wherein the second color developer is contained in an amount of 0.1 to 1 part by mass relative to 1 part by mass of the first color developer.

[0045] Item 11.

[0046] The thermosensitive recording material according to any one of items 1 to 10, wherein

[0047] The maximum particle size (D100) of the hollow particles is 10 to 30 μm and the average particle size (D50) is 4.0 to 15 μm, the ratio D100 / D50 of the maximum particle size (D100) to the average particle size (D50) is 1.8 to 3.0, and

[0048] The volume % of hollow particles having a particle size of 2.0 μm or less is 1% or less.

[0049] Item 12.

[0050] The thermosensitive recording material according to any one of items 1 to 11, wherein the hollow ratio of the hollow particles is 80% to 98%.

[0051] Item 13.

[0052] The thermosensitive recording material according to any one of items 1 to 12, wherein the binder in the undercoat layer comprises a binder resin having a glass transition temperature of -10°C or lower.

[0053] Item 14.

[0054] The thermosensitive recording material according to any one of items 1 to 13, wherein the binder in the undercoat layer comprises a binder resin having a glass transition temperature of -30°C or lower.

[0055] Item 15.

[0056] The thermosensitive recording material according to any one of items 1 to 14, which has an adhesive layer on at least one surface of the support.

[0057] Effects of the Invention

[0058] The thermosensitive recording medium of the present invention has excellent water resistance and water plasticizer resistance in the recorded area, and excellent alcohol resistance in the recorded area and background area. The thermosensitive recording medium can also improve the color density. DETAILED DESCRIPTION

[0059] In the present specification, the expression “includes” or “comprising” includes the following concepts: “comprising,” “consisting essentially of,” and “consisting of.

[0060] In the present specification, a numerical range represented by "to" means a range including the numerical values ​​described before and after "to" as a lower limit and an upper limit.

[0061] As used herein, "latex" includes latex in the form of a gel or a dry film formed by drying a dispersion medium.

[0062] The present invention relates to a thermosensitive recording medium, which comprises at least an undercoat layer and a thermosensitive recording layer in this order on a support.

[0063] The base coating contains inorganic pigments, hollow particles and a binder.

[0064] The heat-sensitive recording layer contains a leuco dye, a developer and a binder.

[0065] The thermosensitive recording layer contains a first developer and a second developer as developers, and

[0066] The thermosensitive recording layer contains an N,N'-diaryl urea compound represented by formula (1) as a second developer:

[0067]

[0068] in

[0069] R2 means C 1-12 Alkyl, C 7-12 Arylalkyl or C 6-12 Aryl, aralkyl and aryl groups can be C 1-12 Alkyl, C 1-12 Alkoxy, C 6-12 An aryl group or a halogen atom is substituted, and multiple R2 may be the same or different; and

[0070] A1 represents a hydrogen atom or C 1-4 alkyl, and multiple A1 may be the same or different.

[0071] Support

[0072] The support in the present invention is not particularly limited in type, shape or size. For example, high-quality paper (acid paper, neutral paper), medium-quality paper, coated paper, coated paper, cast-coated paper, glass paper, resin-laminated paper, polyolefin-based synthetic paper, synthetic fiber paper, non-woven fabric, synthetic resin film, or various transparent supports can be appropriately selected and used. The thickness of the support is not particularly limited, and is generally about 20 to 200 μm. The density of the support is not particularly limited, and is preferably about 0.60 to 0.85 g / cm 3 .

[0073] Base coating

[0074] The thermosensitive recording material of the present invention has an undercoat layer between the support and the thermosensitive recording layer, and the undercoat layer contains an inorganic pigment, hollow particles, and a binder.

[0075] Hollow particles

[0076] From the viewpoint of enhancing the buffering property, the hollow particles are preferably formed of an organic resin. The undercoat layer containing the hollow particles and thus having excellent heat-insulating properties can prevent the diffusion of heat applied to the thermosensitive recording layer and increase the sensitivity of the thermosensitive recording body.

[0077] Hollow particles formed of organic resins can be divided into foaming type and non-foaming type according to the production method. Of the two types, foaming type hollow particles generally have a larger average particle size and a higher hollow ratio than non-foaming type hollow particles. Therefore, foaming type hollow particles achieve better sensitivity and image quality than non-foaming type hollow particles.

[0078] Non-foamed hollow particles can be produced by polymerizing seeds in a solution, polymerizing other resins to coat the seeds, and removing the seeds inside by swelling and dissolving to form voids inside. The seeds inside are removed by swelling and dissolving using an alkaline aqueous solution or the like. Non-foamed hollow particles having a relatively large average particle size can also be produced by alkali swelling treatment of core-shell particles in which core particles having alkali swelling properties are coated with a shell layer having no alkali swelling properties.

[0079] Expandable hollow particles can be produced by preparing particles in which a volatile liquid is sealed in a resin, and causing the liquid in the particles to evaporate and expand while softening the resin by heating.

[0080] In the production process of the foamed hollow particles, the liquid inside the particles is expanded by heating, thereby increasing the hollow ratio and providing excellent heat insulation; therefore, the use of the foamed hollow particles can improve the sensitivity of the thermosensitive recording body and improve the recording concentration. The improvement in sensitivity is particularly important in the color development in the middle tone range where the heat energy applied to the thermosensitive recording layer is small. In addition, when the thermosensitive recording layer is formed via an undercoat layer having excellent heat insulation, the diffusion of heat applied to the thermosensitive recording layer is prevented, resulting in excellent image uniformity and improved image quality. Therefore, in this embodiment, it is preferred to use foamed hollow particles that are excellent in improving the heat insulation of the undercoat layer.

[0081] The example of the resin that can be used for foaming type hollow particles includes thermoplastic resin, such as styrene-acrylic resin, polystyrene resin, acrylic resin, polyethylene resin, polypropylene resin, polyacetal resin, chlorinated polyether resin, polyvinyl chloride resin, polyvinylidene chloride resin, acrylic resin (for example, acrylic resin containing acrylonitrile as a component), styrene resin, vinylidene chloride resin and copolymer resin mainly formed by polyvinylidene chloride and acrylonitrile. As the gas contained in the foaming type hollow particles, propane, butane, isobutane, air etc. can be used generally. Among various resins, from the viewpoint of the strength of keeping the shape of the foaming particles, acrylonitrile resin and copolymer resin mainly formed by polyvinylidene chloride and acrylonitrile are preferably used as the resin that can be used for hollow particles.

[0082] The maximum particle size of the hollow particles of the present invention is preferably 10 to 30 μm, and more preferably 15 to 25 μm. The maximum particle size is also referred to as "D100". When the maximum particle size of the hollow particles is 10 μm or more, the cushioning property of the undercoat layer is improved; therefore, the close fit between the thermosensitive recording body and the thermal head during printing is improved, and a thermosensitive recording body with high image quality is obtained. This high image quality can produce an improved recording concentration in the mid-tone range of coloring with less energy than that used to provide the maximum recording concentration (Dmax). When the maximum particle size of the hollow particles is 30 μm or less, the smoothness of the undercoat layer is improved; therefore, the thermosensitive recording layer provided via the undercoat layer can be made uniform, and a thermosensitive recording body in which the formation of white spots in the image is less likely to occur can be obtained.

[0083] The average particle size of the hollow particles of the present invention is preferably 4.0 to 15 μm, and more preferably 7.5 to 15 μm. The average particle size as used herein is the diameter at which the volume of the larger side particles is equal to the volume of the smaller side particles when the particles are divided into two types based on the particle size, i.e., the median diameter, which is the particle size corresponding to a frequency of 50% by volume. The average particle size is also referred to as "D50". When the average particle size of the hollow particles is 4.0 μm or more, the cushioning property of the undercoat layer is improved; therefore, the closeness of the thermosensitive recording body to the thermal head during printing is improved, and a thermosensitive recording body with high image quality is obtained. This high image quality can produce an improved recording concentration in the range of intermediate tones developed with less energy than that used to provide the maximum recording concentration (Dmax). When the average particle size of the hollow particles is 15 μm or less, the smoothness of the undercoat layer is improved; therefore, the thermosensitive recording layer provided by the undercoat layer can be made uniform, and a thermosensitive recording body in which the formation of white spots in the image is less likely to occur can be obtained.

[0084] The maximum particle size (D100) and average particle size (D50) of the hollow particles can be measured using a laser diffraction particle size distribution analyzer. The average particle size (D50) can be shown as the average value of the particle sizes of 10 particles, and the particle size is measured from an image (SEM image) of each particle using an electron microscope.

[0085] The ratio of the maximum particle size (D100) of the hollow particles to the average particle size (D50) of the hollow particles, i.e., D100 / D50, is an index indicating the degree of particle size distribution. The ratio of D100 / D50 is preferably 1.8 to 3.0, and more preferably 2.0 to 2.8. When the ratio of D100 / D50 of the hollow particles is 1.8 or more, the hollow particles can be fully foamed, the maximum particle size will be large enough, the hollow rate will be high, and the heat insulation of the base coating can be improved. When the ratio of D100 / D50 of the hollow particles is 3.0 or less, the size of the hollow particles is uniform, which improves the smoothness of the base coating and suppresses white spots in the image.

[0086] In the particle size distribution measured by a laser diffraction particle size distribution analyzer, the volume % of hollow particles with a particle size of 2.0 μm or less is preferably 1% or less. It is also preferred that the volume % of hollow particles with a particle size of 2.0 μm or less is 0.5% or less, and more preferably, hollow particles with a particle size of 2.0 μm or less are not included. Hollow particles with a particle size of 2 μm or less are considered to contribute very little to heat insulation because they are too small to have a sufficient hollow area. When the volume % of hollow particles with a particle size of 2 μm or less in the undercoat layer is 1% or less, recording concentration, image quality, etc. can be improved.

[0087] The hollow ratio of the hollow particles is preferably 80% to 98%, and more preferably 90% to 98%. When the hollow ratio of the hollow particles is 80% or more, excellent heat insulation can be imparted to the undercoat layer containing the hollow particles. When the hollow ratio of the hollow particles is 98% or less, the strength of the film around the hollow portion is improved, so that hollow particles that do not collapse even when the undercoat layer is formed can be obtained.

[0088] The hollow ratio of the hollow particles is determined by measuring the true specific gravity according to the IPA method and using the true specific gravity value as follows.

[0089] (1) Sample pretreatment

[0090] The samples were dried at 60°C for one day and one night.

[0091] (2) Reagents

[0092] Isopropyl alcohol (IPA: ultrapure reagent)

[0093] (3) Measurement method

[0094] -Weighing volumetric flask (W1).

[0095] - Weigh approximately 0.5 g of the dry sample (W2) in a volumetric flask.

[0096] - Add about 50 mg of IPA thereto, and shake the volumetric flask thoroughly to completely remove the air outside the capsules.

[0097] - Add IPA to the marked line and weigh the volumetric flask (W3).

[0098] - As a blank, add IPA only to the mark on the volumetric flask and weigh the volumetric flask (W4).

[0099] (4) Calculation of true specific gravity

[0100] True specific gravity = {(W2-W1)×((W4-W1) / 100)} / {(W4-W1)-(W3-W2)}

[0101] (5) Calculation of hollow ratio

[0102] Hollowness (%) = {1-1 / (1.1 / true specific gravity)}×100

[0103] The hollow ratio can also be calculated according to the following formula: 3 / D 3 )×100. In the formula, d represents the inner diameter of the hollow particle, and D represents the outer diameter of the hollow particle.

[0104] Since the hollow particles in the present invention have a relatively large particle size, the content of the hollow particles in the undercoat layer can be reduced. The content of the hollow particles is based on the total solid content of the undercoat layer, preferably 3 to 40% by mass, and more preferably 5 to 35% by mass. The hollow particle content of more than 3% by mass can improve the heat insulation of the undercoat layer, and the hollow particle content of less than 40% by mass makes it less likely to cause problems in terms of coating properties, and makes it possible to easily form a uniform undercoat layer and improve the recording concentration. In addition, the coating film strength of the undercoat layer can be improved.

[0105] Binder

[0106] Examples of binders include water-soluble polymer materials, such as polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, carboxymethylcellulose, methylcellulose and ethylcellulose, sodium polyacrylate, polyvinyl pyrrolidone, acrylamide-acrylate copolymer, acrylamide-acrylate-methacrylate copolymer, styrene-maleic anhydride copolymer, isobutylene-maleic anhydride copolymer, casein, gelatin and its derivatives; emulsions, such as polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylate, vinyl chloride-vinyl acetate copolymer, polybutyl methacrylate and ethylene-vinyl acetate copolymer; and latex of water-insoluble polymers such as styrene-butadiene copolymer and styrene-butadiene-acrylic acid copolymer; etc. Among them, it is preferred to use a binder containing latex. The content of the binder can be selected from a wide range, and based on the total solid content of the undercoat layer, it is generally preferably about 20% to 70% by mass, and more preferably about 25% to 60% by mass.

[0107] The binder preferably contains a binder resin having a glass transition temperature (Tg) of -10°C or less. When the glass transition temperature is -10°C or less, image quality can be improved even in a low energy range. The glass transition temperature is more preferably -30°C or less because image quality can be further improved in a low energy range. A glass transition temperature of -50°C or less is not preferred because sticking occurs. Therefore, the glass transition temperature is preferably -40°C or more.

[0108] Inorganic Pigments

[0109] The undercoat layer of the present invention contains an inorganic pigment. From the viewpoint of increasing the recording density and improving water-resistance and alcohol resistance, the oil absorption of the inorganic pigment is preferably 130 ml / 100 g or less, more preferably 125 ml / 100 g or less, and even more preferably 110 ml / 100 g or less. From the viewpoint of effectively reducing printing problems such as the occurrence of head residues and adhesion, the oil absorption of the inorganic pigment is also preferably 50 ml / 100 g or more, more preferably 80 ml / 100 g or more. The oil absorption is a value obtained by the method according to JIS K 5101.

[0110] Various inorganic pigments can be used as the inorganic pigment, and preferred examples include calcined kaolin and clay, etc. From the viewpoint of improving color development sensitivity, the content of the inorganic pigment is preferably 60% by mass or less, and more preferably 50% by mass or less based on the total solid content of the undercoat layer. From the viewpoint of effectively reducing printing problems such as the occurrence of head residue and adhesion, the content of the inorganic pigment is also preferably 20% by mass or more, and more preferably 25% by mass or more based on the total solid content of the undercoat layer.

[0111] For example, the primer coating material is prepared by mixing the hollow particles, the binder, the inorganic pigment, and the auxiliary agent as required using water as a medium, applying the coating material to the support, and then drying to form the primer coating material on the support. The amount of the primer coating material applied is not particularly limited, but is preferably about 2 to 20 g / m2 in terms of dry weight. 2 , more preferably about 2 to 12 g / m 2 .

[0112] Thermal recording layer

[0113] Leuco dye

[0114] The thermosensitive recording layer of the thermosensitive recording medium of the present invention may contain any of various known colorless or light-colored leuco dyes. Specific examples of such leuco dyes are described below.

[0115] Specific examples of the leuco dye include blue color-developing dyes such as 3,3-bis(p-dimethylaminophenyl)-6-dimethylaminophthalide, 3-(4-diethylamino-2-methylphenyl)-3-(4-dimethylaminophenyl)-6-dimethylaminophthalide and fluoran; green color-developing dyes such as 3-(N-ethyl-N-p-tolyl)amino-7-N-methylanilinofluoran, 3-diethylamino-7-anilinofluoran, 3-diethylamino-7-dibenzylaminofluoran and rhodamine B-anilinolactam; red color-developing dyes such as 3,6-bis(diethylamino)fluoran-γ-anilinolactam, 3-cyclohexylamino-6-chlorofluoran, 3-diethylamino-6-methyl-7-chlorofluoran, and 3-diethylamino-7-chlorofluoran;Black color-developing dyes, such as 3-(N-ethyl-N-isopentyl)amino-6-methyl-7-anilinofluoran, 3-(N-methyl-N-cyclohexyl)amino-6-methyl-7-anilinofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-di(n-butyl)amino-6-methyl-7-anilinofluoran, 3-di(n-pentyl)amino-6-methyl-7-anilinofluoran, 3-(N-ethyl-N-isopentylamino)-6-methyl-7-anilinofluoran, 3-diethylamino-7-(m-trifluoromethylanilino)fluoran, 3-(N-isopentyl-N-ethylamino)-7-(o-chloroanilino)fluoran, 3-(N-ethyl-N-2- Tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-(N-n-hexyl-N-ethylamino)-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-ethylamino]-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-methylamino]-6-methyl-7-anilinofluoran, 3-[N-(3-ethoxypropyl)-N-methylamino]-6-methyl-7-anilinofluoran, 3-diethylamino-7-(2-chloroanilino)fluoran, 3-di(n-butylamino)-7-(2-chloroanilino)fluoran, 4,4'-bis-dimethylaminobenzodihydroindane benzyl ether, N-2,4,5-trichlorophenylleucoaramine amine), 3-diethylamino-7-butylaminofluoran, 3-ethyl-tolylamino-6-methyl-7-anilinofluoran, 3-cyclohexyl-methylamino-6-methyl-7-anilinofluoran, 3-diethylamino-6-chloro-7-(β-ethoxyethyl)aminofluoran, 3-diethylamino-6-chloro-7-(γ-chloropropyl)aminofluoran, 3-diethylamino-6-methyl-7-anilinofluoran, 3-(N-isopentyl-N-ethylamino)-6-methyl-7-anilinofluoran, 3-dibutylamino-7-chloroanilinofluoran, 3-diethylamino-7-(o-chlorophenylamino)fluoran, 3-(N-ethyl-p-toluidinyl)-6-methyl-7-phenyl Aminofluran, 3-(N-ethyl-p-toluidinyl)-6-methyl-7-(p-toluidinyl)fluoran, 3-(N-ethyl-N-tetrahydrofurfurylamino)-6-methyl-7-anilinofluoran, 3-diethylamino-6-chloro-7-anilinofluoran, 3-dimethylamino-6-methyl-7-anilinofluoran, 3-pyrrolidinyl-6-methyl-7-anilinofluoran, 3-piperidinyl-6-methyl-7-anilinofluoran, 2,2-bis{4-[6'-(N-cyclohexyl-N-methylamino)-3'-methylspiro[phthalide-3,9'-xanthone-2'-ylamino]phenyl}propane and 3-diethylamino-7-(3'-trifluoromethylphenyl)aminofluoran;Dyes having absorption wavelengths in the near-infrared region, such as 3,3-bis[1-(4-methoxyphenyl)-1-(4-dimethylaminophenyl)ethylidene-2-yl]-4,5,6,7-tetrachlorophthalide, 3,3-bis[1-(4-methoxyphenyl)-1-(4-pyrrolidinylphenyl)ethylidene-2-yl]-4,5,6,7-tetrachlorophthalide, 3-p-(p-dimethylaminoanilino)anilino-6-methyl-7-chlorofluoran, 3-p-(p-chloroanilino)anilino-6-methyl-7-chlorofluoran, and 3,6-bis(dimethylamino)fluorene-9-spiro-3'-(6'-dimethylamino)phthalide; etc. Of course, the usable leuco dyes are not limited to these compounds, and two or more such compounds may be used in combination as required. ;

[0116] The content of the leuco dye is not particularly limited, and is preferably about 3 to 30% by mass, more preferably about 5 to 25% by mass, and even more preferably about 7 to 20% by mass based on the total solid content of the thermosensitive recording layer. A leuco dye content of 3% by mass or more can improve the color developing ability, thereby improving the recording density, while a leuco dye content of 30% by mass or less can improve heat resistance.

[0117] Color developer

[0118] In the present invention, a first developer and a second developer are included as developers, and an N,N′-diaryl urea compound represented by the above formula (1) is included as the second developer. The first developer is a main developer, and the second developer also has an effect of improving storage properties. Therefore, excellent water resistance, water plasticizer resistance, alcohol resistance, etc. can be exhibited.

[0119] Specific examples of the first color developer include phenolic compounds such as 4-tert-butylphenol, 4-acetylphenol, 4-tert-octylphenol, 4,4'-sec-butylidene diphenol, 4-phenylphenol, 4,4'-dihydroxydiphenylmethane, 4,4'-isopropylidene diphenol, 4,4'-cyclohexylidene biphenyl, 4,4'-cyclohexylidene diphenol, 1,1-bis(4-hydroxyphenyl)-ethane, 1,1-bis(4-hydroxyphenyl)-1-phenylethane, 4,4'-bis(p-toluenesulfonylaminocarbonylamino)diphenylmethane, 1,1-bis(4-hydroxyphenyl)cyclohexane, 2,2'-bis[4-(4-hydroxyphenyl)phenoxy]diethyl ether, 4,4'-dihydroxydiphenyl sulfide, 4,4'-thiobis( 3-methyl-6-tert-butylphenol), 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, 2,2-bis(4-hydroxyphenyl)-4-methylpentane, 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4-hydroxyphenyl(4'-n-propoxyphenyl) sulfone, 4-hydroxy-4'-benzyloxydiphenyl sulfone, 3,3'-diallyl-4,4'-dihydroxydiphenyl sulfone, bis(p-hydroxyphenyl)butyl acetate, bis(p-hydroxyphenyl)methyl acetate, hydroquinone monobenzyl ether, bis(3-allyl-4-hydroxyphenyl) sulfone, 4-hydroxy-4'-methyldiphenyl sulfone, 4-allyloxy-4'-hydroxydiphenyl sulfone, 3,4-dihydroxyphenyl-4'-methylphenyl sulfone, 4-hydroxydiphenyl ketones, dimethyl 4-hydroxyphthalate, methyl 4-hydroxybenzoate, propyl 4-hydroxybenzoate, sec-butyl 4-hydroxybenzoate, phenyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, benzyl 4-hydroxybenzoate, toluene 4-hydroxybenzoate, chlorophenyl 4-hydroxybenzoate and 4,4'-dihydroxydiphenyl ether; aromatic carboxylic acids such as benzoic acid, p-chlorobenzoic acid, p-tert-butylbenzoic acid, trichlorobenzoic acid, terephthalic acid, salicylic acid, 3-tert-butylsalicylic acid, 3-isopropylsalicylic acid, 3-benzylsalicylic acid, 3-(α-methylbenzyl)salicylic acid, 3,5-di-tert-butylsalicylic acid, 4-[2-(p-methoxyphenoxy)ethoxy]salicylic acid, 4-[3-(p-toluenesulfonyl)propoxy] Salicylic acid, 5-[p-(2-p-methoxyphenoxyethoxy]cumyl]salicylic acid, and zinc 4-[3-(p-toluenesulfonyl)propoxy]salicylate; salts of these phenolic compounds or aromatic carboxylic acids with polyvalent metals such as zinc, magnesium, aluminum, calcium, titanium, manganese, tin and nickel; antipyrine complexes of zinc thiocyanate; organic acidic substances such as complex zinc salts of terephthalic acid and other aromatic carboxylic acids; thiourea compounds such as N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenyl urea, N-p-toluenesulfonyl-N'-p-butoxycarbonylphenyl urea, N-p-toluenesulfonyl-N'-phenyl urea, 4,4'-bis(p-toluenesulfonylaminocarbonylamino)diphenylmethane and N,N'-di-m-chlorophenylthiourea;Organic compounds having a -SO2NH- bond in the molecule, such as N-(p-toluenesulfonyl)carbamic acid p-cumylphenyl ester, N-(p-toluenesulfonyl)carbamic acid p-benzyloxyphenyl ester, N-[2-(3-phenylureido)phenyl]benzenesulfonamide, N-(o-toluoyl)-p-toluenesulfonamide and 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide; inorganic acidic substances such as activated clay, attapulgite, colloidal silica and aluminum silicate; etc. The first developer is of course not limited to these, and the first developer used may be a combination of two or more compounds if necessary.;

[0120] It is preferred that the thermosensitive recording layer of the present invention contains the diphenyl sulfone derivative represented by the above formula (2) as the first developer. This can further improve the color development density.

[0121] In formula (2), C of R3 or R4 1-4 The alkyl group may be linear or branched, and examples include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, and tert-butyl. As used herein, the alkyl group also includes C 1-4 The alkyl portion of the alkoxy group. 2-4 The alkenyl group may be linear or branched, and examples include vinyl, n-propenyl, and n-butenyl. As used herein, the alkenyl group also includes C 2-4 Aralkyl refers to an arylalkyl group, C 7-12 Examples of aralkyl groups include benzyl, 1-phenylethyl, 2-phenylethyl and 3-phenylpropyl, etc. Examples of halogen atoms include fluorine, chlorine, bromine and iodine. If a plurality of R3 and / or R4 are present, they may be the same or different.

[0122] The substitution position of R3, R4 or OH is not particularly limited, and is preferably 3, 4 or 5. m is preferably 0 or 1, n is preferably 1, and p and q are preferably the same or different and are each 0 or 1.

[0123] The diphenyl sulfone derivative represented by formula (2) is not particularly limited, but is preferably at least one selected from the group consisting of 4-hydroxy-4′-isopropoxydiphenyl sulfone, 4,4′-dihydroxydiphenyl sulfone, 2,4′-dihydroxydiphenyl sulfone, bis(3-allyl-4-hydroxy)diphenyl sulfone, 4-hydroxyphenyl(4′-n-propoxyphenyl)sulfone, 4-allyloxy-4′-hydroxydiphenyl sulfone and 4-hydroxy-4′-benzyloxydiphenyl sulfone.

[0124] In the present invention, the first color developer is also preferably N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea. This provides an excellent balance between color development concentration and storage stability, and allows the effects of the present invention to be fully exerted.

[0125] In the present invention, the first color developer is also preferably N-[2-(3-phenylureido)phenyl]benzenesulfonamide. This provides an excellent balance between color development concentration and storage stability, and allows the effects of the present invention to be fully exerted.

[0126] In the present invention, the first color developer is also preferably 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide. This provides an excellent balance between color development concentration and preservability, and allows the effects of the present invention to be fully exerted.

[0127] In the formula (1) of the N,N'-diaryl urea compound included as the second color developer, the C of R2 1-12 The alkyl group may be linear, branched or alicyclic, preferably C 1-6 Alkyl, more preferably C 1-3 Alkyl. C 1-12 Examples of alkyl groups include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, tert-butyl, cyclopentyl, hexyl, cyclohexyl, 2-ethylhexyl, and lauryl. 1-12 The alkyl portion of an alkoxy group.

[0128] Aralkyl refers to arylalkyl, C 7-12 Examples of the aralkyl group include benzyl, 1-phenylethyl, 2-phenylethyl and 3-phenylpropyl.

[0129] Aryl means a monocyclic or polycyclic group formed by one or more 5-membered or 6-membered aromatic hydrocarbon rings. 6-12 Examples of aryl groups include phenyl, 1-naphthyl, and 2-naphthyl, etc. As used herein, aryl groups also include the aryl portion of aralkyl groups.

[0130] Examples of the halogen atom include fluorine, chlorine, bromine and iodine.

[0131] In formula (1), the substitution positions of each R2-SO3- may be the same or different. The substitution position is preferably 3, 4 or 5, more preferably 3. 7-12 Aralkyl and C 6-12 When the aryl group is substituted, the number of substituents is not particularly limited, and is, for example, 1 to 4.

[0132] C represented by A1 1-4 The alkyl group may be linear or branched. Examples include methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl and the like.

[0133] The substitution positions of each A1 may be the same or different. The substitution position is preferably the 3-position, 4-position or 5-position.

[0134] The N,N'-diaryl urea compound represented by formula (1) is not particularly limited, and is preferably selected from N,N'-bis-[3-(p-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(o-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(benzenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(mesitylenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(4-ethylbenzenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(2-naphthalenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(p-toluenesulfonyloxy)phenyl]urea, At least one selected from the group consisting of N,N'-bis-[3-(benzylsulfonyloxy)phenyl]urea, N,N'-bis-[3-(ethanesulfonyloxy)phenyl]urea, N,N'-bis-[3-(p-toluenesulfonyloxy)-4-methyl-phenyl]urea, N,N'-bis-[4-(p-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[4-(benzenesulfonyloxy)phenyl]urea, N,N'-bis-[4-(ethanesulfonyloxy)phenyl]urea and N,N'-bis-[2-(p-toluenesulfonyloxy)]phenylurea. Among them, N,N'-bis-[3-(p-toluenesulfonyloxy)phenyl]urea is preferred.

[0135] The content of the first developer is preferably about 0.2 to 3 parts by mass relative to 1 part by mass of the leuco dye. The content of the second developer is preferably about 0.1 to 3 parts by mass, more preferably about 0.1 to 1 part by mass relative to 1 part by mass of the first developer. When the content of the second developer is 0.1 parts by mass or more, the storage property can be improved. When the content of the second developer is 3 parts by mass or less, the color concentration can be improved.

[0136] The content of N, N'-diaryl urea compounds is not particularly limited and can be adjusted according to the leuco dye used. Generally, the content of N, N'-diaryl urea compounds is preferably 0.1 mass parts or more relative to 1 mass part of leuco dye, more preferably 0.2 mass parts or more, and even more preferably 0.4 mass parts or more. The content of N, N'-diaryl urea compounds is also preferably 6 mass parts or less relative to 1 mass part of leuco dye, more preferably 5 mass parts or less, and even more preferably 4 mass parts or less. The content of 0.1 mass parts or more can improve water resistance, water plasticizer resistance and alcohol resistance. The content of 6 mass parts or less can improve recording performance.

[0137] Binder

[0138] Examples of the binder include water-soluble polymer materials, such as polyvinyl alcohol and its derivatives, starch and its derivatives, cellulose derivatives such as hydroxymethylcellulose, hydroxyethylcellulose, hydroxypropylcellulose, methylcellulose and ethylcellulose, sodium polyacrylate, polyvinyl pyrrolidone, acrylamide-acrylate copolymer, acrylamide-acrylate-methacrylate copolymer, styrene-maleic anhydride copolymer, isobutylene-maleic anhydride copolymer, casein, gelatin, and its derivatives; emulsions such as polyvinyl acetate, polyurethane, polyacrylic acid, polyacrylate, vinyl chloride-vinyl acetate copolymer, polybutyl methacrylate and ethylene-vinyl acetate copolymer; and latex of water-insoluble polymers such as styrene-butadiene copolymer and styrene-butadiene-acrylic acid copolymer; etc. Among them, polyvinyl alcohol and latex are preferred. The content of the binder can be selected from a wide range, and is generally preferably about 5 to 30% by mass, and more preferably about 10 to 20% by mass based on the total solid content of the thermosensitive recording layer.

[0139] In the present invention, the thermosensitive recording layer may further contain a preservability improver mainly for further enhancing the preservability of the color developed image. As such a preservability improver, for example, a phenol compound selected from 1,1,3-tris(2-methyl-4-hydroxy-5-cyclohexylphenyl)butane, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 1,1-bis(2-methyl-4-hydroxy-5-tert-butylphenyl)butane, 4,4'-[1,4-phenylenebis(1-methylethylidene)]bisphenol and 4,4'-[1,3-phenylenebis(1-methylethylidene)]bisphenol can be used. At least one of the group consisting of bis(1-methylethylidene)] bisphenol; epoxy compounds such as 4-benzyloxyphenyl-4'-(2-methyl-2,3-epoxypropoxy)phenyl sulfone, 4-(2-methyl-1,2-epoxyethyl)diphenyl sulfone and 4-(2-ethyl-1,2-epoxyethyl)diphenyl sulfone; and isocyanuric acid compounds such as 1,3,5-tris(2,6-dimethylbenzyl-3-hydroxy-4-tert-butyl)isocyanuric acid. Of course, the usable storage improver is not limited to these compounds, and two or more such compounds may be used in combination as needed.

[0140] When a preservability improver is used, its amount used may be an effective amount for improving preservability. The preservability improver is generally preferably used in an amount of about 1 to 25 mass %, and more preferably about 5 to 20 mass %, based on the total solid content of the thermosensitive recording layer.

[0141] In the present invention, the thermosensitive recording layer may further contain a sensitizer. Use of a sensitizer improves recording sensitivity. Examples of useful sensitizers include stearic acid amide, methoxycarbonyl-N-stearic acid benzamide, N-benzoyl stearic acid amide, N-eicosanoic acid amide, ethylene bis stearic acid amide, behenic acid amide, methylene bis stearic acid amide, N-hydroxymethyl stearic acid amide, dibenzyl terephthalate, dimethyl terephthalate, dioctyl terephthalate, diphenyl sulfone, benzyl p-benzyloxybenzoate, 1-hydroxy-2-naphthoic acid phenyl ester, 2-naphthyl benzyl ether, m-terphenyl, p-benzyl biphenyl, oxalic acid-di-p-chlorobenzyl ester, oxalic acid-di-p-methylbenzyl ester, oxalic acid-dibenzyl ester, p-tolyl biphenyl ether, di(p-methoxyphenoxyethyl) ether, 1,2-di(3-methylphenoxy)ethane, 1,2-di(4-methylphenoxy)ethane 1,2-bis(4-methoxyphenoxy)ethane, 1,2-bis(4-chlorophenoxy)ethane, 1,2-bis(phenoxy)ethane, 1-(4-methoxyphenoxy)-2-(3-methylphenoxy)ethane, p-methylthiophenylbenzyl ether, 1,4-bis(phenylthio)butane, p-acetyltoluidine, p-acetylethoxyaniline (p-acetophenetidide), N-acetoacetyl-p-toluidine, 1,2-bis(phenoxytoluene), di(β-biphenylethoxy)benzene, p-bis(vinyloxyethoxy)benzene, 1-isopropylphenyl-2-phenylethane, di-o-chlorobenzyl adipate, 1,2-bis(3,4-dimethylphenyl)ethane, 1,3-bis(2-naphthyloxy)propane, biphenyl, and benzophenone. Among them, 1,2-bis(3-methylphenoxy)ethane is preferred from the viewpoint of excellent balance between color development density and storage stability. These sensitizers can be used in combination as long as the combined use does not impair the effect of the present invention. The content of the sensitizer can be an effective amount for sensitization, and is usually preferably 2 to 25% by mass, more preferably 5 to 20% by mass, and even more preferably 5 to 15% by mass based on the total solid content of the thermosensitive recording layer.

[0142] From the viewpoint of improving the whiteness of the thermosensitive recording layer and improving the uniformity of the image obtained, the thermosensitive recording layer may contain fine particle pigments with high whiteness and an average particle size of 10 μm or less. Examples of usable fine particle pigments include: inorganic pigments such as calcium carbonate, magnesium carbonate, kaolin, clay, talc, calcined clay, silicon dioxide, diatomaceous earth, synthetic aluminum silicate, zinc oxide, titanium oxide, aluminum hydroxide, barium sulfate, surface-treated calcium carbonate, and surface-treated silicon dioxide; and organic pigments such as urea-formalin resin, styrene-methacrylic acid copolymer resin, and polystyrene resin. The content of fine particle pigments is preferably an amount that does not reduce the recording concentration, that is, the total solid content based on the thermosensitive recording layer is 50% by mass or less.

[0143] As other components constituting the thermosensitive recording layer, a binder may be used. In addition, auxiliary agents such as a crosslinking agent, waxes, metal soaps, a water resistance improver, a dispersant, a color dye, a fluorescent dye, etc. may be used as required.

[0144] When the thermosensitive recording layer contains a crosslinking agent, the water resistance of the thermosensitive recording layer can be improved. Examples of crosslinking agents include aldehyde compounds such as glyoxal; polyamine compounds such as polyethyleneimine; epoxy compounds, polyamide resins, melamine resins, glyoxylates, dimethylol urea compounds, aziridine compounds, blocked isocyanate compounds; inorganic compounds such as ammonium persulfate, ferric chloride, magnesium chloride, sodium tetraborate and potassium tetraborate; boric acid, boric acid triesters, boron polymers, hydrazide compounds, and glyoxylates, etc. These can be used alone or in combination of two or more. The amount of the crosslinking agent used is preferably about 1 to 5% by mass based on the total solid content of the thermosensitive recording layer.

[0145] The heat-sensitive recording layer is formed on the undercoat layer as follows: for example, by using water as a dispersion medium and using at least one of various agitators or wet pulverizers such as a ball mill, a co-ball mill, an attritor, or a vertical or horizontal sand mill, a leuco dye and a developer, and, if necessary, together with or separately from a sensitizer and a preservability improver, together with a water-soluble synthetic polymer compound such as polyacrylamide, polyvinyl pyrrolidone, polyvinyl alcohol, methylcellulose, or a styrene-maleic anhydride copolymer salt, and other additives such as a surfactant, to form a dispersion; then, the dispersion obtained by reducing the average particle size so that the average particle size is 2 μm or less is mixed with a binder, and optionally further mixed with an inorganic pigment and an auxiliary agent, etc., to prepare a heat-sensitive recording layer coating; the heat-sensitive recording layer coating is applied on the undercoat layer; and then dried. The coating amount of the heat-sensitive recording layer is not particularly limited, and is preferably about 1 to 12 g / m in terms of the coating amount after drying. 2 , more preferably 2 to 10 g / m 2 , even more preferably 2.5 to 8 g / m 2 , and particularly preferably 3 to 5.5 g / m 2 Note that the thermosensitive recording layer may be formed as two or more separate layers, and the composition and coating amount of each layer may be the same or different, as necessary.

[0146] Protective layer

[0147] As required, the thermosensitive recording medium may include a protective layer formed on the thermosensitive recording layer. The protective layer preferably comprises a pigment and a binder. The protective layer preferably further comprises a lubricant, such as a polyolefin wax or zinc stearate, to prevent the protective layer from adhering to the thermal head. The protective layer may also comprise an ultraviolet light absorber. When a glossy protective layer is formed, the obtained product may have an increased added value.

[0148] The pigment contained in the protective layer is not particularly limited. Examples include inorganic pigments such as amorphous silica, kaolin, clay, light calcium carbonate, heavy calcium carbonate, calcined kaolin, titanium oxide, magnesium carbonate, aluminum hydroxide, colloidal silica, and synthetic layered mica; and plastic pigments such as urea-formalin resin fillers; etc.

[0149] The binder included in the protective layer is not particularly limited, and an aqueous binder selected from a water-soluble binder and a water-dispersible binder can be used. The binder can be appropriately selected from binders that can be used for the heat-sensitive recording layer. Among them, various modified polyvinyl alcohols such as acetoacetyl-modified polyvinyl alcohol, carboxyl-modified polyvinyl alcohol and diacetone-modified polyvinyl alcohol can be more preferably used.

[0150] For example, a pigment and a binder are mixed with an auxiliary agent or the like using water as a dispersion medium to prepare a coating for a protective layer, the coating is applied to the thermosensitive recording layer, and then dried to form a protective layer on the thermosensitive recording layer. The coating amount of the coating for the protective layer is not particularly limited, and is preferably about 0.3 to 15 g / m2 in terms of dry mass. 2 , more preferably about 0.3 to 10 g / m 2 , even more preferably about 0.5 to 8 g / m 2 , particularly preferably about 1 to 8 g / m 2 , and more preferably about 1 to 5 g / m 2 The protective layer may be formed as two or more separate layers as necessary, and the composition and coating amount of each layer may be the same or different.

[0151] Other layers

[0152] In the present invention, the thermosensitive recording body preferably has an adhesive layer on at least one surface of the support. This can increase the added value of the thermosensitive recording body. For example, adhesive paper, rewet adhesive paper or delayed adhesive paper can be formed as an adhesive layer by coating one surface of the support with, for example, an adhesive such as an adhesive, a rewet adhesive or a delayed adhesive type adhesive. The recording paper capable of double-sided recording can also be formed by giving the surface of the support body opposite to the thermosensitive recording layer the function of thermal transfer paper, inkjet recording paper, carbonless paper, electrostatic recording paper or electrostatic copy paper. Of course, the thermosensitive recording body can be formed as a double-sided thermosensitive recording body. A back layer can also be provided to suppress the penetration of oil and plasticizer from the back of the thermosensitive recording body, or for curl control and antistatic purposes. The thermosensitive recording body can also be formed as a linerless label that does not require a release paper by forming a release layer containing silicone on a protective layer and applying an adhesive to one side.

[0153] Thermal recording medium

[0154] Thermosensitive recording medium can be produced by forming the above-mentioned layers on a support. Any known coating method, such as air knife method, scraper method, gravure method, roller coating method, spraying method, dipping method, rod coating method, curtain coating method, slot die method, slip die method and extrusion method can be used as a method for forming the above-mentioned layers on a support. Each coating can be applied in a manner such that the first coating is applied and dried, and then the second coating is applied and dried to form layer after layer, or the same coating can be applied separately to form more than two layers of layers. In addition, simultaneous multilayer coating can also be carried out, wherein all coatings are applied at once to form more than two layers of layers at the same time. At any stage after forming each layer or after all layers are formed, the layer can be smoothed by known methods such as super calendering or soft calendering.

[0155] Example

[0156] The present invention is described in more detail with reference to examples. However, the present invention is not limited to these examples. In the examples, unless otherwise stated, "parts" and "%" represent "parts by mass" and "% by mass". Particle diameters, such as average particle diameter and maximum particle diameter, are measured using a SALD2200 laser diffraction particle size distribution analyzer (produced by Shimadzu Corporation). "Average particle diameter" used herein refers to median diameter (D50).

[0157] The hollow particles used in Examples and Comparative Examples are as follows.

[0158] Hollow particles A: average particle size (D50): 5.0 μm; maximum particle size (D100): 13.5 μm; hollow ratio: 90%; proportion of particles with a particle size of less than 2 μm: 0.2% by volume; solid content concentration: 15.0%

[0159] Hollow particles B: average particle size (D50): 11 μm; maximum particle size (D100): 23 μm; hollow ratio: 93%; proportion of particles with a particle size of 2 μm or less: 0% by volume; solid content concentration: 15.0%

[0160] Hollow particles C: Ropaque SN-1055 (produced by Dow); average particle size (D50): 1.0 μm; maximum particle size (D100): 1.8 μm; hollow ratio: 55%; solid content concentration: 26.5%

[0161] The average particle size (D50) and the maximum particle size (D100) of these hollow particles were measured at a refractive index of 1.70-0.01i using a SALD2200 laser diffraction particle size analyzer (manufactured by Shimadzu Corporation).

[0162] The latexes used in Examples and Comparative Examples are as follows.

[0163] Latex A: Developed product of styrene-butadiene copolymer latex (Tg: -35°C; particle size: 300nm; solid content concentration: 48%)

[0164] Latex B: Developed product of styrene-butadiene copolymer latex (Tg: -10°C; particle size: 190nm; solid content concentration: 48%)

[0165] Latex C: Styrene-butadiene copolymer latex (trade name: L-1571, produced by Asahi Kasei Corporation; Tg: -3°C; particle size: 190 nm; solid content concentration: 48%)

[0166] Example 1

[0167] (1) Preparation of coating solution for undercoat layer

[0168] A coating liquid for an undercoat layer was prepared by mixing and stirring 100 parts of hollow particles A, 38 parts of calcined kaolin (trade name: Ansilex 93, produced by BASF), 79.2 parts of latex A, 32 parts of a 25% aqueous oxidized starch solution, 1.1 parts of carboxymethyl cellulose (trade name: Cellogen AGgum, produced by DKS Co., Ltd.) and 100 parts of water.

[0169] (2) Preparation of leuco dye dispersion (dispersion A)

[0170] 40 parts of 3-di-(n-butyl)amino-6-methyl-7-anilinofluoran, 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand grinder) to an average particle diameter of 0.5 μm, thereby obtaining a leuco dye dispersion (dispersion A).

[0171] (3) Preparation of developer dispersion (dispersion B)

[0172] 40 parts of 4-hydroxy-4'-isopropoxydiphenyl sulfone, 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle size of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid B).

[0173] (4) Preparation of developer dispersion (dispersion C)

[0174] 40 parts of N,N'-di-[3-(p-toluenesulfonyl)oxy]phenylurea, 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion C).

[0175] (5) Preparation of sensitizer dispersion (dispersion D)

[0176] 40 parts of 1,2-bis(3-methylphenoxy)ethane (trade name: KS-232, manufactured by Sankosha Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500; saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a sensitizer dispersion (dispersion D).

[0177] (6) Preparation of coating liquid for thermosensitive recording layer

[0178] A coating liquid for a thermosensitive recording layer was prepared by mixing and stirring 31.8 parts of leuco dye dispersion A, 63.6 parts of developer dispersion B, 15.9 parts of developer dispersion C, 22.7 parts of sensitizer dispersion D, 46.7 parts of a 15% aqueous solution of completely saponified polyvinyl alcohol (trade name: PVA110, saponification degree: 99 mol%, average polymerization degree: 1000, produced by Kuraray Co., Ltd.), 20.8 parts of styrene-butadiene copolymer latex (trade name: L-1571, produced by Asahi Kasei Corp., solid content concentration: 48%), 18 parts of aluminum hydroxide (trade name: Higilite H-42, produced by Showa Keikinzoku), 5 parts of adipic acid dihydrazide (produced by Otsuka Chemical Co., Ltd.) and 200 parts of water.

[0179] (7) Preparation of coating liquid for protective layer

[0180] A protective layer coating liquid was prepared by mixing and stirring a composition comprising 308 parts of a 12% aqueous solution of diacetone-modified polyvinyl alcohol (trade name: DF-10, produced by Japan Vam & Poval Co., Ltd.), 60 parts of kaolin (trade name: Hydragloss 90, produced by KaMin LLC), 5.6 parts of zinc stearate wax (trade name: Hidorin Z-8, produced by Chukyo Yushi Co., Ltd.; solid content concentration: 36%) and 150 parts of water.

[0181] (8) Preparation of Thermosensitive Recording Material

[0182] The coating liquid for the undercoat layer, the coating liquid for the thermosensitive recording layer, and the coating liquid for the protective layer were applied in an amount of 4.5 g / m 2 3.5g / m 2 and 2.5g / m 2 Coated to a basis weight of 60g / m 2 The thermosensitive recording body is obtained by applying a thermosensitive recording layer to the surface of a high-quality paper and drying the film to form an undercoat layer, a thermosensitive recording layer and a protective layer in sequence. The obtained product is then subjected to supercalendering to smooth the surface, thereby obtaining a thermosensitive recording body.

[0183] Example 2

[0184] A thermosensitive recording body was obtained in the same manner as in Example 1, except that in the preparation of the thermosensitive recording layer coating liquid of Example 1, the amount of the developer dispersion liquid C was changed from 15.9 parts to 6.8 parts.

[0185] Example 3

[0186] A thermosensitive recording body was obtained in the same manner as in Example 1 except that in the preparation of the thermosensitive recording layer coating liquid of Example 1, the amount of the developer dispersion liquid B was changed from 63.6 parts to 39.8 parts, and the amount of the developer dispersion liquid C was changed from 15.9 parts to 39.8 parts.

[0187] Example 4

[0188] A thermosensitive recording body was obtained in the same manner as in Example 1 except that in the preparation of the thermosensitive recording layer coating liquid of Example 1, the amount of the developer dispersion liquid B was changed from 63.6 parts to 31.8 parts, and the amount of the developer dispersion liquid C was changed from 15.9 parts to 47.7 parts.

[0189] Example 5

[0190] (9) Preparation of developer dispersion (dispersion E)

[0191] 40 parts of 2,4'-dihydroxydiphenyl sulfone (trade name: 2,4'-BPS, manufactured by Nicca Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion E).

[0192] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of Developer Dispersion Liquid E was used instead of 63.6 parts of Developer Dispersion Liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0193] Example 6

[0194] (10) Preparation of developer dispersion (dispersion F)

[0195] 40 parts of 4,4'-dihydroxydiphenyl sulfone (trade name: 4,4'-BPS, manufactured by Nicca Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion F).

[0196] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of Developer Dispersion Liquid F was used instead of 63.6 parts of Developer Dispersion Liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0197] Example 7

[0198] (11) Preparation of developer dispersion (dispersion G)

[0199] 40 parts of bis(3-allyl-4-hydroxy)diphenylsulfone (trade name: TG-SH, manufactured by Nippon Kayaku Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid G).

[0200] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of Developer Dispersion Liquid G was used instead of 63.6 parts of Developer Dispersion Liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0201] Example 8

[0202] (12) Preparation of developer dispersion (dispersion H)

[0203] 40 parts of 4-hydroxyphenyl (4'-n-propoxyphenyl) sulfone (trade name: Tomirac KN, manufactured by Mitsubishi Chemical Corporation), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion H).

[0204] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of the developer dispersion liquid H was used instead of 63.6 parts of the developer dispersion liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0205] Example 9

[0206] (13) Preparation of developer dispersion (dispersion J)

[0207] 40 parts of 4-hydroxy-4'-benzyloxydiphenyl sulfone (trade name: BPS-MBE, manufactured by Nicca Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion J).

[0208] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of Developer Dispersion Liquid J was used instead of 63.6 parts of Developer Dispersion Liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0209] Example 10

[0210] (14) Preparation of developer dispersion (dispersion K)

[0211] 40 parts of 4-allyloxy-4'-hydroxydiphenyl sulfone (trade name: BPS-MAE, manufactured by Nicca Chemical Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized to an average particle diameter of 1.0 μm using a sand mill (manufactured by Aimex Co., Ltd., sand mill) to obtain a developer dispersion (dispersion K).

[0212] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of the developer dispersion liquid K was used instead of 63.6 parts of the developer dispersion liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0213] Embodiment 11

[0214] (15) Preparation of developer dispersion (dispersion liquid L)

[0215] 40 parts of N-p-toluenesulfonyl-N'-3-(p-toluenesulfonyloxy)phenylurea (trade name: PF201, manufactured by Solenis), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid L).

[0216] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of the developer dispersion liquid L was used instead of 63.6 parts of the developer dispersion liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0217] Example 12

[0218] (16) Preparation of developer dispersion (dispersion M)

[0219] 40 parts of N-[2-(3-phenylureido)phenyl]benzenesulfonamide (trade name: NKK-1304, manufactured by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion M).

[0220] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of the developer dispersion liquid M was used instead of 63.6 parts of the developer dispersion liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0221] Embodiment 13

[0222] A thermosensitive recording material was obtained in the same manner as in Example 12, except that in the preparation of the undercoat layer coating liquid of Example 12, the amount of hollow particles A was changed from 100 parts to 46.7 parts, the amount of calcined kaolin (trade name: Ansilex 93, produced by BASF) was changed from 38 parts to 46 parts, and the amount of water was changed from 100 parts to 145 parts.

[0223] Embodiment 14

[0224] A thermosensitive recording material was obtained in the same manner as in Example 12, except that in the preparation of the undercoat layer coating liquid of Example 12, latex B was used instead of latex A.

[0225] Embodiment 15

[0226] A thermosensitive recording material was obtained in the same manner as in Example 12, except that in the preparation of the undercoat layer coating liquid of Example 12, latex C was used instead of latex A.

[0227] Example 16

[0228] A thermosensitive recording material was obtained in the same manner as in Example 12, except that in the preparation of the undercoat layer coating liquid of Example 12, the hollow particles B were used instead of the hollow particles A.

[0229] Embodiment 17

[0230] A thermosensitive recording body was obtained in the same manner as in Example 12 except that in the preparation of the undercoat layer coating liquid of Example 12, 56.6 parts of hollow particles C were used instead of 100 parts of hollow particles A, and the amount of water was changed from 100 parts to 175 parts.

[0231] Embodiment 18

[0232] (17) Preparation of developer dispersion (dispersion N)

[0233] 40 parts of 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide (trade name: PF425, manufactured by Solenis), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle size of 1.0 μm, thereby obtaining a developer dispersion (dispersion N).

[0234] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 63.6 parts of Developer Dispersion Liquid N was used instead of 63.6 parts of Developer Dispersion Liquid B in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0235] Comparative Example 1

[0236] A thermosensitive recording body was obtained in the same manner as in Example 1 except that in the preparation of the thermosensitive recording layer coating liquid of Example 1, the amount of the developer dispersion liquid B was changed from 63.6 parts to 79.5 parts, and the amount of the developer dispersion liquid C was changed from 15.9 parts to 0 parts.

[0237] Comparative Example 2

[0238] (18) Preparation of developer dispersion (dispersion O)

[0239] 40 parts of a diphenyl sulfone derivative represented by the following formula (3) (trade name: D-90, produced by Nippon Soda Co., Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (produced by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid O).

[0240]

[0241] Wherein r=1 to 6.

[0242] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 15.9 parts of Developer Dispersion Liquid O was used instead of 15.9 parts of Developer Dispersion Liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0243] Comparative Example 3

[0244] (19) Preparation of developer dispersion (dispersion P)

[0245] 40 parts of 4,4-bis(4-methyl-3-phenoxycarbonylaminophenylurea)diphenylsulfone (trade name: UU, manufactured by Chemipro Kasei Kaisha, Ltd.), 40 parts of a 10% aqueous solution of polyvinyl alcohol (polymerization degree: 500, saponification degree: 88%) and 20 parts of water were mixed. The resulting mixture was pulverized with a sand mill (manufactured by Aimex Co., Ltd., sand mill) to an average particle diameter of 1.0 μm, thereby obtaining a developer dispersion (dispersion liquid P).

[0246] A thermosensitive recording body was obtained in the same manner as in Example 1, except that 15.9 parts of the developer dispersion liquid P was used instead of 15.9 parts of the developer dispersion liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 1.

[0247] Comparative Example 4

[0248] A thermosensitive recording body was obtained in the same manner as in Example 10, except that 15.9 parts of Developer Dispersion Liquid O was used instead of 15.9 parts of Developer Dispersion Liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 10.

[0249] Comparative Example 5

[0250] A thermosensitive recording body was obtained in the same manner as in Example 10, except that 15.9 parts of the developer dispersion liquid P was used instead of 15.9 parts of the developer dispersion liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 10.

[0251] Comparative Example 6

[0252] A thermosensitive recording body was obtained in the same manner as in Example 11, except that in the preparation of the thermosensitive recording layer coating liquid of Example 11, the amount of the developer dispersion liquid L was changed from 63.6 parts to 79.5 parts, and the amount of the developer dispersion liquid C was changed from 15.9 parts to 0 parts.

[0253] Comparative Example 7

[0254] A thermosensitive recording body was obtained in the same manner as in Example 11, except that 15.9 parts of Developer Dispersion Liquid O was used instead of 15.9 parts of Developer Dispersion Liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 11.

[0255] Comparative Example 8

[0256] A thermosensitive recording body was obtained in the same manner as in Example 11, except that 15.9 parts of the developer dispersion liquid P was used instead of 15.9 parts of the developer dispersion liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 11.

[0257] Comparative Example 9

[0258] A thermosensitive recording body was obtained in the same manner as in Example 12, except that in the preparation of the thermosensitive recording layer coating liquid of Example 12, the amount of the developer dispersion liquid M was changed from 63.6 parts to 79.5 parts, and the amount of the developer dispersion liquid C was changed from 15.9 parts to 0 parts.

[0259] Comparative Example 10

[0260] A thermosensitive recording body was obtained in the same manner as in Example 12, except that 15.9 parts of Developer Dispersion Liquid O was used instead of 15.9 parts of Developer Dispersion Liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 12.

[0261] Comparative Example 11

[0262] A thermosensitive recording body was obtained in the same manner as in Example 12, except that 15.9 parts of the developer dispersion liquid P was used instead of 15.9 parts of the developer dispersion liquid C in the preparation of the thermosensitive recording layer coating liquid of Example 12.

[0263] The Examples and Comparative Examples were evaluated according to the following methods. Table 1 shows the results.

[0264] Record concentration

[0265] An image was recorded on each thermosensitive recording medium using a thermosensitive recording evaluation machine (trade name: TH-PMD, produced by Ohkura Electric Co., Ltd.) with applied energy of 0.17 mJ / dot (midtone color density) and 0.25 mJ / dot (maximum color density). The printed portion was measured using a spectrophotometer (X-Rite 504, produced by X-Rite). A larger value indicates a larger print density.

[0266] The evaluation criteria for the mid-tone color density are as follows.

[0267] Color density is 1.00 or above: compatible with high-speed printing, very good

[0268] Color density is 0.80 or more and less than 1.00: required for practical use

[0269] Color density less than 0.80: Low sensitivity, with many defects such as white spots, which is problematic in actual use

[0270] The evaluation criteria for the maximum color density are as follows.

[0271] Color density is 1.40 or above: Very good

[0272] Color density is 1.20 or more and less than 1.40: required for practical use

[0273] Color density is less than 1.20: The printing density is low, which is undesirable in actual use

[0274] Water resistance

[0275] A sample of each thermosensitive recording medium that had been color developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.) was immersed in water for 24 hours. After this treatment, the optical density of the recorded portion was measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). In addition, the residual rate of the recorded portion was obtained according to the following equation.

[0276] Residual rate (%) = (recording density after treatment / recording density before treatment) × 100

[0277] ·The evaluation criteria are as follows.

[0278] Survival rate is 80% or more: Good

[0279] Survival rate is 60% or more and less than 80%: No real problem

[0280] Residual rate is less than 60%: the recorded concentration after treatment is low, which is problematic in practical use Water resistance to plasticizers

[0281] A wrap film (trade name: Hi-S Soft, produced by Nippon Carbide Industries Co., Inc.) was wound three times around a polycarbonate tube (diameter: 40 mm), and a sample prepared by immersing each thermosensitive recording body developed using a label printer (trade name: L-2000, produced by Ishida Co., Ltd.) in water for 5 seconds was placed on the film. The wrap film was further wound three times around the sample, and the sample was allowed to stand at 40° C. for 24 hours. After this treatment, the optical density of the recording portion was measured with a spectrophotometer (X-Rite 504, produced by X-Rite). In addition, the residual rate of the recording portion was obtained according to the following equation.

[0282] Residual rate (%) = (recording density after treatment / recording density before treatment) × 100

[0283] ·The evaluation criteria are as follows.

[0284] Survival rate is 80% or more: Good

[0285] Survival rate is 60% or more and less than 80%: No real problem

[0286] Residual rate less than 60%: The recorded concentration after treatment is low, which is problematic in practical use Alcohol resistance

[0287] A sample of each thermosensitive recording medium that had been color developed using a label printer (trade name: L-2000, manufactured by Ishida Co., Ltd.) was immersed in a 75 volume % ethanol aqueous solution for 10 minutes. After this treatment, the optical density of the white paper portion and the optical density of the recording portion were measured using a spectrophotometer (X-Rite 504, manufactured by X-Rite). In addition, the residual rate of the recording portion was obtained according to the following equation.

[0288] Residual rate (%) = (recording density after treatment / recording density before treatment) × 100

[0289] ·The evaluation criteria are as follows.

[0290] White paper density less than 0.10: Good

[0291] White paper density is 0.10 or more and less than 0.20: Slight fogging is observed, but there is no actual problem

[0292] White paper density is 0.20 or more: Strong fogging, which is problematic in actual use

[0293] Survival rate is 80% or more: Good

[0294] Survival rate is 60% or more and less than 80%: No real problem

[0295] The residual rate is less than 60%: the recorded concentration after processing is low, which is problematic in practical use

[0296]

[0297] As can be seen from Table 1, the thermosensitive recording materials of Examples 1 to 18 are excellent in water resistance, water plasticizer resistance, and alcohol resistance. In contrast, D-90 is insufficient as a storage quality improver, and UU causes fogging in the white paper portion in terms of alcohol resistance.

Claims

1. A thermosensitive recording medium comprising at least an undercoat layer and a thermosensitive recording layer in this order on a support, The base coating layer comprises inorganic pigments, hollow particles and a binder, The heat-sensitive recording layer comprises a leuco dye, a developer and a binder. The thermosensitive recording layer contains a first developer and a second developer as developers, and The thermosensitive recording layer contains an N,N'-diaryl urea compound represented by formula (1) as the second developer: in R2 means C 1-12 Alkyl, C 7-12 Arylalkyl or C 6-12 Aryl, the aralkyl and aryl groups may be C 1-12 Alkyl, C 1-12 Alkoxy, C 6-12 An aryl group or a halogen atom is substituted, and multiple R2 may be the same or different; and A1 represents a hydrogen atom or C 1-4 alkyl, and multiple A1 may be the same or different.

2. The thermosensitive recording material according to claim 1, wherein the N,N'-diaryl urea compound represented by formula (1) is selected from N,N'-bis-[3-(p-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(o-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(benzenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(mesitylenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(4-ethylbenzenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(2-naphthalenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(4-ethylbenzenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(2-naphthalenesulfonyloxy)phenyl]urea, N,N'-bis-[3-(2-naphthalenesulfonyloxy)phenyl]urea, -[3-(p-methoxybenzenesulfonyloxy)phenyl]urea, at least one of the group consisting of N,N'-bis-[3-(benzylsulfonyloxy)phenyl]urea, N,N'-bis-[3-(ethanesulfonyloxy)phenyl]urea, N,N'-bis-[3-(p-toluenesulfonyloxy)-4-methyl-phenyl]urea, N,N'-bis-[4-(p-toluenesulfonyloxy)phenyl]urea, N,N'-bis-[4-(benzenesulfonyloxy)phenyl]urea, N,N'-bis-[4-(ethanesulfonyloxy)phenyl]urea and N,N'-bis-[2-(p-toluenesulfonyloxy)]phenylurea.

3. The thermosensitive recording material according to claim 1, wherein the N,N'-diaryl urea compound represented by formula (1) is N,N'-di-[3-(p-toluenesulfonyl)oxy]phenyl urea.

4. The thermosensitive recording material according to any one of claims 1 to 3, comprising a diphenyl sulfone derivative represented by formula (2) as the first developer: Wherein R3 and R4 are the same or different and each represents C 1-4 Alkyl, C 2-4 Alkenyl, C 1-4 Alkoxy, C 2-4 Alkenyloxy, C 7-12 an aralkyloxy group or a halogen atom; m is an integer from 0 to 2; n is an integer from 1 to 3; and p and q are the same or different and each represents an integer of 0 to 2.

5. The thermosensitive recording material according to claim 4, wherein the diphenyl sulfone derivative represented by the formula (2) is at least one selected from the group consisting of 4-hydroxy-4'-isopropoxydiphenyl sulfone, 4,4'-dihydroxydiphenyl sulfone, 2,4'-dihydroxydiphenyl sulfone, bis(3-allyl-4-hydroxy)diphenyl sulfone, 4-hydroxyphenyl(4'-n-propoxyphenyl)sulfone, 4-allyloxy-4'-hydroxydiphenyl sulfone and 4-hydroxy-4'-benzyloxydiphenyl sulfone. 6 . The thermosensitive recording material according to claim 1 , wherein the first developer is N-p-toluenesulfonyl-N′-3-(p-toluenesulfonyloxy)phenyl urea.

7. The thermosensitive recording material according to any one of claims 1 to 3, wherein the first developer is N-[2-(3-phenylureido)phenyl]benzenesulfonamide.

8. The thermosensitive recording material according to any one of claims 1 to 3, wherein the first developer is 5-(N-3-methylphenyl-sulfonamide)-N',N"-bis-(3-methylphenyl)-isophthalic acid diamide.

9. The thermosensitive recording material according to any one of claims 1 to 3, wherein The second developer is contained in an amount of 0.1 to 3 parts by mass relative to 1 part by mass of the first developer.

10. The thermosensitive recording material according to any one of claims 1 to 3, wherein The second developer is contained in an amount of 0.1 to 1 part by mass relative to 1 part by mass of the first developer.

11. The thermosensitive recording material according to any one of claims 1 to 3, wherein The maximum particle size (D100) of the hollow particles is 10 to 30 μm and the average particle size (D50) is 4.0 to 15 μm, The ratio D100 / D50 of the maximum particle size (D100) to the average particle size (D50) is 1.8 to 3.0, and The volume % of hollow particles having a particle size of 2.0 μm or less is 1% or less. 12 . The thermosensitive recording material according to claim 1 , wherein the hollow particles have a hollow ratio of 80% to 98%.

13. The thermosensitive recording material according to any one of claims 1 to 3, wherein the binder in the undercoat layer comprises a binder resin having a glass transition temperature of -10°C or lower.

14. The thermosensitive recording material according to any one of claims 1 to 3, wherein the binder in the undercoat layer comprises a binder resin having a glass transition temperature of -30°C or lower. 15 . The thermosensitive recording material according to claim 1 , which has an adhesive layer on at least one surface of the support.

Citation Information

Patent Citations

  • Heat-sensitive recording body

    CN104995033A

  • N,N'-diarylurea derivative, manufacturing method thereof and thermosensitive recording material using same

    CN111032626A

  • Thermal recording material

    CN1296448A

  • Thermal recording material

    JP2003080846A

  • Heat-sensitive recording material

    JP2019043005A