Polyurethane composition for gas barrier in low indoor temperature buildings

By using a gas-proof layer formed by a two-component polyurethane composition in the refrigerated warehouse, the problem of insufficient gas-proof layer performance in the prior art is solved, high bond strength and low vapor permeability are achieved, and energy consumption and maintenance are reduced. Cost and environmentally friendly.

CN118974128APending Publication Date: 2024-11-15BASF SE
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380031749.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-06
Filing Date
2023-03-31
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The prior art has the gas-proof performance of low indoor temperature buildings, especially refrigerated warehouses, which still lacks the performance, resulting in vapor permeation and damage to the insulation layer, increasing energy consumption and maintenance costs.

Method used

Using a two-component polyurethane composition, wherein component A comprises a polyol, a chain extender, a catalyst and a water scavenger, component B comprises a polyisocyanate, and a gas-proof layer is formed by spray mixing, preferably component A and component B The weight ratio is 1:1 to 1.3, and after curing, a gas-proof layer with high bond strength and low vapor permeability is formed.

Benefits of technology

It significantly reduces the vapor permeability in buildings with low indoor temperatures, improves waterproofing and insulation effects, reduces energy consumption and maintenance costs of refrigerated warehouses, and does not require organic solvents and is environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005066576930000161
    Figure BDA0005066576930000161
Patent Text Reader

Abstract

The present invention relates to a two-component polyurethane composition for the preparation of gas barrier layers in low indoor temperature buildings, comprising component A and component B, component A comprising: (b) a polyol comprising at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms, (c) a chain extender, (d) a catalyst, (e) a water scavenger, and (f) optionally, a cross-linking agent, a defoaming agent and / or other auxiliary agents and additives; and the component B comprises (a) at least one polyisocyanate. The invention also relates to a method for producing gas barrier layers in low-indoor-temperature buildings using said two-component polyurethane composition, and to the use of the two-component polyurethane composition for reducing vapor permeation in low-indoor-temperature buildings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a two-component polyurethane composition for preparing a gas barrier in a low indoor temperature building, which comprises component A and component B, wherein component A comprises: (b) a polyol, comprising at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms, (c) a chain extender, (d) a catalyst, (e) a water scavenger, and (f) optionally, a crosslinking agent, a defoaming agent and / or other auxiliary agents and additives; and component B comprises: (a) at least one polyisocyanate. The present invention also relates to a method for preparing a gas barrier in a low indoor temperature building by using the above-mentioned two-component polyurethane composition, and use of the above-mentioned two-component polyurethane composition for reducing vapor permeation in a low indoor temperature building. Background Art

[0002] In the modern food industry, low indoor temperature buildings (such as cold storage warehouses) are widely used to store food for a long time. When building such low indoor temperature buildings, it is required that the insulation layer should have excellent heat preservation and water resistance to prevent the indoor temperature from rising and the food from spoiling due to moisture. However, many cold storage warehouses are faced with the problems of increased energy consumption and increased maintenance costs after 5 to 10 years of operation. The reasons for this phenomenon include damage to the insulation layer and penetration of steam into the wall of the cold storage warehouse. Condensation and frost have been found inside the insulation layer of these cold storage warehouses, and some insulation layers have even been soaked in moisture. Therefore, means for moisture-proof and gas-proof have been envisioned and have been incorporated into the wall of the cold storage warehouse.

[0003] CN107903803A discloses a two-component polyurethane coating for a gas barrier layer, wherein component A includes isocyanate and polyether polyol, and component B includes fluorinated acrylate resin, polyether polyol, catalyst, chain extender, defoamer, dispersant, filler and other additives. According to CN107903803A, the main technical means to prevent vapor include fluorinated acrylate resin, barrier filler, dispersant and defoamer to obtain a gas barrier effect.

[0004] CN109810623A discloses a coating for a gas barrier layer in a refrigerated warehouse, which comprises raw materials such as polyether polyol, isocyanate, plasticizer, catalyst, stabilizer and solvent. The coating is not a two-component composition, but is prepared by adding each component in sequence.

[0005] CN109177391A discloses a waterproof and gas-proof membrane for building a cold storage warehouse, comprising a waterproof membrane made of an aluminized polyester film, a polypropylene filament nonwoven fabric, and a polyurethane adhesive II. The polyurethane adhesive II is a two-component composition comprising polymeric MDI (pMDI), a polyether polyol, CaCO3 powder, water, cyclohexylamine, and an ethyl acetate aqueous solution. In the waterproof and gas-proof membrane of CN109177391A, the gas-proof effect is mainly obtained by the waterproof membrane made of an aluminized polyester film and a polypropylene filament nonwoven fabric.

[0006] Despite the above achievements, the water and vapor barrier properties of refrigerated warehouses are still unsatisfactory and there remains a need in the art to provide improved vapor barriers in low indoor temperature buildings. Summary of the invention

[0007] An object of the present invention is to provide a polyurethane composition for preparing a gas barrier in a low indoor temperature building, which composition shows an improved effect in reducing water vapor penetration and permeation into the insulation layer of a low indoor temperature building (such as a cold storage warehouse). This object is achieved by a two-component polyurethane composition for preparing a gas barrier, the composition comprising component A and component B, component A comprising

[0008] (b) a polyol comprising at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms,

[0009] (c) a chain extender,

[0010] (d) a catalyst,

[0011] (e) a water scavenger, and

[0012] (f) optionally, crosslinking agents, defoaming agents and / or other auxiliary agents and additives,

[0013] Component B includes

[0014] (a) at least one polyisocyanate.

[0015] The two-component polyurethane composition described above can be used to prepare the gas barrier layer by mixing the two components A and B together and curing the mixture thus formed. Preferably, the mixing of components A and B is achieved by spraying.

[0016] In one embodiment, the component (a) polyisocyanate is selected from the group consisting of tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate, isophorone diisocyanate (IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, methylene dicyclohexyl 4,4′-, 2,4′- and / or 2,2′-diisocyanate. Isocyanates (H12MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), 3,3'-dimethyl-4,4'-diisocyanatobiphenyl ester (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), dimethyldiphenyl 3,3'-diisocyanate, diphenylethane 1,2-diisocyanate and / or diphenylmethane diisocyanate (MDI), including diphenylmethane 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate, mixtures of monomeric diphenylmethane diisocyanate and diphenylmethane diisocyanate homologues having at least two rings (polymeric MDI), and mixtures of two or more of these isocyanates.

[0017] In one embodiment, component (b) polyol comprises at least one natural oil polyol having at least one, preferably more than one, more preferably three aliphatic chains containing 12 to 30 carbon atoms, preferably 16 to 26 carbon atoms, more preferably 18 to 24 carbon atoms.

[0018] In another embodiment, component (c) the chain extender is a substance having two hydrogen atoms reactive toward isocyanate and having a molar mass of less than 500 g / mol, preferably 60 g / mol to 400 g / mol. Preferably, the chain extender is a diol.

[0019] In one embodiment, the component (d) catalyst is selected from amines and organometallic compounds used alone or in combination. Preferably, the catalyst is an organobismuth compound.

[0020] In one embodiment, component (e) the water scavenger is selected from epoxy resins and aluminosilicates.

[0021] In another embodiment, component (f) includes crosslinkers, defoamers, fillers, surfactants, colorants, pigments, flame retardants, stabilizers, viscosity reducers, and substances with fungistatic and bacteriostatic effects.

[0022] In another embodiment, the two-component polyurethane composition of the present invention has a solid content of 98 wt % or more, preferably 99 wt % or more, or more preferably 99.5 wt % or more, measured according to GB / T 16777-2008.

[0023] In one embodiment, component A and component B are mixed in a weight ratio of 1:1 to 1.3, more preferably 1:1 to 1.2.

[0024] The present invention also relates to a method for preparing a gas barrier layer from the two-component polyurethane composition defined above, comprising the steps of mixing component A and component B of the two-component polyurethane composition together and subsequently curing the mixture thus formed.

[0025] The invention also relates to the use of a two-component polyurethane composition as defined above for reducing vapour permeation in buildings with low indoor temperatures, such as in refrigerated warehouses.

[0026] Compared with conventional polyurethane compositions, the two-component polyurethane composition of the present invention can be conveniently applied by, for example, spraying without the need for the promotion of organic solvents, and the prepared gas barrier layer thus has a reduced vapor permeability and improved bonding strength with the substrate. The gas barrier layer can impart improved waterproofing and heat preservation effects to refrigerated warehouses. DETAILED DESCRIPTION

[0027] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by those of ordinary skill in the art to which the invention belongs. As used herein, unless otherwise specified, the following terms have the meanings assigned to them below.

[0028] As used herein, the articles "a" and "an" refer to one or to more than one (ie, to at least one) of the grammatical object of the article. For example, "an element" means one element or more than one element.

[0029] As used herein, the term "about" should be understood to refer to a range of numerical values ​​that one of skill in the art would consider equivalent to the recited value in the context of achieving the same function or result.

[0030] As used herein, the term "additive" refers to an additive included in a formulated system to enhance the physical or chemical properties of the system and provide the desired results. Such additives include, but are not limited to, dyes, pigments, toughening agents, impact modifiers, rheology modifiers, plasticizers, thixotropic agents, natural or synthetic rubbers, fillers, reinforcements, thickeners, inhibitors, fluorescent or other markers, thermal degradation reducers, thermal resistance imparting agents, surfactants, wetting agents, defoamers, dispersants, flow or sliding aids, biocides and stabilizers.

[0031] Unless otherwise indicated, all percentages (%) are by weight.

[0032] The radical definitions or explanations given above in general terms or within the preferred range are applicable to the final product and are correspondingly applicable to starting materials and intermediates. These free radical definitions can be combined with each other as required, i.e., comprising a combination between a general definition and / or a corresponding preferred range and / or an embodiment.

[0033] All embodiments and preferred embodiments disclosed herein may be combined as desired, which are also considered to be within the scope of the present invention.

[0034] Unless indicated otherwise, temperature refers to room temperature and pressure refers to ambient pressure.

[0035] Unless otherwise stated, solvents refer to all organic and inorganic solvents known to the person skilled in the art and do not include monomer molecules of any type.

[0036] The present invention relates to a two-component polyurethane composition for preparing an air barrier in a low indoor temperature building, the composition comprising component A and component B, wherein component A comprises

[0037] (b) a polyol comprising at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms,

[0038] (c) a chain extender,

[0039] (d) a catalyst,

[0040] (e) a water scavenger, and

[0041] (f) optionally, crosslinking agents, defoaming agents and / or other auxiliary agents and additives,

[0042] Component B includes

[0043] (a) at least one polyisocyanate.

[0044] (a) Polyisocyanate

[0045] The polyisocyanates (a) used in the polyurethane composition according to the invention include all polyisocyanates known for the production of polyurethanes. These polyisocyanates include aliphatic, alicyclic and aromatic divalent or polyvalent isocyanates known from the prior art, and any desired mixtures thereof. The aliphatic diisocyanates used are conventional aliphatic and / or alicyclic diisocyanates, for example tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanates, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate, 1- Isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, methylene dicyclohexyl 4,4'-, 2,4'- and / or 2,2'-diisocyanate (H12MDI). Suitable aromatic diisocyanates are, in particular, naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), 3,3′-dimethyl-4,4′-diisocyanatobiphenyl ester (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4′-diisocyanate (EDI), dimethyldiphenyl 3,3′-diisocyanate, diphenylethane 1,2-diisocyanate and / or diphenylmethane diisocyanate (MDI), including diphenylmethane 4,4′-diisocyanate, diphenylmethane 2,4′-diisocyanate, mixtures of monomeric diphenylmethane diisocyanates with diphenylmethane diisocyanate homologues having at least two rings (polymeric MDI).

[0046] The polyisocyanate (a) preferably used here is an aromatic polyisocyanate which is readily available industrially, and a mixture of diphenylmethane diisocyanate (MDI) and polyphenylpolymethylene polyisocyanate is particularly preferred.

[0047] The polyisocyanate (a) can also be used in the form of a polyisocyanate prepolymer. These polyisocyanate prepolymers can be obtained by reacting an excess of the above-mentioned polyisocyanate (component (a)) with a polymeric compound having isocyanate-reactive groups and / or a chain extender, for example at a temperature of 20° C. to 100° C., preferably about 80° C., to provide an isocyanate prepolymer.

[0048] Polymeric compounds having isocyanate-reactive groups and chain extenders are known to the person skilled in the art and are described, for example, in “Kunststoffhandbuch [Plastics Handbook], Volume 7, Polyurethane [Polyurethanes]”, Carl Hanser Verlag, 3rd edition, 1993, Chapter 3.1.

[0049] In a preferred embodiment, the polyisocyanate (a) is polymeric diphenylmethane diisocyanate (pMDI).

[0050] (b) Polyols

[0051] The component (b) polyol used here preferably has a number average molecular weight in the range of 400 g / mol to 15000 g / mol, preferably in the range of 500 g / mol to 12000 g / mol, more preferably in the range of 500 g / mol to 6000 g / mol, in particular in the range of 500 g / mol to 3000 g / mol, and an average functionality of 2 to 8, preferably 2 to 6, more preferably 2 to 4. Useful compounds under this heading can therefore be selected from the group comprising polyether polyols, polyester polyols, polycarbonate polyols, polycaprolactone polyols or mixtures thereof, preferably polyether polyols. Polyether polyols are prepared, for example, from epoxides such as propylene oxide and / or ethylene oxide, or from tetrahydrofuran with active hydrogen starting compounds such as aliphatic alcohols, phenols, amines, carboxylic acids, esters, water or natural compounds such as sucrose, sorbitol or mannitol by using a catalyst. Suitable catalysts here include basic catalysts or double metal cyanide catalysts, as described, for example, in PCT / EP2005 / 010124, EP 90444 or WO 05 / 090440.

[0052] In the present invention, polyol (b) comprises at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms. Preferably, polyol (b) comprises at least one natural oil polyol having at least one, preferably more than one, more preferably three aliphatic chains containing 12 to 30 carbon atoms, preferably 16 to 26 carbon atoms, more preferably 18 to 24 carbon atoms. In the context of the present invention, examples of suitable natural oil polyols include castor oil, hydrogenated castor oil, soybean oil polyol, palm oil polyol, rosin-based polyols, hydroxy-modified fatty acid esters based on myristoleic acid, palmitoleic acid, oleic acid, vaccenic acid, petroselinic acid, gadoleic acid, erucic acid, nervonic acid, linoleic acid, linolenic acid, octadecatetraenoic acid, arachidonic acid, eicosapentaenoic acid, oleic acid and docosahexaenoic acid, and their derivatives. The term "derivatives" includes alkoxylates, transesterification products, ozonolysis / reduction products, ozonolysis / glycolysis products, hydroformylation / reduction products, epoxidation / ring opening products of carbon-carbon double bonds or other hydroxyl-containing products of these oils and esters. Preference is given to using castor oil and its reaction products with alkylene oxides or ketone-formaldehyde resins. Such compounds are known, for example, under the names 750 is available from BASF. As is known in the art, castor oil contains ricinoleic acid triglyceride as its main component, which contains hydroxyl groups in its carbon chain. Castor oil-based polyether polyols are obtained by reacting castor oil as a starting material with ethylene oxide and / or propylene oxide.

[0053] In certain embodiments, polyol (b) may also include at least one polyether polyol different from the natural oil polyol mentioned above, which is started by amines, esters and / or alcohols having one or more aliphatic chains containing at least 6 carbon atoms. The amines, esters and / or alcohols defined here are referred to as starting compounds. Suitable starting compounds for the polyether polyols in the present invention include amines, esters and / or alcohols having at least one C6-C30 aliphatic chain, preferably C6-C20 aliphatic chain. The aliphatic chain may be saturated or unsaturated, and may contain one or more alkenyl groups or alkynyl groups. In addition, functional groups (such as hydroxyl groups) may be attached to carbon atoms in the aliphatic chain. Examples of starting compounds include octadecylamine, stearyl alcohol, sucrose and sorbitol. In a preferred embodiment, the polyether polyol has a functionality greater than 5.

[0054] The polyether polyols that can be used in the present invention are produced by known methods. By way of example, they can be prepared by using alkali metal hydroxides such as sodium hydroxide or potassium hydroxide, or using alkali metal alcoholates such as sodium methoxide, sodium ethoxide or potassium ethoxide or potassium isopropoxide as catalysts, and adding at least one C6-C30 aliphatic alcohol, ester and / or amine starting molecule with 2 to 8, preferably 2 to 6 reactive hydrogen atoms as mentioned above, or by using Lewis acids such as antimony pentachloride, boron fluoride etherate or bleaching earth as cationic polymerization catalysts. Polyether polyols can also be prepared by one or more alkylene oxides having 2 to 4 carbon atoms in the alkylene part via double metal cyanide catalysis. Tertiary amines can also be used as catalysts, examples being triethylamine, tributylamine, trimethylamine, dimethylethanolamine, imidazole or dimethylcyclohexylamine. For specific intended uses, monofunctional initiators can also be incorporated into the structure of polyethers. Polyether polyols can be used alone or in the form of a mixture.

[0055] Examples of suitable alkylene oxides are tetrahydrofuran, 1,3-propylene oxide, 1,2- or 2,3-butylene oxide, styrene oxide, ethylene oxide and 1,2-propylene oxide, preferably ethylene oxide and 1,2-propylene oxide. These alkylene oxides can be used individually, successively or in the form of a mixture.

[0056] In one embodiment of the present invention, polyol (b) is present in an amount of 50% to 95% by weight, preferably 60% to 92% by weight, more preferably 70% to 90% by weight, based on the total weight of component A in the composition. In another embodiment of the present invention, at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms accounts for 40% to 100%, preferably 60% to 90% by weight of polyol (b). In particular, polyol (b) contains only castor oil as at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms.

[0057] (c) Chain Extender

[0058] Component (c) chain extenders which can be used are substances having a molar mass of preferably less than 500 g / mol, particularly preferably 60 g / mol to 400 g / mol, wherein the chain extenders have two hydrogen atoms reactive toward isocyanates. These chain extenders can be used individually or preferably in the form of a mixture. Preference is given to using diols having a molecular weight of less than 400 g / mol, particularly 60 g / mol to 400 g / mol, and especially 60 g / mol to 350 g / mol. Examples of chain extenders that can be used are aliphatic, cycloaliphatic and / or araliphatic diols having 2 to 14, preferably 2 to 10, carbon atoms, such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,10-decanediol and bis(2-hydroxyethyl)hydroquinone, 1,2-, 1,3- and 1,4-dihydroxycyclohexane, diethylene glycol, dipropylene glycol, tripropylene glycol, and low molecular weight hydroxylated polyalkylene oxides based on ethylene oxide and / or 1,2-propylene oxide and the aforementioned diols as starter molecules. Particular preference is given to using low molecular weight hydroxylated polyalkylene oxides based on ethylene oxide and / or 1,2-propylene oxide, particularly preferably on ethylene oxide.

[0059] The proportion of chain extender (c), based on the weight of component A, is preferably 1% to 25% by weight, particularly preferably 3% to 20% by weight and in particular 5% to 15% by weight.

[0060] (d) Catalyst

[0061] Component (d) catalyst greatly accelerates the reaction of component (b) and chain extender (c) with polyisocyanate (a). Catalyst (d) preferably comprises an amine-based catalyst and / or an organometallic compound.

[0062] Typical catalysts that can be used to produce polyurethanes include, for example: amidines such as 2,3-dimethyl-3,4,5,6-tetrahydropyrimidine, tertiary amines such as triethylamine, tributylamine, dimethylbenzylamine, N-methyl-, N-ethyl- and N-cyclohexylmorpholine, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylbutanediamine, N,N,N',N'-tetramethylhexanediamine, pentamethyldiethylenetriamine, tetramethyldiaminoethyl ether, bis(dimethylaminopropyl)urea, dimethylpiperazine, 1,2-dimethylimidazole, 1-azabicyclo[3.3.0]octane and preferably 1,4-diazabicyclo[2.2.2]octane, and alkanolamine compounds such as triethanolamine, triisopropanolamine, N-methyl- and N-ethyldiethanolamine, and dimethylethanolamine. Likewise suitable are organometallic compounds, preferably organobismuth compounds, especially bismuth carboxylates, such as bismuth(III) neodecanoate, bismuth 2-ethylhexanoate and bismuth octoate, or mixtures thereof. The organometallic compounds can be used alone or, preferably, in combination with strongly basic amines.

[0063] Amine-based catalysts have at least one, preferably 1 to 8, particularly preferably 1 to 2 groups reactive to isocyanate, such as primary amine, secondary amine, hydroxyl, amide or urea, preferably primary amine, secondary amine, hydroxyl. Amine-based amine catalysts are mainly used to produce low-emission polyurethanes, especially for automotive interiors. Such catalysts are known and described, for example, in EP1888664. These catalysts include compounds preferably containing one or more tertiary amino groups in addition to isocyanate-reactive groups. At least one tertiary amino group in the incorporable catalyst preferably carries at least two aliphatic hydrocarbon free radicals, preferably each free radical has 1 to 10 carbon atoms, particularly preferably each free radical has 1 to 6 carbon atoms. Particularly preferably, the tertiary amino group carries two free radicals independently selected from methyl free radicals and ethyl free radicals, plus another organic free radical. Examples of amine-based catalysts that can be used are bis(dimethylaminopropyl)urea, bis(N,N-dimethylaminoethoxyethyl)urethane, dimethylaminopropyl urea, N,N,N-trimethyl-N-hydroxyethylbis(aminopropyl ether), N,N,N-trimethyl-N-hydroxyethylbis(aminoethyl ether), diethylethanolamine, bis(N,N-dimethyl-3-aminopropyl)amine, dimethylaminopropylamine, 3-dimethylaminopropyl-N,N-dimethylpropane- 1,3-diamine, dimethyl-2-(2-aminoethoxyethanol), (1,3-bis(dimethylamino)propan-2-ol), N,N-bis(3-dimethylaminopropyl)-N-isopropanolamine, bis(dimethylaminopropyl)-2-hydroxyethylamine, N,N,N-trimethyl-N-(3-aminopropyl)-bis(aminoethyl ether), 1,4-diazabicyclo[2.2.2]octane-2-methanol and 3-dimethylaminoisopropyldiisopropanolamine, or mixtures thereof.

[0064] Catalyst (d) can be used, for example, in an amount of 0.005 to 5 wt %, preferably 0.01 to 3 wt %, more preferably 0.1 to 2 wt %, based on the total weight of component A. In a particularly preferred embodiment, the component (d) catalyst used is an organobismuth catalyst.

[0065] (e) Water scavenger

[0066] Component (e) water scavenger is a substance that can remove water, steam, moisture and / or vapor from the composition and / or the surrounding environment in which the composition is stored or used. These substances include, for example, epoxy resins and / or aluminosilicates. Possible aluminosilicates are selected from the group consisting of sodium aluminosilicate, potassium aluminosilicate, calcium silicate, cesium aluminosilicate, barium aluminosilicate, magnesium aluminosilicate, strontium aluminosilicate, sodium aluminophosphate, potassium aluminophosphate, calcium aluminophosphate, and mixtures thereof. It is particularly preferred to use T-paste as a water scavenger.

[0067] The number average particle size of the water scavenger is preferably not more than 200 μm, more preferably not more than 150 μm, and especially not more than 100 μm. The pore width of the water scavenger of the present invention is preferably to

[0068] The amount of water scavenger here is preferably greater than 0.5% by weight, particularly preferably in the range from 1 to 10 parts by weight, more preferably in the range from 2 to 8% by weight, based on the total weight of component A.

[0069] (f) Cross-linking agents, defoaming agents and / or other auxiliary agents and additives

[0070] The two-component polyurethane composition according to the present invention may also optionally contain a crosslinking agent, a defoaming agent and / or other auxiliaries and additives. If present, component (f) is present in an amount of 0.5% to 30% by weight, preferably 1% to 20% by weight, more preferably 1.5% to 10% by weight, based on the total weight of component A.

[0071] Crosslinkers are molecules with more than two isocyanate-reactive hydrogens. Preference is given to using triols and / or triamines with a molecular weight below 300 g / mol, more preferably in the range from 62 g / mol to below 300 g / mol, in particular in the range from 62 g / mol to 250 g / mol. Suitable crosslinkers are, for example, aliphatic, cycloaliphatic and / or araliphatic or aromatic triamines and triols having 2 to 14, preferably 2 to 10, carbon atoms, such as 1,2,4-, 1,3,5-trihydroxycyclohexane, glycerol and trimethylolpropane, diethanolamine, triethanolamine, and low molecular weight, hydroxyl-containing polyalkylene oxides based on ethylene oxide and / or 1,2-propylene oxide and the aforementioned diols and / or triols as starting molecules. Particularly preferably used as crosslinkers are low molecular weight, hydroxyl-containing polyalkylene oxides based on ethylene oxide and / or 1,2-propylene oxide, more preferably based on 1,2-propylene oxide, and trifunctional starters, especially glycerol and trimethylolpropane. When crosslinkers are used, the proportion of crosslinkers, based on the total weight of component A, will generally be in the range of 1% to 12% by weight, preferably 2% to 8% by weight.

[0072] The defoamers used preferably include silicone-based foam stabilizers. The foam stabilizers used may also include siloxane-polyoxyalkylene copolymers, organopolysiloxanes, ethoxylated fatty alcohols and alkylphenols, as well as castor oil esters and the corresponding ricinoleic acid esters.

[0073] Other auxiliaries and additives which may be used include fillers, surfactants, dyes, pigments, flame retardants, stabilizers, viscosity reducers, and substances having fungistatic and bacteriostatic action.

[0074] Stabilizers used against the effects of aging and weathering include primarily antioxidants. By way of example, these may be sterically hindered phenols, HALS stabilizers (hindered amine light stabilizers), triazines, benzophenones and benzotriazoles.

[0075] Examples of surfactants that can be used are compounds for promoting homogenization of the starting materials and ensuring phase stability of the polyol component over an extended period of time. Optionally, these substances are also suitable for regulating cell structure. By way of example, emulsifiers such as sodium salts of castor oil sulfate or sodium salts of fatty acids, and salts of fatty acids and amines, such as diethylamine oleate, stearic acid diethanolamine salt, ricinoleic acid diethanolamine salt, sulfonates, such as dodecylbenzene- or alkali metal salts or ammonium salts of dinaphthomethane disulfonic acid and ricinoleic acid; foam stabilizers such as siloxane-oxyalkylene copolymers and other organopolysiloxanes, ethoxylated alkylphenols, ethoxylated fatty alcohols, paraffin oils, castor oil esters and corresponding ricinoleic acid esters, Turkish red oil and peanut oil, and cell regulators such as paraffin, fatty alcohols and dimethylpolysiloxanes. Other suitable compounds for improving emulsification effects or cell structure and / or for stabilizing foam are oligomeric polyacrylates with polyoxyalkylene and fluoroalkane free radicals as side groups.

[0076] Surfactants are typically used in amounts of 0.01% to 5% by weight, based on the total weight of component A.

[0077] Fillers (especially reinforcing fillers) that can be added include materials known per se, which are conventional organic fillers and inorganic fillers, reinforcing agents and weighting agents. In detail, examples that can be mentioned are: inorganic fillers, for example silicate minerals, for example phyllosilicates, such as antigorite, serpentine, hornblende, amphibole, chrysotile, zeolite, talc; metal oxides, for example kaolin, aluminum oxide, aluminum silicate, titanium oxide and iron oxide; metal salts, for example chalk, barite; inorganic pigments, such as cadmium sulfide, zinc sulfide; and glass particles. Examples of organic fillers that can be used are: carbon black, melamine, rosin (collophony), cyclopentadiene-based resins, and polymer-modified polyoxyalkylene polyols.

[0078] The flame retardant used includes a flame retardant containing expandable graphite, and a flame retardant containing an oligomeric organic phosphorus flame retardant. Expandable graphite is well known. Expandable graphite includes one or more expandable materials so that considerable expansion occurs under fire conditions. Expandable graphite is produced by known methods. The conventional method here is to first modify graphite with an oxidant (such as nitrate, chromate or peroxide) or via electrolysis to open the crystal layer, and then insert nitrate or sulfate into the graphite, thereby being able to cause expansion under given conditions. The oligomeric organic phosphorus flame retardant preferably contains a phosphorus content of not less than 5% by weight, and in a preferred embodiment there are at least 3 phosphate units. "Phosphorus ester unit" includes phosphate units and phosphonate units here. Therefore, the oligomeric organic phosphorus flame retardant of the present invention includes a structure with pure phosphonate units, a structure with pure phosphate units, and a structure with phosphonate units and phosphate units.

[0079] For polyurethane, in addition to oligomeric organic phosphorus flame retardants and expandable graphite, one or more commonly used arbitrary flame retardants can also be used. These flame retardants include halogen-substituted phosphates, such as tricresyl phosphate, tris(2-chloroethyl) phosphate, tris(2-chloropropyl) phosphate, tris(1,3-dichloropropyl) phosphate, tris(2,3-dibromopropyl) phosphate and tetrakis(2-chloroethyl)ethylene diphosphate, and / or inorganic flame retardants, such as red phosphorus, alumina hydrate, antimony trioxide, arsenic oxide, ammonium polyphosphate and calcium sulfate, and / or cyanuric acid derivatives, such as melamine. It is preferred that the flame retardant does not include a compound with a halogen group.

[0080] Further information on the manner of use and mode of action of the aforementioned auxiliaries and additives as well as further examples are given by way of example in “Kunststoffhandbuch, Band 7, Polyurethane” [“Plastics handbook, Volume 7, Polyurethanes”], Carl Hanser Verlag, 3rd edition, 1993, Chapter 3.4.

[0081] The two-component polyurethane composition of the present invention can be obtained by using polyisocyanate (a) as component B, and simply mixing components (b) to (f) as component A, and then storing them separately. These components are stable at ambient pressure and room temperature, and can be formulated into a ready-to-use form before application. In the two-component polyurethane composition, the weight ratio of component A to component B is preferably in the range of 1:1 to 1.3, more preferably in the range of 1:1 to 1.2. In one embodiment, the two-component polyurethane composition of the present invention can have a solid content of 98% by weight or more, preferably 99% by weight or more, more preferably 99.5% by weight or more, measured according to GB / T 16777-2008. That is, no organic solvent is required in the two-component polyurethane composition. In one embodiment, the two-component polyurethane composition of the present invention does not contain an organic solvent.

[0082] The present invention also relates to a method for preparing a gas barrier in a low indoor temperature building, comprising mixing component A and component B in the aforementioned two-component polyurethane composition together, and then curing the step of the mixture thus formed. When building a low indoor temperature building (such as a cold storage), the gas barrier prepared by the two-component polyurethane composition is usually formed between a base layer and a thermal insulation layer. The mixing of component A and component B is preferably achieved by spraying. In spraying, component A and component B can be sprayed on the base layer of the cold storage warehouse at a certain weight ratio under high pressure by a spraying device with two independent nozzles, and the weight ratio is preferably 1:1 to 1.3, more preferably 1:1 to 1.2, and the mixture thus formed is cured on the base layer. The pressure of spraying can be 1000psi or more, or 1300psi or more, or 1500psi or more. The curing of the sprayed mixture can be completed in, for example, 0.5h to 8h, preferably 1h to 4h, more preferably 1h to 2h. In one embodiment, component A and component B are sprayed in powder form, and when mixed, these components immediately begin to react with each other and solidify in a short time. Even if the solid content is 98% by weight, 99% by weight or higher, component A and component B can be conveniently sprayed, and no organic solvent needs to be added to the mixture, which makes the two-component polyurethane composition of the present invention environmentally friendly and safe for users.

[0083] In one embodiment, the gas barrier layer can be prepared in one step by a two-component polyurethane composition as described above. Here, "in one step" should be understood to mean that the components for preparing the gas barrier layer, i.e., components (a) to (e) and (if present) (f) are all mixed together, the reaction starts immediately, and then the reaction is carried out to obtain a cured polyurethane material without admixing additional compounds, especially without admixing additional compounds containing isocyanate-reactive groups. The isocyanate index during the production of the polyurethane coating is 90 to 130, preferably 95 to 120, more preferably 100 to 110. For the purposes of the present invention, the isocyanate index is the stoichiometric ratio of isocyanate groups to groups reactive to isocyanate multiplied by 100. Here, "groups reactive to isocyanate" are any groups present in the reaction mixture and reactive to isocyanate.

[0084] The polyurethane gas barrier layer formed by the two-component polyurethane composition of the present invention acquires excellent physical properties once cured. The polyurethane gas barrier layer thus formed may have a high bonding strength, for example, 2.9 MPa or more, preferably 3.0 MPa or more, more preferably 3.3 MPa or more, as measured according to GB / T 16777-2008. The polyurethane gas barrier layer forms a strong bond with the substrate layer and improves the overall strength of the wall in low indoor temperature buildings. In addition, the polyurethane gas barrier layer imparts significantly reduced vapor permeability to the substrate layer and the thermal insulation layer. The polyurethane gas barrier layer formed by the two-component polyurethane composition of the present invention may have a thermal conductivity of 10 g / (m 2 .24h) or less, preferably 2.5g / (m 2 .24h) or less, more preferably 1.8g / (m 2 .24h) or less, still more preferably 1.6g / (m 2 .24h) or less. It should be understood that for the same composition, the vapor permeability of the thicker gas barrier layer is less than the vapor permeability of the thinner gas barrier layer. The vapor permeability is measured at a temperature of 23±0.5°C according to GB / T 17146-2015. Therefore, even if the insulation layer of the refrigerated warehouse is damaged to some extent and the vapor penetrates the insulation layer, the polyurethane gas barrier layer located between the insulation layer and the base layer can effectively prevent the vapor from entering the interior space of the refrigerated warehouse. Therefore, the present invention also relates to the use of the two-component polyurethane composition according to the present invention for producing a gas barrier in a building with an indoor temperature below 18°C. Here, the indoor temperature is preferably below 15°C, more preferably below 10°C, and even more preferably below 6°C.

[0085] The two-component polyurethane composition of the present invention can prepare a vapor barrier layer that is firmly bonded to a substrate layer and effectively reduces vapor permeability in low indoor temperature buildings (such as refrigerated warehouses) by including at least one polyether polyol of a specific type in component A together with other components.

[0086] Example

[0087] The present invention will now be described with reference to Examples (EX) and Comparative Examples (CEX), but these Examples and Comparative Examples are not intended to limit the present invention.

[0088] The following materials were used:

[0089] Isocyanate: Polymeric MDI, commercially available as Lupranate M20s from BASF, functionality of about 2.7, NCO content of 31.5%.

[0090] Polyol 1: Castor oil, commercially available from BASF, having a hydroxyl number of 163 mg KOH / g and a functionality of about 2.7. Castor oil is a mixture of triglycerides characterized by containing about 90% by weight of ricinoleic acid triglycerides.

[0091] Polyol 2: TAE-202 purchased from EnHou Polymer Chemical Ind. Co., Ltd., a polyether polyol starting from C18 alkylamine, with a hydroxyl value of 314 mg KOH / g, an average molecular weight of 357 g / mol, and a functionality of 2.

[0092] Polyol 3: NJ4502 purchased from Jurong Ningwu New Material Co., Ltd., a polyether polyol starting from sorbitol, with a hydroxyl value of 450±20 mg KOH / g and a functionality of 5.2.

[0093] Glycerin: Commercially available from SinoPharm Jiangsu Co. Ltd.

[0094] DEOA: diethanolamine commercially available from BASF.

[0095] MEG: Ethylene glycol commercially available from BASF.

[0096] DC193: A water-soluble silicone oil defoamer purchased from Evonik.

[0097] T-Paste: Type A zeolite sodium aluminosilicate in oil from UOP, used as a water scavenger.

[0098] E-100: diethyltoluenediamine available from Albemarle Corporation.

[0099] Coscat TM 83: Organic bismuth catalyst purchased from Vertellus.

[0100] X96: A reactive colorant available from Milliken.

[0101] Measurement method :

[0102] The bonding strength was determined according to GB / T 16777-2008 (Test methods for building waterproof coatings).

[0103] The vapor permeability is determined according to GB / T 17146-2015 (Test method for water vapor transmission characteristics of building materials and products) at a temperature of 23±0.5°C.

[0104] The solid content is measured according to GB / T 16777-2008 (Test methods for building waterproof coatings).

[0105] The reaction time is determined according to GB / T 23446-2009 (Spraying polyurea waterproof coating).

[0106] Example 1 :

[0107] 64.5 parts by weight of polyol 1, 15 parts by weight of polyol 3, 10 parts by weight of DEOA, 5 parts by weight of MEG, 0.1 parts by weight of DC193, 4 parts by weight of T-paste, 1 part by weight of E-100, 0.3 parts by weight of Coscat 83 and 0.1 parts by weight of X96 were fully mixed to obtain component A. 120 parts by weight of pMDI was used as component B. Component A and component B were stored in two separate barrels in a reactor H-40 purchased from GRACO. In order to produce the polyurethane coating, component A and component B were sprayed simultaneously from two independent nozzles by a sprayer onto a 30 cm×30 cm cement board. After spraying, the mixture began to solidify, and after curing for 5 minutes, a uniform polyurethane coating was formed on the cement board. The thickness of the coating was about 0.5 mm to 1 mm.

[0108] Example 2 :

[0109] The same process as in Example 1 was repeated, except that 44.5 parts by weight of polyol 1, 15 parts by weight of polyol 2, 25 parts by weight of polyol 3, 10 parts by weight of DEOA, 0.1 parts by weight of DC193, 4 parts by weight of T-paste, 1 part by weight of E-100, 0.3 parts by weight of Coscat 83 and 0.1 parts by weight of X96 were fully mixed to obtain component A.

[0110] Comparative Examples 1 and 2 :

[0111] The same process as in Example 1 was repeated except that the formulation was different and is given in Table 1.

[0112] For measurement, polyurethane coating samples were formed by the two-component polyurethane system in the examples and comparative examples according to GB / T 16777-2008, and then the bonding strength and vapor permeability were tested according to the measurement method mentioned above. The polyurethane coating has a thickness of 0.5 mm to 3 mm. The composition of each sample is summarized in Table 1 below, and the test results are summarized in Tables 2 and 3 below. In Table 2, the permeability values ​​of specific films are given, as well as the thickness of the films. For the same thickness, the films with lower permeability values ​​show stronger water vapor impermeability. For the same permeability values, the films with smaller thickness show stronger water vapor impermeability.

[0113] Table 1: Composition of polyurethane coatings produced in Examples and Comparative Examples

[0114] Sample / g EX 1 EX 2 CEX 1 CEX 2 PMDI 120 120 120 120 Polyol 1 64.5 44.5 55 Polyol 2 15 15 100 Polyol 3 15 25 15 Glycerol 10 DEOA 10 10 MEG 5 DC193 0.1 0.1 0.1 T-Paste 4 4 E-100 1 1 1 2 Coscat 83 0.3 0.3 0.3 X96 0.1 0.1 0.1

[0115] Table 2: Test results of samples

[0116]

[0117]

[0118] Table 3: Reaction time of Examples and Comparative Examples

[0119] sample Reaction time (s) EX 1 16 EX 2 13 CEX 1 9 CEX 2 18

[0120] As can be seen from Table 2 above, all samples in the examples produce polyurethane coatings with impermeable gas barrier layers. However, the sample prepared from the composition used in Example 1 exhibited the highest bond strength and the lowest vapor permeability among all samples. Without being bound by any theory, it is believed that the significant decrease in vapor permeability of Example 1 is due to the fact that castor oil used is used in the highest amount in these examples, and castor oil has three aliphatic C18 chains. In contrast, the sample prepared in Comparative Example 2, in which castor oil is not added, exhibits a significantly higher vapor permeability, which makes it unsuitable for use as a gas barrier in a refrigerated warehouse. In addition, Comparative Example 1, which does not include a chain extender but uses glycerol, has a high vapor permeability and a high tendency to delaminate due to the poor compatibility of glycerol with other components. In addition, Example 1 contains T-paste as a water scavenger, which reduces the content of free water by absorption or other mechanisms. As is known in the art, water in a polyurethane system can react with isocyanates and cause the sample to foam to a certain extent, thereby deteriorating the anti-vapor permeability of the sample.

[0121] The structures, materials, compositions and methods described herein are intended to be representative embodiments of the present invention, and it should be understood that the scope of the present invention is not limited by the scope of these embodiments. Those skilled in the art will recognize that the present invention can be operated using variations of the disclosed structures, materials, compositions and methods, and such variations are considered to be within the scope of the present invention. Therefore, it is intended that the present invention encompasses such modifications and variations that fall within the scope of the appended claims and their equivalents.

Claims

1. A two-component polyurethane composition for preparing an air barrier layer, comprising component A and component B, wherein component A comprises (b) a polyol comprising at least one natural oil polyol having one or more aliphatic chains containing at least 12 carbon atoms, (c) a chain extender, (d) a catalyst, (e) a water scavenger, and (f) optionally, crosslinking agents, defoaming agents and / or other auxiliary agents and additives, The component B comprises (a) at least one polyisocyanate.

2. The two-component polyurethane composition according to claim 1, wherein the natural oil polyol has one or more aliphatic chains containing 12 to 30 carbon atoms, preferably 16 to 26 carbon atoms, more preferably 18 to 24 carbon atoms.

3. A two-component polyurethane composition according to claim 1 or 2, wherein the natural oil polyol is selected from the group consisting of castor oil, hydrogenated castor oil, soybean oil polyol, palm oil polyol, rosin-based polyol, and hydroxy-modified fatty acid esters based on myristoleic acid, palmitoleic acid, oleic acid, vaccenic acid, petroselinic acid, gadoleic acid, erucic acid, nervonic acid, linoleic acid, linolenic acid, stearidonic acid, arachidonic acid, eicosapentaenoic acid, oleic acid and docosahexaenoic acid, and their derivatives.

4. The two-component polyurethane composition according to any one of claims 1 to 3, wherein the natural oil polyol is castor oil.

5. The two-component polyurethane composition according to any one of claims 1 to 4, wherein the natural oil polyol accounts for 40% to 100%, preferably 60% to 90% by weight of the polyol (b).

6. The two-component system according to any one of claims 1 to 5, wherein the polyol (b) further comprises at least one polyether polyol starting from amines, esters and / or alcohols having more than one, preferably three, aliphatic chains containing 6 to 30 carbon atoms.

7. The two-component polyurethane composition according to any one of claims 1 to 6, further comprising one or more polyether polyols having a functionality greater than 5.

8. A two-component polyurethane composition according to any one of claims 1 to 7, wherein the polyisocyanate is selected from the group consisting of tri-, tetra-, penta-, hexa-, hepta- and / or octamethylene diisocyanate, 2-methylpentamethylene 1,5-diisocyanate, 2-ethyltetramethylene 1,4-diisocyanate, hexamethylene 1,6-diisocyanate (HDI), pentamethylene 1,5-diisocyanate, butylene 1,4-diisocyanate, trimethylhexamethylene 1,6-diisocyanate, isophorone diisocyanate (IPDI), 1,4- and / or 1,3-bis(isocyanatomethyl)cyclohexane (HXDI), cyclohexane 1,4-diisocyanate, 1-methylcyclohexane 2,4- and / or 2,6-diisocyanate, methylene dicyclohexyl 4,4′-, 2,4′- and / or 2,2'-diisocyanate (H12MDI), naphthylene 1,5-diisocyanate (NDI), tolylene 2,4- and / or 2,6-diisocyanate (TDI), 3,3'-dimethyl-4,4'-diisocyanatobiphenyl ester (TODI), p-phenylene diisocyanate (PDI), diphenylethane 4,4'-diisocyanate (EDI), dimethyldiphenyl 3,3'-diisocyanate, diphenylethane 1,2-diisocyanate and / or diphenylmethane diisocyanate (MDI), including diphenylmethane 4,4'-diisocyanate, diphenylmethane 2,4'-diisocyanate, mixtures of monomeric diphenylmethane diisocyanate and diphenylmethane diisocyanate homologues having at least two rings (polymeric MDI), and mixtures of two or more of these isocyanates.

9. The two-component polyurethane composition according to any one of claims 1 to 8, wherein the polyisocyanate is polymeric MDI.

10. The two-component polyurethane composition according to any one of claims 1 to 9, wherein the chain extender is selected from aliphatic, cycloaliphatic and / or araliphatic diols having 2 to 14 carbon atoms.

11. The two-component polyurethane composition according to any one of claims 1 to 10, wherein the water scavenger is selected from the group consisting of epoxy resins and aluminosilicates.

12. The two-component polyurethane composition according to any one of claims 1 to 11, wherein the catalyst comprises an organometallic compound catalyst.

13. A two-component polyurethane composition according to any one of claims 1 to 12, wherein the component (f) comprises at least one substance selected from the group consisting of a crosslinker, a defoamer, a filler, a surfactant, a colorant, a pigment, a flame retardant, a stabilizer, a viscosity reducer, and substances having fungistatic and bacteriostatic effects.

14. A two-component polyurethane composition according to any one of claims 1 to 13, wherein the polyurethane composition has a solids content of 98 wt % or more, preferably 99 wt % or more, or more preferably 99.5 wt % or more according to GB / T 16777-2008. 15 . The two-component polyurethane composition according to claim 1 , wherein the component A and the component B are mixed in a weight ratio of 1:1 to 1.3, preferably 1:1 to 1.

2.

16. A method for preparing a gas barrier layer, comprising the following steps: Component A and component B of the two-component polyurethane composition according to any one of claims 1 to 15 are mixed together, and the mixture thus formed is subsequently cured.

17. The method according to claim 16, wherein the mixing of component A and component B is achieved by spraying.

18. Use of a two-component polyurethane composition according to any one of claims 1 to 15 for reducing vapor permeation in buildings with low indoor temperatures.

19. The use according to claim 18, wherein the low indoor temperature building is a refrigerated warehouse.

Citation Information

Patent Citations

  • High-vapor-barrier polyurethane coating for refrigeration house and preparation method of high-vapor-barrier polyurethane coating

    CN107903803A

  • Waterproof airproof film special for refrigeration storage construction industry, preparation method and mounting method thereof

    CN109177391A

  • Polyurethane dampproof vapor isolation paint for cold storage warehouse and preparation process thereof

    CN109810623A

  • Polyether alcohols and method for the production of polyether alcohols for polyurethane synthesis

    WO2005090440A1

  • Method for producing polyurethane soft foam materials

    WO2006034800A1