Polyethylene resin composition
By performing paddle polymerization under Ziegler-Natta catalyst, a polyethylene resin composition with a specific molecular structure is prepared, which solves the problem of insufficient heat resistance and shrinkage characteristics of polyethylene resin when making a stretched film, and realizes the Excellent tensile strength and transparency, suitable for the manufacture of biaxial tensile films.
Patent Information
- Application Number
- CN202380031910.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-12-20
- Filing Date
- 2023-12-22
- Publication Date
- 2024-11-15
AI Technical Summary
The existing polyethylene resins have problems with insufficient heat resistance and shrinkage characteristics when manufacturing the stretched film, and it is difficult to meet the application needs on the printing layer.
A polyethylene resin composition was developed to prepare polyethylene with a specific molecular weight distribution and short branched content by performing paddle polymerization of ethylene with C4 to C10α-olefin comonomer in the presence of Ziegler-Natta catalyst Vinyl resin meets the requirements of density, NCD index, molecular weight distribution and high crystalline fraction content.
The polyethylene resin composition significantly improves tensile strength, shrinkage characteristics and transparency, and is suitable for manufacturing biaxial tensile films that exhibit excellent tensileability and physical properties, solving the problem of insufficient heat resistance and shrinkage characteristics.
Smart Images

Figure CN118974162A_ABST
Abstract
Description
Technical Field
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0002] This application is based on and claims the benefit of priority of Korean Patent Application No. 10-2022-0189079 filed on December 29, 2022 and Korean Patent Application No. 10-2023-0187175 filed on December 20, 2023, respectively, the disclosures of which are hereby incorporated herein by reference in their entirety.
[0003] The present invention relates to a polyethylene resin composition having excellent stretchability and physical properties. Background Art
[0004] With recent consumer concerns about the environment, easily recyclable single-material packaging is gaining attention. Typically, in the food packaging and distribution industry, there is a trend to manufacture "all-PE" films using only the common material polyethylene (PE).
[0005] In the past, composite materials of BOPA, BOPET, BOPP, etc., with a printing layer applied, have been used for multilayer film packaging materials. In order to replace the composite materials with PE, they need higher physical properties than the existing PE blown films.
[0006] Meanwhile, a biaxially oriented polyethylene (BOPE) film is manufactured by stretching a cast sheet in the machine direction (MD) and the transverse direction (TD), and has significantly better tensile strength, impact strength, and transparency than existing blown films.
[0007] However, conventional development of BOPE resins focuses on linear low-density polyethylene (LLDPE) having excellent tensile properties due to low density. However, when LLDPE is used to manufacture BOPE films, there is a problem that it is difficult to apply it on a printed layer due to severe shrinkage and low heat resistance.
[0008] Therefore, research and development are required to prepare polyethylene or polyethylene resin compositions having higher density with improved heat resistance, shrinkage characteristics, tensile strength, and the like. Summary of the invention
[0009] [Technical issues]
[0010] In order to solve the problems of the prior art, a polyethylene resin composition is provided which exhibits excellent stretching characteristics when manufacturing a stretched film and is capable of improving the tensile strength, shrinkage characteristics and transparency of the stretched film.
[0011] Also provided is a stretched film produced using the polyethylene resin composition and exhibiting excellent tensile strength properties, shrinkage characteristics, and transparency.
[0012] [Technical solution]
[0013] In order to achieve the above object, a polyethylene resin composition satisfying the following requirements (a1) to (a6) is provided:
[0014] (a1) Density measured according to ASTM D792: 0.940 g / cm 3 Up to 0.965g / cm 3 ,
[0015] (a2) NCD index calculated according to the following equation 1: 0 or above,
[0016] (a3) In gel permeation chromatography analysis, when a molecular weight distribution curve is plotted with the logarithmic value (log M) of the weight average molecular weight (M) (g / mol) as the x-axis and the molecular weight distribution relative to the logarithmic value (dwt / dlog M) as the y-axis, the type of molecular weight distribution curve: bimodal,
[0017] (a4) in a temperature rising elution fractionation (TREF) analysis, the content of a highly crystalline fraction eluted at an elution temperature of 100° C. or higher, based on the total weight of all eluted fractions: 35% by weight or higher,
[0018] (a5) Z average molecular weight (Mz): 500000 g / mol to 800000 g / mol,
[0019] (a6) Number of SCBs per 1000 carbon atoms: greater than 3 and less than 8,
[0020] [Equation 1]
[0021] NCD index = - (SCB number per 1000 carbon atoms at logMw of 5.5 - SCB number per 1000 carbon atoms at logMw of 4.5)
[0022] In Equation 1, Mw represents a weight average molecular weight (g / mol), and SCB represents a short chain branch having 2 to 7 carbon atoms attached to a polyethylene main chain.
[0023] Also provided is a method for preparing the polyethylene resin composition, the method comprising a first step of preparing a first polyethylene by conducting a first slurry polymerization reaction of ethylene and a first C4 to C10 α-olefin comonomer in the presence of a Ziegler-Natta catalyst while introducing hydrogen in a first reactor; and a second step of transferring the first polyethylene to a second reactor connected to the first reactor, and then introducing only ethylene or ethylene and C4 to C10 α-olefin comonomers and conducting a second slurry polymerization reaction, wherein the input amount of the C4 to C10 α-olefin comonomer introduced in the first slurry polymerization reaction is greater than the input amount of the C4 to C10 α-olefin comonomer introduced in the second slurry polymerization reaction.
[0024] Also provided is a stretched film comprising the polyethylene resin composition, specifically a biaxially stretched film.
[0025] [Beneficial Effects]
[0026] According to the present invention, there is provided a polyethylene resin composition which exhibits excellent stretching characteristics when a stretched film is produced and which is capable of improving the tensile strength, shrinkage characteristics and transparency of the stretched film.
[0027] Also provided is a stretched film produced using the polyethylene resin composition and exhibiting excellent tensile strength properties, shrinkage characteristics, and transparency. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 This is a graph showing changes in loss modulus according to temperature observed in dynamic mechanical analysis (DMA) of the polyethylene resin compositions of Examples 3 and 6 and Comparative Example 1. DETAILED DESCRIPTION
[0029] As used herein, the terms “first”, “second”, etc. are used to describe various components, and these terms are only used to distinguish a certain component from other components.
[0030] In addition, the terms used in this specification are only used to illustrate exemplary embodiments and are not intended to limit the present invention. Singular expressions may include plural expressions unless there is a different expression in the context. It must be understood that in this specification, the terms "comprising", "equipped with", "having" are only used to specify the presence of effective features, numbers, steps, components or combinations thereof, and do not preclude the possibility of the presence or addition of more than one different feature, number, step, component or combination thereof.
[0031] Furthermore, throughout this specification, the term "polyethylene" or "ethylene polymer (ethylene copolymer)" includes an ethylene homopolymer and / or a copolymer of ethylene and an α-olefin.
[0032] The present invention can be modified in various ways and has various forms, and specific exemplary embodiments will be explained and described in detail as follows. However, it should be understood that this description is not intended to limit the present invention to the specific forms disclosed, but on the contrary, it is intended to cover all modifications, equivalents and substitutes that fall within the spirit and scope of the present invention.
[0033] Hereinafter, the polyethylene resin composition of the present invention will be described in detail.
[0034] The polyethylene resin composition of the present invention meets the following requirements (a1) to (a6):
[0035] (a1) Density measured according to ASTM D792: 0.940 g / cm 3 Up to 0.965g / cm 3 ,
[0036] (a2) NCD index calculated according to the following equation 1: 0 or above,
[0037] (a3) In gel permeation chromatography analysis, when a molecular weight distribution curve is plotted with the logarithmic value (log M) of the weight average molecular weight (M) (g / mol) as the x-axis and the molecular weight distribution relative to the logarithmic value (dwt / dlog M) as the y-axis, the type of molecular weight distribution curve: bimodal,
[0038] (a4) in a temperature rising elution fractionation (TREF) analysis, the content of a highly crystalline fraction eluted at an elution temperature of 100° C. or higher, based on the total weight of all eluted fractions: 35% by weight or higher,
[0039] (a5) Z average molecular weight (Mz): 500,000 g / mol to 800,000 g / mol,
[0040] (a6) Number of SCBs per 1000 carbon atoms: greater than 3 and less than 8,
[0041] [Equation 1]
[0042] NCD index = - (SCB number per 1000 carbon atoms at logMw of 5.5 - SCB number per 1000 carbon atoms at logMw of 4.5)
[0043] In Equation 1, Mw represents the weight average molecular weight (g / mol) of polyethylene, and SCB represents a short chain branch having 2 to 7 carbon atoms attached to a polyethylene main chain.
[0044] Generally, biaxially oriented polyethylene (BOPE) films are produced by stretching a cast sheet in the machine direction (MD) and the transverse direction (TD). As described, since biaxial stretching must proceed from MD stretching to TD stretching, polyethylene used for BOPE requires excellent stretchability.
[0045] In order to ensure the stretchability of polyethylene, there must be a structure that allows interlaminar lateral connection between lamellae in the polyethylene so that secondary crystallization occurs as late as possible in MD stretching, followed by TD stretching.
[0046] The present inventors found that as the content of SCB derived from the comonomer in the low molecular weight region of the polyethylene resin composition increases and the fluidity of the binding molecules between crystals increases, filament formation is suppressed during film stretching, so it can exhibit excellent stretchability and can be more conducive to stretching in the TD direction, and they completed the present invention by controlling the molecular structure within the polyethylene resin composition.
[0047] Furthermore, in the present invention, the molecular structure in which the content of SCB derived from the comonomer is high in the low molecular weight region as described above (ie, the normal comonomer distribution (NCD) structure) is parameterized by the NCD index as in Equation 1 and optimized to a range showing excellent stretchability.
[0048] Meanwhile, the NCD structure defined in the present invention is different from a broad orthogonal comonomer distribution (BOCD) structure in which the content of SCB derived from the comonomer is low in the low molecular weight region and the content of SCB derived from the comonomer is high in the high molecular weight region.
[0049] Specifically, the polyethylene resin composition of the present invention has an NCD index calculated according to Equation 1 of 0 or more.
[0050] When the NCD index is 0 or more (i.e., a positive value), the composition has an NCD structure in which the content of SCB derived from the comonomer in the low molecular weight region is high. On the contrary, when the NCD index is less than 0 (i.e., a negative value), the composition has a BOCD structure in which the content of SCB derived from the comonomer in the low molecular weight region is low and the content of SCB derived from the comonomer in the high molecular weight region is high. In addition, when the NCD index is less than 0 and the value is close to 0, the composition has a flat structure in which SCB is uniformly distributed.
[0051] When the NCD index is less than 0 (i.e., a negative value), it is not an NCD structure, and the larger the value, the more deteriorated the NCD characteristics. In this case, since the mobility and chain entanglement of low molecular weight tie molecules involved in microfibril formation are reduced during TD stretching after stretching in the MD direction, stretchability is deteriorated.
[0052] More specifically, the NCD index of the polyethylene resin composition of the present invention is 0 or more, or 0.5 or more, or 1 or more, or 1.5 or more, or 1.8 or more, or 1.82 or more, or 2 or more. On the contrary, when the NCD index exceeds 10, the density of the low molecular weight region is very low during the polymerization process, resulting in difficulty in manufacturing by a slurry process, or the average SCB content increases and the density decreases, resulting in deterioration of the tensile strength, shrinkage characteristics and heat resistance of the film. Therefore, the NCD index of the polyethylene resin composition may be 10 or less, or 8 or less, or 6 or less, or 5 or less, or 4 or less, or 3.9 or less, or 3 or less.
[0053] In the present invention, as defined in Equation 1, the NCD index of the polyethylene resin composition is calculated using the number of SCBs per 1000 carbon atoms at log Mw = 5.5 and the number of SCBs per 1000 carbon atoms at log Mw = 4.5, and these values can be obtained by GPC and FT-IR analysis of the polyethylene resin composition.
[0054] Specifically, the molecular weight distribution according to each molecular weight and the number of SCB (short chain branches, side chains having 2 to 7 carbon atoms per 1000 carbon atoms) can be determined by GPC and FT-IR analysis of the polyethylene resin composition. The detailed measurement method and measurement conditions are described in detail in the experimental examples.
[0055] Furthermore, in GPC analysis, the polyethylene resin composition has a bimodal molecular weight distribution curve in a molecular weight distribution curve having a logarithmic value (logM) of the weight average molecular weight (M) (g / mol) as the x-axis and a molecular weight distribution relative to the logarithmic value (dwt / dlog M) as the y-axis.
[0056] In the present invention, a bimodal molecular weight distribution curve means that the molecular weight distribution curve has two peaks on the GPC graph. In this regard, the peak also includes the case where the two peaks have independent peak shapes and do not exist independently, but partially overlap and exist as a shoulder peak with no minimum value between the maximum values of the two peaks. In other words, when it is not interpreted as a single peak forming a normal distribution and can be deconvoluted into two distributions, it can be defined as a bimodal structure.
[0057] Such a bimodal molecular weight distribution indicates that the low molecular weight and high molecular weight distribution in the polyethylene resin composition are increased. Due to such a molecular weight distribution structure, the polyethylene resin composition can show improved physical properties compared to a polyethylene resin composition showing a unimodal molecular weight distribution, and in particular, can enhance the molecular structure morphology that is conducive to biaxial stretching, thereby showing better stretchability.
[0058] Furthermore, in the TREF analysis of the polyethylene resin composition, the content of the high crystalline fraction eluted at an elution temperature of 100° C. or higher is 35% by weight or higher based on the total weight of all eluted fractions.
[0059] Since the content of the high crystalline fraction is high, the polyethylene resin composition can exhibit excellent stiffness and heat resistance when manufacturing a stretched film. More specifically, in a TREF analysis of the polyethylene resin composition, the content of the high crystalline fraction eluted at an elution temperature of 100° C. or higher may be 35% by weight or higher, or 38% by weight or higher, or 38.2% by weight or higher, or 40% by weight or higher, and may be 50% by weight or lower, or 49.5% by weight or lower, or 46% by weight or lower, based on the total weight of all eluted fractions.
[0060] Meanwhile, for the polyethylene resin composition, the content ratio of the high crystalline fraction eluted at an elution temperature of 100°C or higher is obtained as follows: a TREF analysis curve with elution temperature (Te) (°C) as the x-axis and elution amount (dw / dt) as the y-axis is obtained from the TREF analysis results, and from the TREF analysis curve, the weight ratio of the high crystalline fraction eluted at an elution temperature of 100°C or higher is calculated based on the total weight of all eluted fractions (high crystalline fraction, T≥100°C).
[0061] In addition, in the present invention, TREF analysis of the polyethylene resin composition can be performed using a TREF device of PolymerChar in a temperature range of -20°C to 130°C and using trichlorobenzene as a solvent. For example, in the present invention, the cooling rate in the crystallization step during the TREF analysis is set to 0.1°C / min. The detailed analysis method and conditions are described in detail in the following experimental examples.
[0062] In addition, the polyethylene resin composition has a Z average molecular weight (Mz) of 500,000 g / mol to 800,000 g / mol.
[0063] Among the various molecular weights representing the polyethylene resin composition, the Z average molecular weight represents the content of the area of the tail corresponding to the high molecular weight side in the molecular weight distribution curve, i.e., the fraction (weight %) of the high molecular weight tail relative to the total weight of the polyethylene resin composition. By having an Mz within the above range, the polyethylene resin composition of the present invention can show better biaxial stretchability. When Mz is less than 500,000 g / mol, the content of the high molecular weight tail is low, and there is a risk of rupture when stretched in the MD direction. When Mz is greater than 800,000 g / mol, too many ultra-high molecular weight chains form unmelted gels, which may become defects during stretching. More specifically, the Mz of the polyethylene resin composition can be 500,000 g / mol or more, or 550,000 g / mol or more, or 560,000 g / mol or more, or 570,000 g / mol or more, or 600,000 g / mol or more, or greater than 600,000 g / mol, or 605,000 g / mol or more, 800,000 g / mol or less, or 700,000 g / mol or less, or 650,000 g / mol or less, or 637,000 g / mol or less, or 636,600 g / mol or less.
[0064] Meanwhile, the Z average molecular weight (Mz) of the polyethylene resin composition is a value converted into standard polystyrene measured by gel permeation chromatography analysis. The GPC analysis method and measurement conditions for measuring the Z average molecular weight are as described in the following experimental examples.
[0065] Furthermore, the polyethylene resin composition has an SCB number of more than 3 and 8 per 1000 carbon atoms.
[0066] For polyethylene resin compositions, the number of SCBs per 1000 carbon atoms affects the crystallinity and crystal distribution of the composition. Therefore, when the number of SCBs is less than 3, due to the high crystallinity and low content of low crystals, stretchability may deteriorate, and when the number of SCBs is greater than 8, the crystallinity may be excessively reduced, and the tensile strength, shrinkage characteristics and heat resistance of the film may deteriorate. In addition, when a polyethylene resin composition having an SCB content greater than 8 is prepared by a slurry polymerization process as in the present invention, it is difficult to prepare due to process instability factors such as scaling in terms of the basic characteristics of the slurry process. More specifically, the number of SCBs per 1000 carbon atoms can be greater than 3, or more than 3.1, or more than 3.2, or more than 3.3, or more than 3.5, less than 8, or less than 7.9, or less than 7.
[0067] In the present invention, short chain branching (SCB) refers to a branched short chain connected to the polyethylene main chain, specifically a short chain branch having 2 to 7 carbon atoms connected to the polyethylene main chain. SCB is a short chain branch usually formed when α-olefins having more than 4 carbon atoms such as 1-butene, 1-hexene and 1-octene are used as comonomers, and its content can be proportional to the content of α-olefin monomers contained in the polymer chain. The SCB content refers to the number of branches having 2 to 7 carbon atoms per 1000 carbon atoms (unit: branch / 1,000C), and can be measured by using proton nuclear magnetic resonance ( 1 In the present invention, the SCB content is determined by FT-IR analysis, and the detailed analysis method is described in detail in the following experimental examples.
[0068] In addition, the polyethylene resin composition of the present invention has a 3 Up to 0.965g / cm 3 Therefore, it can show excellent strength properties. More specifically, the density of the polyethylene resin composition can be 0.940 g / cm 3 Above or greater than 0.940g / cm 3 , 0.945g / cm 3 Above, or 0.946g / cm 3 Above, or 0.947g / cm 3 Above, or 0.949g / cm 3 Above, or 0.950g / cm 3 Above, 0.965g / cm 3 Below, or less than 0.960g / cm 3 , or 0.955g / cm 3 Below, or 0.954g / cm 3 Below, or 0.952g / cm 3 the following.
[0069] Meanwhile, the density of the polyethylene resin composition is a value measured according to ASTM D792 standard.
[0070] Furthermore, in dynamic mechanical analysis (DMA), the polyethylene resin composition of the present invention shows a peak (β relaxation peak) at -40°C to 10°C in a graph of loss modulus according to temperature.
[0071] The β relaxation peak appearing at −40 °C to 10 °C is the result of polymer chain movement between lamellar crystals, and the increased fluidity can manifest as excellent stretchability when making films.
[0072] In addition to the above physical property requirements, the polyethylene resin composition of the present invention may also meet one or more, two or more, or all five of the following requirements (b1) to (b5):
[0073] (b1) Melt index (MI) measured at 190°C under a load of 2.16 kg 2.16 ): 0.5g / 10min to 3.0g / 10min,
[0074] (b2) MFRR [5 / 2.16]: 3 to 5,
[0075] (b3) weight average molecular weight (Mw): 80,000 g / mol to 130,000 g / mol,
[0076] (b4) number average molecular weight (Mn): 5,000 g / mol to 15,000 g / mol, and
[0077] (b5) Polydispersity index [Mw / Mn]: 8 to 20.
[0078] Specifically, the polyethylene resin composition of the present invention has a melt index (MI) measured at 190° C. under a load of 2.16 kg according to ASTM D1238. 2.16 ) may be 0.5 g / 10 min or more and 3.0 g / 10 min or less. More specifically, the melt index (MI 2.16 ) can be 0.5g / 10min or more, or 1g / 10min or more, or greater than 1g / 10min, or 1.2g / 10min or more, or 1.21g / 10min or more, or 1.25g / 10min or more, or 1.28g / 10min or more, or 1.3g / 10min or more, and can be 3.0g / 10min or less, or 2.5g / 10min or less, or 2.0g / 10min or less, or 1.5g / 10min or less, or 1.49g / 10min or less, or 1.45g / 10min or less.
[0079] In addition, the MFRR (MI5 / MI 2.16 ) may be 3 or more and 5 or less, which is obtained by dividing the melt index (MI5) measured at a temperature of 190° C. under a load of 5 kg according to ASTM D1238 by the melt index (MI5) measured at a temperature of 190° C. under a load of 2.16 kg. 2.16 ) ratio. More specifically, MFRR (MI5 / MI 2.16) can be 3 or more, or 3.5 or more, or 3.9 or more, or 3.91 or more, or 4 or more, 5 or less, or 4.8 or less, or 4.5 or less, or 4.45 or less, or 4.43 or less, or 4.3 or less.
[0080] In addition, the weight average molecular weight (Mw) of the polyethylene resin composition may be 80,000 g / mol or more and 130,000 g / mol or less. More specifically, the weight average molecular weight (Mw) may be 80,000 g / mol or more, or 90,000 g / mol or more, or 95,000 g / mol or more, or 98,000 g / mol or more, or 100,000 g / mol or more, and may be 130,000 g / mol or less, or 120,000 g / mol or less, or 110,000 g / mol or less, or 109,600 g / mol or less, or 109,000 g / mol or less.
[0081] In addition, the polyethylene resin composition may have a number average molecular weight (Mn) of 5,000 g / mol or more and less than 11,000 g / mol.
[0082] The number average molecular weight of the polyethylene resin composition affects the stretchability and physical properties of the resin composition. When the number average molecular weight is 11,000 g / mol or more, the stretchability may be deteriorated when manufacturing a film, and when the number average molecular weight is less than 5,000 g / mol, the physical properties such as stiffness of the manufactured film may be deteriorated.
[0083] Therefore, the number average molecular weight (Mn) of the polyethylene resin composition may be more specifically 5,000 g / mol or more, or 5,500 g / mol or more, or 5,800 g / mol or more, or 6,000 g / mol or more, and may be less than 11,000 g / mol, or 10,500 g / mol or less, or 10,000 g / mol or less.
[0084] Furthermore, the polydispersity index [Mw / Mn] of the polyethylene resin composition may be 8 or more and 20 or less. More specifically, the polydispersity index may be 8 or more, or 10 or more, or 10.4 or more, or 11 or more, and may be 20 or less, or 17 or less, or 16.8 or less, or 15 or less.
[0085] Meanwhile, in the present invention, the weight average molecular weight (Mw) and number average molecular weight (Mn) of the polyethylene resin composition can be determined by gel permeation chromatography (GPC) analysis, and each is a value converted to standard polystyrene. In addition, the polydispersity index of the polyethylene resin composition can be calculated by dividing the weight average molecular weight (Mw) determined above by the number average molecular weight (Mn). The detailed measurement method and conditions are described in the following experimental examples.
[0086] The polyethylene resin composition of the present invention satisfies all the above physical property requirements, and thus exhibits excellent stretchability and physical properties. As a result, when manufacturing a biaxially stretched film, there is no need to worry about defects such as breakage and shrinkage during stretching in the TD direction, and the manufactured biaxially stretched film can exhibit excellent stretch ratio characteristics and tensile strength characteristics.
[0087] Furthermore, the polyethylene resin composition of the present invention specifically includes an ethylene / C4 to C10 α-olefin copolymer.
[0088] Specific examples of the C4 to C10 α-olefin monomers may include 1-butene, 1-pentene, 4-methyl-1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tetradecene, 1-hexadecene, 1-eicosene, and the like, and two or more thereof may be used.
[0089] The ethylene / C4 to C10 α-olefin copolymer is specifically an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer or an ethylene / 1-butene / 1-octene copolymer.
[0090] Meanwhile, the polyethylene resin composition of the present invention as described above may be prepared by slurry polymerization using a plurality of reactors.
[0091] For example, the polyethylene resin composition can be prepared by a preparation method comprising:
[0092] a first step of preparing a first polyethylene by conducting a first slurry polymerization of ethylene and a first comonomer of C4 to C10 alpha olefins in the presence of a Ziegler-Natta catalyst in a first reactor while introducing hydrogen; and
[0093] The first polyethylene is transferred to a second reactor connected to the first reactor, and then only ethylene or ethylene and a C4 to C10 alpha-olefin second comonomer are introduced and a second slurry polymerization is carried out in a second step,
[0094] The input amount of the first comonomer of C4 to C10 α-olefin introduced in the first slurry polymerization reaction is greater than the input amount of the second comonomer of C4 to C10 α-olefin introduced in the second slurry polymerization reaction.
[0095] In the preparation method of the present invention, a Ziegler-Natta polymerization catalyst is used, which is conducive to forming a wide molecular weight distribution when a polyethylene resin composition is prepared by a multimodal polymerization process using multiple reactors, and a slurry polymerization process is also used, which produces an ultra-high molecular weight tail in the GPC molecular weight distribution curve to form a wider molecular weight distribution, and the input amount of the comonomer introduced into the first and second reactors is controlled, so that the prepared polyethylene resin composition meets all the physical property requirements of (a1) to (a6), and as a result, exhibits excellent stretchability. In particular, when the input amount of the comonomer in the first polymerization reactor is higher than its input amount in the second polymerization reactor, the SCB content increases, which is a structure derived from the comonomer in the low molecular weight region of the prepared polyethylene resin composition, and the fluidity of the binding molecules between crystals increases. As a result, filament formation is suppressed during the stretching process, so it can exhibit excellent stretchability, and in particular, it can be more conducive to stretching in the TD direction.
[0096] The method for preparing the polyethylene resin composition of the present invention is carried out by multimodal slurry polymerization using multiple reactors. More specifically, two or more reactors may be used, for example, two or more continuous stirred tank reactors (CSTR).
[0097] In addition, for the preparation method, a first reactor in which a first slurry polymerization reaction for preparing a first polyethylene occurs and a second reactor connected to the first reactor and in which a second slurry polymerization reaction for preparing a second polyethylene occurs may be used. Therefore, in the second reactor, the first polyethylene transferred from the first reactor is further polymerized with ethylene, or ethylene and a C4 to C10 α-olefin second comonomer introduced into the second reactor, thereby forming an ethylene / α-olefin copolymer.
[0098] Furthermore, for the preparation method, the polymerization process in the first and second reactors is performed by a slurry polymerization process.
[0099] In solution polymerization, since the catalyst is activated by high temperature and high pressure reaction, catalyst decomposition and chain transfer are promoted, and the molecular weight distribution (MWD) of the obtained resin composition is narrow and the content of high molecular weight tail is low. Therefore, when the resin composition prepared by solution polymerization is used to make a film, it exhibits degraded stretchability, especially when stretched in the MD direction, it breaks. On the contrary, in the slurry polymerization process of the present invention, polymerization is carried out at a relatively low temperature, therefore, it is possible to ensure the molecular structure with wide MWD and containing a large amount of high molecular weight tails required for the polyethylene resin composition for the production of transparent film. As a result, the composition can exhibit excellent biaxial stretchability.
[0100] In addition, for the preparation method of the present invention, only ethylene can be introduced without inputting comonomers during the second slurry polymerization reaction, or the input amount of the first comonomer introduced into the first slurry polymerization reaction can be greater than the input amount of the second comonomer introduced into the second slurry polymerization reaction. In this case, an NCD structure with a high SCB content derived from the comonomer in the low molecular weight region and a bimodal molecular weight distribution can be achieved. Since the SCB content is high in the low molecular weight region, the mobility of the tethered molecules between crystals increases, and as a result, filament formation is suppressed during the stretching process, which can be more conducive to stretching in the TD direction.
[0101] Specifically, the weight ratio of the second comonomer introduced in the second slurry polymerization process to the first comonomer introduced in the first slurry polymerization process (the weight of the second comonomer introduced in the second slurry polymerization process / the weight of the first comonomer introduced in the first slurry polymerization process) can be greater than 0 and less than 1. When the weight ratio of the comonomers is greater than 1, a polyethylene resin composition that meets the above-mentioned physical property requirements (especially the NCD index requirements) cannot be prepared. More specifically, the weight ratio of the comonomers is 0 (only ethylene monomer is introduced without comonomers in the second slurry polymerization process) or the weight ratio can be greater than 0, or greater than 0.01, or greater than 0.05, or greater than 0.09, or greater than 0.1, and can be less than 1, or less than 0.5, or less than 0.4, or less than 0.35, or less than 0.3.
[0102] In addition, the total amount of ethylene and the total amount of comonomer introduced into the first and second reactors may satisfy a weight ratio of 1:0.001 to 1:0.1, more specifically, the weight ratio may be 1:0.02 to 1:0.1, or 1:0.02 to 1:0.06, or 1:0.02 to 1:0.055. When the total amount of ethylene and the total amount of comonomer introduced into the first and second reactors satisfy the above weight ratio range, the physical properties of the above polyethylene resin composition may be more easily achieved.
[0103] In addition, for the preparation method of the polyethylene resin composition of the present invention, the polymerization temperature (T1) and pressure (P1) in the first slurry polymerization process are higher than the polymerization temperature (T2) and pressure (P2) in the second slurry polymerization process. In addition to controlling the input amount of the comonomer, by further increasing the temperature and pressure conditions in the first slurry polymerization process, the bimodal molecular weight distribution and NCD structure in the polyethylene resin composition can be more easily achieved.
[0104] Specifically, the difference (T1-T2) between the polymerization temperature (T1) during the first slurry polymerization reaction and the polymerization temperature (T2) during the second slurry polymerization reaction can be above 3°C, or above 4°C, or above 5°C, and can be below 10°C, or below 8°C, or below 6°C.
[0105] In addition, the difference (P1-P2) between the pressure (P1) during the first slurry polymerization reaction and the pressure (P2) during the second slurry polymerization reaction may be 2 kgf / cm 2 Above, or 3kgf / cm 2 Above, or 3.2kgf / cm 2 Above, and can be 6kgf / cm 2 Below, or 5.5kgf / cm 2 Below, or 5.3kgf / cm 2 the following.
[0106] In addition, in the preparation method of the present invention, while satisfying the above-mentioned temperature difference and pressure difference, the polymerization temperature (T1) in the first slurry polymerization process is 70°C to 90°C, and the polymerization temperature (T2) in the second slurry polymerization process is 70°C to 90°C.
[0107] In addition, the pressure (P1) during the first slurry polymerization reaction was 5 kgf / cm 2 Up to 10kgf / cm 2 , and the pressure (P2) during the second slurry polymerization reaction can be 1 kgf / cm 2 Up to 5kgf / cm 2 .
[0108] Hereinafter, each step will be described in detail.
[0109] In the preparation method of the polyethylene resin composition of the present invention, the first step is to prepare a first polyethylene by conducting a first slurry polymerization reaction of ethylene and a first C4 to C10 α-olefin comonomer in a first reactor while introducing hydrogen in the presence of a Ziegler-Natta catalyst.
[0110] The Ziegler-Natta catalyst used to prepare the first polyethylene may specifically be a magnesium-supported titanium catalyst. In addition, the magnesium-supported titanium catalyst may further contain a halogenated hydrocarbon.
[0111] Specifically, the magnesium-supported titanium catalyst comprises a solid magnesium carrier. Examples of magnesium carriers may include magnesium, magnesium oxide, magnesium chloride, silicon dioxide-magnesium oxide, magnesium oxide, etc., and any one thereof or a mixture of two or more thereof may be used. Wherein, in view of catalytic activity and the physical properties that are easy to achieve the best polyethylene resin composition, the magnesium carrier may be magnesium.
[0112] Meanwhile, the magnesium-supported titanium catalyst comprises a titanium-containing compound represented by the following chemical formula (1) as a main catalyst:
[0113] [Chemical formula 1]
[0114] Ti(OR 1 ) m X 1 4-m
[0115] In Chemical Formula 1,
[0116] R 1 are the same or different and are alkyl groups having 1 to 10 carbon atoms,
[0117] X 1 is a halogen atom, more specifically Cl, Br or I, and
[0118] m is an integer of 0-4.
[0119] In Chemical Formula 1, R 1 Specifically, it may be an alkyl group having 1 or more, 2 or more, or 3 or more carbon atoms and 10 or less, 8 or less, or 5 or less carbon atoms.
[0120] In addition, you can 1 Specifically, Br or Cl, and more specifically, Cl.
[0121] Specific examples of the titanium-containing compound may include titanium tetrachloride (TiCl 4 ) or titanium oxychloride, and any one of them or a mixture of both may be used.
[0122] In addition, based on the content of Mg in the magnesium support and the content of Ti in the titanium-containing compound, the catalyst containing the titanium-containing compound contains Mg:Ti in a molar ratio of 1:1 to 10:1, or 2:1 to 7:1, or 4:1 to 5:1. When contained within the above molar ratio range, excellent catalytic activity can be achieved.
[0123] Furthermore, the shape of the catalyst is not particularly limited but may be, for example, in the form of spherical fine particles.
[0124] Furthermore, the average particle size of the catalyst may be 5 μm to 100 μm, more specifically 5 μm or more, 8 μm or more, or 10 μm or more, and may be 100 μm or less, 50 μm or less, 20 μm or less, or 13 μm or less.
[0125] Meanwhile, the average particle size of the catalyst in the present invention can be measured by scanning electron microscopy (SEM) observation. Specifically, after obtaining an SEM image of more than 100 catalyst particles, random straight lines are drawn, and the average size of the catalyst particles can be calculated from the length of the corresponding straight line, the number of particles contained in the straight line, and the magnification.
[0126] In addition, the magnesium-supported titanium catalyst may further contain a halogenated hydrocarbon.
[0127] The halogenated hydrocarbons change the electrical properties of titanium by coordinating around titanium as active sites, and a large amount of halogenated hydrocarbons create ample three-dimensional space between titanium atoms, thereby greatly improving the catalytic activity during polyethylene polymerization.
[0128] The halogenated hydrocarbon may specifically be an alkane having 1 to 12 carbon atoms, a cycloalkane having 3 to 12 carbon atoms, an alkene having 2 to 12 carbon atoms, an alkyne having 2 to 12 carbon atoms, or an aromatic hydrocarbon having 6 to 30 carbon atoms substituted with one or more halogen groups. The halogen group may be fluorine, chlorine or bromine.
[0129] Specific examples may include bromoform, tetrachloroethane, hexachloroethane, pentachloroethane, 1,1,2,2-tetrachloroethane, 1-bromo-1-chloroethane, 1,2-dibromoethane, 1,2-dichloroethane, ethyl bromide, hexachloropropane, 1,2,3-trichloropropane, 1,2-dichloropropane, 1-chloropropane, 2-chloropropane, chlorobutane, dichlorobutane, 1-chloro-2-methylpropane, n-butyl chloride, tert-butyl chloride, 1-chloro-3-methylbutane, 1-chloropentane, 1,5-dichloropentane, bromopropane, Pentane, neopentyl chloride, 1-chloroheptane, cyclopropyl bromide, cyclobutyl chloride, cyclohexyl chloride, cyclohexyl bromide, vinylidene chloride, 1,2,3,3-tetrachloropropene, 1,2-dibromo-1-propene, 1,3-dichloropropene, hexachloro-1,3-butadiene, 2-bromo-2-butene, propargyl chloride, chlorobenzene, tetrachlorobenzene, trichlorobenzene, dichlorobenzene, 4-chlorobenzyl chloride, benzyl chloride, or 1,1-dichloro-2-phenylcyclopropane, and one of them or a mixture of two or more thereof may be used.
[0130] Based on 1 mol of the titanium-containing compound as the main catalyst, the content of the halogenated hydrocarbon can be more than 0.1 mol, or more than 0.12 mol, or more than 0.13 mol, and can be less than 500 mol, or less than 100 mol, or less than 50 mol, or less than 10 mol, or less than 1 mol, or less than 0.5 mol.
[0131] The Ziegler-Natta catalyst can be prepared by a preparation method including: a carrier treatment step of mixing and reacting the raw material of the magnesium carrier with an alcohol; and a titanium-containing compound loading step of reacting the product obtained by the above step with a titanium-containing compound represented by Chemical Formula 1, and further including a step of contacting and reacting with a halogenated hydrocarbon in the carrier treatment step or the titanium-containing compound loading step or after the titanium-containing compound loading step. Therefore, before the first step, the preparation method of the polyethylene resin composition of the present invention includes a step of preparing a Ziegler-Natta catalyst, specifically, including a carrier treatment step and a titanium-containing compound loading step, and may further include a step of contacting and reacting with a halogenated hydrocarbon in the carrier treatment step or the titanium-containing compound loading step or after the titanium-containing compound loading step.
[0132] Specifically, the support treatment step for preparing the Ziegler-Natta catalyst may be performed by mixing and reacting a raw material of the magnesium support with an alcohol in a non-polar solvent.
[0133] Specific examples of alcohols may include methanol, ethanol, 1-propanol, isopropanol, n-butanol, isobutanol, 1-pentanol, isopentanol, n-hexanol, 1-octanol, 2-ethyl-1-hexanol, etc., and one or a mixture of two or more thereof may be used. Among them, ethanol or 2-ethyl-1-hexanol may be used.
[0134] The amount of the alcohol used may be 1 mol or more, or 1.5 mol or more, or 2 mol or more, and may be 10 mol or less, or 8 mol or less, or 6 mol or less, based on 1 mol of the raw material of the magnesium carrier.
[0135] Meanwhile, the raw material of the magnesium support may include the magnesium support itself, such as magnesium, magnesium oxide, magnesium chloride or silica-magnesium oxide, etc., or a magnesium alcoholate such as magnesium ethoxide, and one or a mixture of two or more thereof may be used. For example, when magnesium alcoholate is used as the raw material of the magnesium support, it is converted into magnesium chloride by titanium tetrachloride (TiCl4) introduced as a main catalyst, and is included in the catalyst finally prepared as a support.
[0136] The method of mixing the raw material of the magnesium support with alcohol can be specifically performed as follows: the alcohol is added to a slurry prepared by mixing the raw material of the magnesium support with a non-polar solvent such as hexane, or a solution obtained by dissolving the alcohol in a non-polar solvent is added to the slurry, and then the solution is stirred at a temperature of 20° C. to 150° C. until it becomes a transparent solution. As a result of the above mixing, a homogeneous solution of the magnesium support is obtained, and in the solution, an adduct in which the crystals of the magnesium support are surrounded by the alcohol molecules is formed.
[0137] Next, the titanium-containing compound supporting step for preparing the Ziegler-Natta catalyst is performed by reacting the reaction product of the magnesium support and alcohol produced in the support treatment step with a titanium-containing compound.
[0138] Specifically, a titanium compound or a solution of a titanium compound dissolved in a nonpolar solvent is directly added to the reaction product of the magnesium support and alcohol generated in the support treatment step, and reacted at -50°C to 120°C or -20°C to 80°C.
[0139] The type and content of the titanium-containing compound are as described above.
[0140] Furthermore, when the titanium-containing compound is introduced, the reaction product of the magnesium support and the alcohol generated in the support treatment step may be stirred at 10 rpm to 500 rpm, or 50 rpm to 400 rpm.
[0141] Meanwhile, when preparing the Ziegler-Natta catalyst, the halogenated hydrocarbon is introduced when adding alcohol to the magnesium support in the support treatment step; the halogenated hydrocarbon is introduced when introducing the titanium-containing compound in the titanium-containing compound loading step; or after completing the step of loading the titanium-containing compound, a step of adding the halogenated hydrocarbon and reacting can be further performed.
[0142] The type and content of the halogenated hydrocarbon are as described above.
[0143] The Ziegler-Natta catalyst prepared by the above preparation method can be used as it is in the polyethylene polymerization process, or can be used as a slurry in a non-polar solvent.
[0144] In addition, the Ziegler-Natta catalyst may be used together with an organic metal compound represented by the following Chemical Formula 2 as a co-catalyst:
[0145] [Chemical formula 2]
[0146] R 2 n MX 2 (3-n)
[0147] In chemical formula 2,
[0148] M is selected from the group consisting of elements of Groups IB, IIA, IIIB and IVB of the Periodic Table,
[0149] R 2 are the same or different and are alkyl groups having 1 to 10 carbon atoms,
[0150] X 2 is a halogen, and
[0151] n is an integer of 1 to 3.
[0152] In Chemical Formula 2, M is specifically aluminum, R 2 is an alkyl group having 1 to 5 carbon atoms or 2 to 4 carbon atoms, and X 2 It is Cl or Br.
[0153] Specific examples of the organometallic compound represented by Chemical Formula 2 may include triethylaluminum, methylaluminum dichloride, methylaluminum dibromide, dimethylaluminum chloride, dimethylaluminum bromide, propylaluminum dichloride, propylaluminum dibromide, butylaluminum dichloride, butylaluminum dibromide, dibutylaluminum chloride, dibutylaluminum bromide, isobutylaluminum dichloride, isobutylaluminum dibromide, diisobutylaluminum chloride, diisobutylaluminum bromide, hexylaluminum dichloride, hexylaluminum dibromide, dihexylaluminum chloride, dihexylaluminum bromide, octylaluminum dichloride, octylaluminum dibromide, dioctylaluminum chloride, and dioctylaluminum bromide, and any one of them or a mixture of two or more thereof may be used.
[0154] At the same time, since the co-catalyst affects the polymerization activity of the magnesium-supported catalyst, the polymerization activity of the catalyst can be further improved by controlling the content of the co-catalyst. For example, for the organic metal compound represented by Chemical Formula 2, the amount of aluminum used can be 3 mol or more, or 10 mol or more, or 25 mol or more, and can be 200 mol or less, or 100 mol or less, relative to 1 mol of titanium in the catalyst.
[0155] The cocatalyst can be added to the polyethylene polymerization reaction after mixing with the Ziegler-Natta catalyst, or can be added separately before or after adding the Ziegler-Natta catalyst. Therefore, the preparation method of the polyethylene resin composition of the present invention can also include the step of adding the cocatalyst when preparing the first polyethylene in the first step.
[0156] Meanwhile, the polymerization reaction in the first step is a copolymerization reaction of ethylene and α-olefin, and the input amount of the comonomer can be determined in consideration of the physical properties to be achieved by the first polyethylene and the final polyethylene resin composition. For example, in the present invention, the content of the α-olefin first comonomer introduced into the first reactor can be 0.01 wt % to 5 wt % based on the total weight of the ethylene introduced into the first reactor. When introduced within the above content range, the comprehensive physical properties of the above-mentioned polyethylene resin composition can be easily achieved, and as a result, the increase in the stretch ratio in the TD direction can be achieved due to the increase in the low molecular weight and low crystalline content ratio.
[0157] Furthermore, the polymerization reaction in the first step is carried out under the condition of introducing hydrogen.
[0158] Since the input amount of hydrogen affects the physical properties of the copolymer prepared, the input amount is appropriately determined according to the physical properties to be achieved. For example, in the present invention, based on the gross weight of the monomers including ethylene and α-olefins introduced into the first and second reactors, the input amount of hydrogen can be 0.001 wt % to 0.5 wt %. When hydrogen is introduced within the above range, the comprehensive physical properties of the above-mentioned polyethylene resin composition can be easily achieved. More specifically, the introduction amount of hydrogen can be more than 0.001 wt %, or more than 0.01 wt %, or more than 0.05 wt %, or more than 0.07 wt %, and can be less than 0.5 wt %, or less than 0.3 wt %, or less than 0.1 wt %.
[0159] Furthermore, during the polymerization reaction in the first step, the temperature and pressure conditions are as defined above.
[0160] The first polyethylene is prepared by a polymerization reaction under the above preparation conditions.
[0161] Next, the second step is carried out in a second reactor connected to the first reactor.
[0162] Specifically, the first polyethylene prepared in the first step is transferred to a second reactor connected to the first reactor, ethylene and a C4 to C10 α-olefin second comonomer are introduced, and a second slurry polymerization reaction is performed.
[0163] In the second reactor, an additional polymerization reaction occurs between the first polyethylene transferred from the first reactor and the ethylene or C4 to C10 alpha-olefin second comonomer introduced into the second reactor.
[0164] The second slurry polymerization reaction may be carried out in the presence of a catalyst.
[0165] In this case, the catalyst that can be used is the Ziegler-Natta catalyst as described in step 1. Therefore, the Ziegler-Natta catalysts used for the first and second slurry polymerization reactions may be the same or different from each other. When the same Ziegler-Natta catalyst is used in the first and second slurry polymerization reactions, it is easier to control the physical properties of the polyethylene resin composition to be prepared, thereby achieving the above physical property requirements.
[0166] In addition, the second slurry polymerization reaction can be carried out with or without adding hydrogen. For example, when hydrogen is added, the amount of hydrogen added can be 0.001 wt % to 0.05 wt % based on the total weight of the monomers including ethylene and α-olefin introduced into the second reactor.
[0167] Furthermore, during the polymerization reaction in the second step, the temperature and pressure conditions are as defined above.
[0168] Meanwhile, the preparation method of the present invention may further include a step of melting and extruding the obtained polymerization product after completing the polymerization reaction in the second step.
[0169] The pellet-type polyethylene resin composition can be prepared through the above melting and extrusion steps.
[0170] Since the polymer product after the polymerization reaction in the second step is obtained in the form of powder, the types of available antioxidants are limited. In addition, since the content of the antioxidant varies greatly depending on the powder, the articles manufactured using the polymer product vary greatly in their physical properties. In contrast, when the melting and extrusion process is performed, the components including the antioxidant are uniformly mixed, and the resulting article can have uniform physical properties.
[0171] Meanwhile, as used herein, pellets or pellet-types are small particles or small pieces formed by extrusion of raw materials, and include all shapes defined as pellets in the art, including round, flat, thin-sheet, polygonal, rod-shaped, etc. The size of the pellets is appropriately determined according to the use and shape, and is not specifically limited, but the pellets in the present invention are defined as having an average diameter of 2 mm or more, thereby distinguishing from powders having a small average diameter of about 1 mm. In this regard, the "diameter" is the longest distance in any straight-line distance of the outer peripheral surface of the pellets, and can be measured using an imaging microscope, etc.
[0172] The melt extrusion process can be performed using a conventional extruder, and the specific method and conditions are not particularly limited as long as the morphological conditions of the pellets are met.
[0173] In addition, during the melt extrusion process, one or more additives such as antioxidants, neutralizers, slip agents, anti-caking agents, UV stabilizers, antistatic agents, etc. may be added. Therefore, the prepared polyethylene resin composition may further contain one or more additives, such as antioxidants, neutralizers, slip agents, anti-caking agents, UV stabilizers, and antistatic agents, etc. At the same time, in the present invention, the additives do not affect the physical properties of the polyethylene resin composition, and when the resin composition is used to manufacture an article, the processability and quality of the manufactured article can be improved.
[0174] For example, the antioxidant may include phenolic antioxidants; phosphorus antioxidants; amine antioxidants, etc., and any one of them or a mixture of two or more thereof may be used. Specific examples of the antioxidant may include phenolic antioxidants, such as pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] or 1,3,5-trimethyl-2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, etc.; phosphorus antioxidants, such as tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, and bis(2,4-diisopropylphenylphenyl)pentaerythritol diphosphite, etc.; or amine antioxidants, such as phenylnaphthylamine, 4,4'-(α,α-dimethylbenzyl)diphenylamine, and N,N'-di-2-naphthyl-p-phenylenediamine, etc., and any one of them or a mixture of two or more thereof may be used. In addition, commercially available Irganox can be used TM 1010 (manufactured by BASF), Irganox TM 3114 (manufactured by BASF), Irganox TM 1076 (manufactured by BASF), Irgafos TM 168 (manufactured by BASF), Irgafos TM 626 (manufactured by BASF) or Cyanox TM 1790 (manufactured by CYTEC). Wherein, the polyethylene resin composition may include a mixture of a first phenolic antioxidant and a second phosphorus antioxidant. In this regard, based on the total weight of the polymerized product produced by the secondary polymerization, the addition amount of the first phenolic antioxidant may be 50 ppm or more, or 200 ppm or more, or 250 ppm or more, and may be 500 ppm or less, or 300 ppm or less. Based on the total weight of the polymerized product produced by the secondary polymerization, the addition amount of the second phosphorus antioxidant may be 100 ppm or more, or 300 ppm or more, or 500 ppm or more, and may be 1000 ppm or less, or 700 ppm or less. Therefore, based on the total weight of the resin composition, the content of the first phenolic antioxidant of the polyethylene resin composition can be greater than 50 ppm, or greater than 200 ppm, or greater than 250 ppm, and can be less than 500 ppm, or less than 300 ppm, and the content of the second phosphorus antioxidant can be greater than 100 ppm, or greater than 300 ppm, or greater than 500 ppm, and can be less than 1000 ppm, or less than 700 ppm.
[0175] In addition, neutralizing agent can include calcium stearate (Ca-St), calcium palmitate, zinc stearate, zinc palmitate or hydrotalcite (hydroxy magnesium aluminum carbonate) etc., and can use any one or a mixture of two or more thereof. In addition, commercially available DHT-4A (manufactured by KYOWA) etc. can be used. Based on the gross weight of the polymerized product produced by secondary polymerization, the addition of neutralizing agent can be more than 100ppm, or more than 300ppm, or more than 500ppm, and can be less than 1000ppm, or less than 700ppm. Therefore, based on the gross weight of resin combination, the content of the neutralizing agent of polyethylene resin combination can be more than 100ppm, or more than 300ppm, or more than 500ppm, and can be less than 1000ppm, or less than 700ppm.
[0176] In addition, the melting and extrusion process may be performed according to a conventional method, for example, using an extruder such as a twin-screw extruder at an extrusion temperature of 180° C. to 220° C., or 180° C. to 210° C.
[0177] The polyethylene resin composition satisfying the above physical property requirements is prepared using the above preparation method. The prepared polyethylene resin composition exhibits excellent stretchability and physical properties, and when a biaxially stretched film is manufactured, there is no need to worry about defects such as breakage and shrinkage during stretching in the TD direction. In addition, the manufactured biaxially stretched film can exhibit excellent stretchability and tensile strength.
[0178] According to the present invention, there are provided a composition for producing a film, the composition comprising the polyethylene resin composition, and a stretched film produced using the polyethylene resin composition.
[0179] The composition for producing a film may be prepared in the same manner as a conventional method for preparing a composition for producing a film, except that the above-mentioned polyethylene resin composition is included.
[0180] In addition, the composition for making the film may also include other polyethylene resin compositions having different components or physical properties from the polyethylene resin composition in addition to the above-mentioned polyethylene resin composition. In this case, the other polyethylene resin composition may be included in a state mixed with the polyethylene resin composition, and its content may be determined according to the purpose and physical properties to be achieved. For example, based on the gross weight of the composition for making the film, the content of the other polyethylene resin composition may be greater than 0 wt % and less than 40 wt %.
[0181] Furthermore, the stretched film may specifically be a biaxially stretched film.
[0182] The stretched film can be produced in the same manner as a conventional method for producing a stretched film or a biaxially stretched film, except that the above-mentioned polyethylene resin composition is contained.
[0183] By including the above polyethylene resin composition, the stretched film can exhibit excellent stretchability and strength properties. Specifically, the stretch film of the present invention may have a longitudinal (MD) stretch ratio of 4 to 7, and a transverse (TD) stretch ratio of 4 to 9.
[0184] Furthermore, when stretched at a stretching ratio of 5×8 (MD×TD) and having a thickness of 20 μm, the stretched film satisfies the following requirements (b1) to (b3):
[0185] (b1) Haze measured according to ISO 13468: 20% or less,
[0186] (b2) a tensile modulus of elasticity in the MD direction of 1000 MPa to 1500 MPa and a tensile modulus of elasticity in the TD direction of 2000 MPa to 2500 MPa, as measured according to ASTM D882, and
[0187] (b3) The shrinkage in the MD direction is 3 to 5 and the shrinkage in the TD direction is 7 to 10 at 120°C as measured according to ASTM D1204.
[0188] Specifically, when stretched at a stretch ratio of 5×8 and having a thickness of 20 μm, the haze of the stretched film measured according to ISO 13468 is 20% or less, more specifically 15% or less, or 12% or less, or 10% or less. The lower the haze value, the better the stretched film, so the lower limit is not limited, but can be, for example, 1% or more, or 3% or more.
[0189] In addition, when the stretched film is stretched at a stretch ratio of 5×8 and has a thickness of 20 μm, the elastic tensile modulus in the MD direction is measured according to ASTM D882 standard, and is 1000 MPa to 1500 MPa, more specifically, 1000 MPa or more, or 1100 MPa or more, 1500 MPa or less, or 1400 MPa, and the elastic tensile modulus in the TD direction is 2000 MPa to 2500 MPa, more specifically, 2000 MPa or more, or 2100 MPa or more, 2500 MPa or less, or 2400 MPa.
[0190] Furthermore, when the stretched film was stretched at a stretch ratio of 5×8 and had a thickness of 20 μm, the shrinkage ratio in the MD direction was 3 to 5 and the shrinkage ratio in the TD direction was 7 to 10 at 120° C. as measured according to ASTM D1204.
[0191] Hereinafter, preferred exemplary embodiments will be provided for better understanding of the present invention. However, the following exemplary embodiments are provided only for easier understanding of the present invention, but the content of the present invention is not limited thereto.
[0192] <Preparation of Catalyst>
[0193] Preparation Example 1
[0194] 34 g of anhydrous magnesium chloride (99% by weight or more, water content less than 1%) was placed in a 2-liter Buchi reactor dried with nitrogen, and 600 mL of purified hexane with a water content of less than 0.5 ppm was also placed in the reactor. To the resulting reaction product, 175 mL of anhydrous 2-ethyl-1-hexanol was added under stirring, and then stirred at a temperature of 130° C. for about 2 hours to prepare a homogeneous solution of a magnesium carrier.
[0195] While stirring the homogeneous solution at a temperature of 35°C and a speed of 200rpm, 200mL of TiCl4 was slowly added within 1 hour and stirred for another hour. In the process, a solid material was produced. After the solid material was precipitated, the liquid portion was removed and the separated solid material was washed several times with hexane until the titanium concentration in the washing solution was less than 0.5mmol. To the washed solid material, a total volume of 1 liter of purified hexane was added. The titanium concentration in the resulting hexane slurry was 30mM. To the hexane slurry, 7mL of cyclohexyl chloride was added at a temperature of 40°C and stirred for 1 hour to obtain a Ziegler-Natta catalyst supported on magnesium.
[0196] The prepared catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride in a molar ratio of 0.13 based on 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 4:1, and the average size of the catalyst particles was 8 μm.
[0197] Preparation Example 2
[0198] A Ziegler-Natta catalyst supported on magnesium was prepared in the same manner as in Preparation Example 1, except that magnesium chloride was changed to magnesium ethoxide.
[0199] The prepared catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride in a molar ratio of 0.13 based on 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 5:1, and the average size of the catalyst particles was 10 μm.
[0200] Preparation Example 3
[0201] A Ziegler-Natta catalyst supported on magnesium was prepared in the same manner as in Preparation Example 1, except that anhydrous 2-ethyl-1-hexanol was changed to ethanol.
[0202] The prepared catalyst contained TiCl4 as a main catalyst and cyclohexyl chloride in a molar ratio of 0.13 based on 1 mol of the main catalyst. In addition, the molar ratio of Mg:Ti in the catalyst was 4.5:1, and the average size of the catalyst particles was 13 μm.
[0203] <Preparation of Polyethylene Resin Composition>
[0204] Example 1
[0205] The high density polyethylene resin composition was prepared by a process for preparing polyethylene by polymerization in the presence of a Ziegler-Natta catalyst system in a bimodal slurry process using two 100 L continuously stirred tank reactors (CSTRs).
[0206] Specifically, in the first reactor, the first polyethylene is prepared by conducting a polymerization reaction under the conditions shown in Table 1 below in the presence of ethylene, the Ziegler-Natta catalyst prepared in Preparation Example 1, a TEAL aqueous solution (30 mmol / hr) as a co-catalyst, hydrogen and a first comonomer.
[0207] Subsequently, in the second reactor, a second polymerization reaction was carried out under the conditions shown in the following Table 1. Here, the first polyethylene polymerized in the first reactor was fed into the second reactor in series to carry out secondary polymerization.
[0208] Based on the total weight of the polymerization product obtained as a result of the secondary polymerization, 250 ppm of BASF's Irganox 101 as a first antioxidant, 500 ppm of BASF's Irgafos 168 as a second antioxidant, and 500 ppm of calcium stearate (Ca-St) as a neutralizer were introduced and mixed, and then extruded at an extrusion temperature of 190° C. using a twin-screw extruder (TEK 30MHS, manufactured by SMPLATECH, with a diameter of 32 pi, L / D=40) to prepare a pellet-type polyethylene resin composition.
[0209] Examples 2 to 6
[0210] Each polyethylene resin composition was produced in the same manner as in Example 1, except that the conditions were changed as shown in Table 1 below.
[0211] Example 7
[0212] A polyethylene resin composition was manufactured in the same manner as in Example 1, except that the Ziegler-Natta catalyst prepared in Preparation Example 2 was used.
[0213] Example 8
[0214] A polyethylene resin composition was manufactured in the same manner as in Example 1, except that the Ziegler-Natta catalyst prepared in Preparation Example 3 was used.
[0215] Comparative Examples 1 to 3
[0216] Each polyethylene resin composition was produced in the same manner as in Example 1, except that the conditions were changed as shown in Table 2 below.
[0217] Comparative Example 4
[0218] A polyethylene resin composition was produced in the same manner as in Example 1, except that one continuous stirred tank reactor (CSTR) was used, and the conditions were changed as shown in Table 2 below.
[0219] Comparative Example 5
[0220] A polyethylene resin composition was manufactured in the same manner as in Example 1, except that no comonomer was introduced during the first slurry polymerization, and the conditions were changed as shown in Table 2 below.
[0221] Comparative Example 6
[0222] A polyethylene resin composition was manufactured in the same manner as in Example 1, except that two solution polymerization reactors were used instead of two continuous stirred tank reactors (CSTR), and the conditions were changed as shown in Table 2 below.
[0223] [Table 1]
[0224]
[0225] [Table 2]
[0226]
[0227] In Table 1, MI 2.16 [g / 10 min] is a melt index value of the first polyethylene produced by the polymerization reaction in the first reactor, measured according to ASTM D1238 (Condition E, 190° C., under a load of 2.16 kg).
[0228] Furthermore, the ethylene:comonomer weight ratio is the weight ratio of the total amount of ethylene introduced into the first and second reactors to the total amount of comonomers including the first and second comonomers.
[0229] The input amount of hydrogen (wt%) is expressed as a percentage of the input amount of hydrogen based on the total weight of ethylene introduced into the first and second reactors.
[0230] Experimental Example 1
[0231] The physical properties of the polyethylene resin compositions prepared in Examples and Comparative Examples were measured as follows, and the results are shown in the following Table 3 and the following Table 4, respectively.
[0232] (1) Density: measured according to ASTM D1792.
[0233] (2) Melt index (MI) 2.16 ): measured according to ASTM D1238 (Condition E, 190°C, under 2.16 kg load).
[0234] (3) MFRR(MI5 / MI 2.16 ): MI5 (ASTM D1238, 190°C, 5kg load) divided by MI 2.16 (ASTM D1238, 190°C, under 2.16 kg load) ratio obtained.
[0235] (4) Molecular weight (Mw, Mn, Mz) and molecular weight distribution
[0236] The polyethylene resin compositions of the embodiments and comparative examples were subjected to gel permeation chromatography (GPC) analysis to respectively determine the weight average molecular weight (Mw, g / mol), the number average molecular weight (Mn, g / mol) and the Z average molecular weight (Mz, g / mol), and the weight average molecular weight determined above was divided by the number average molecular weight to obtain the molecular weight distribution (Mw / Mn, MWD).
[0237] Specifically, Waters' PL-GPC220 was used as a gel permeation chromatography (GPC) instrument, and a PolymerLaboratories PLgel MIX-B 300mm long column was used. Here, the measurement temperature was 160°C, 1,2,4-trichlorobenzene was used as a solvent, and the measurement was performed at a flow rate of 1mL / min. The polyethylene resin composition sample was pretreated by dissolving it in 1,2,4-trichlorobenzene containing 0.025% BHT at 160°C using a GPC analyzer (PL-GP220) for 4 hours, and a sample with a concentration of 20mg / 10mL was prepared and then supplied in an amount of 200μL. The Mw and Mn values were obtained using a calibration curve formed using a polystyrene standard. Nine polystyrene standards were used, and the weight average molecular weights (g / mol) of the polystyrene standards were 2,000 / 10,000 / 30,000 / 70,000 / 200,000 / 700,000 / 2,000,000 / 4,000,000 / 10,000,000.
[0238] In addition, by GPC analysis, a molecular weight distribution curve was plotted with the logarithm of the weight-average molecular weight (Mw) (g / mol) (log Mw) on the x-axis and the molecular weight distribution (dwt / dlog M) relative to the logarithm on the y-axis, and the shape of the molecular weight distribution curve was determined.
[0239] (4) Content of short-chain branches (SCB: branches having 2 to 7 carbon atoms) (branches / 1000C) and NCD index
[0240] A polyethylene resin composition sample was pretreated by dissolving it in 1,2,4-trichlorobenzene containing 0.025% BHT at 160 °C for 4 hours using PL-SP260, and a sample with a concentration of 20 mg / 10 mL was prepared and then supplied in an amount of 200 μL. Measurement was performed using FT-IR connected to a GPC instrument (PL-GPC220, manufactured by Waters) under the following conditions.
[0241] <FT-IR Measurement Instrument and Measurement Conditions>
[0242] Measurement instrument: PerkinElmer Spectrum 100
[0243] Measurement temperature: 160 °C
[0244] Wavenumber: 2700 cm -1 to 3000 cm -1
[0245] Number of scans: 8
[0246] Resolution: 8 cm -1
[0247] Detector: DTGS
[0248] By FT-IR analysis, an SCB distribution curve was plotted with the logarithm of the weight-average molecular weight (Mw) (g / mol) (log Mw) on the x-axis and the number of SCBs per 1000 carbon atoms relative to the logarithm on the y-axis.
[0249] In addition, by this analysis, the number of SCBs per 1000 carbon atoms at log Mw = 5.5 and the number of SCBs per 1000 carbon atoms at log Mw = 4.5 were determined and used to obtain the NCD index according to the following Equation 1.
[0250] [Equation 1]
[0251] NCD index = -(number of SCBs per 1000 carbon atoms at log Mw = 5.5 - number of SCBs per 1000 carbon atoms at log Mw = 4.5)
[0252] This represents the value obtained by multiplying the slope of the straight line connecting the y-values (number of SCBs) between 4.5 and 5.5 on the x-axis (log Mw) of the GPC and FT-IR curves by -1. When the polyethylene resin composition has an NCD structure, the slope value becomes negative because the SCB content is higher in the low molecular weight region. Therefore, this value is expressed as a positive number by multiplying by -1 to indicate that the NCD structure is enhanced due to the positive NCD index.
[0253] (5) Content ratio of the highly crystalline fraction
[0254] The polyethylene resin compositions of the examples and comparative examples were subjected to temperature rising elution fractionation (TREF) in the following manner, and the content ratio of the highly crystalline fraction eluted at an elution temperature of 100 °C or higher (highly crystalline fraction, T ≥ 100 °C) was obtained.
[0255] The temperature rising elution fractionation (TREF) analysis of the polyethylene resin composition was carried out using a TREF device of PolymerChar in the temperature range of -20 °C to 130 °C and using trichlorobenzene as the solvent. At this time, the cooling rate in the crystallization step was set to 0.1 °C / min, and the analysis was carried out under the following conditions.
[0256] Specifically, at 150 °C, a 30 mg sample of the polyethylene resin composition was dissolved in 20 mL of trichlorobenzene for 60 minutes and stabilized at 140 °C for 20 minutes. The sample was introduced into the TREF column, then cooled to -20 °C at a cooling rate of 0.1 °C / min and held for 2 minutes. Thereafter, while heating from -20 °C to 130 °C at a rate of 1 °C / min, the solvent trichlorobenzene was applied to the column at a flow rate of 0.5 mL / min, and then the concentration of the eluted polymer was measured.
[0257] <TREF measurement conditions>
[0258] Dissociation rate: 40 °C / min
[0259] Stabilization rate: 40 °C / min
[0260] Crystallization rate 1: 0.1 °C / min
[0261] Elution rate: 1 °C / min
[0262] Cleaning rate: 30 °C / min
[0263] Dissociation temperature: 150 °C
[0264] Stabilization temperature: 140 °C
[0265] Crystallization temperature: 35 °C
[0266] Elution starting temperature: 35°C
[0267] Elution temperature: 140°C
[0268] Temperature after elution: 150℃
[0269] Cleaning temperature: 150℃
[0270] Dissociation time: 60min
[0271] Stabilization time: 20min
[0272] Crystallization time: 10min
[0273] Time before injection: 10 minutes
[0274] Soluble fraction time: 10 min
[0275] Elution time: 10min
[0276] Cleaning time: 10 minutes
[0277] Cleaning cycles: 1
[0278] Content ratio of high crystalline fraction (T≥100°C) (weight %): Through TREF analysis, a TREF analysis curve with elution temperature (Te) (°C) as the x-axis and elution amount (dw / dt) as the y-axis is obtained, and from the TREF analysis graph, the content ratio (weight %) of the high crystalline fraction eluted at an elution temperature above 100°C based on the total weight of all eluted fractions is calculated.
[0279] [Table 3]
[0280]
[0281] [Table 4]
[0282]
[0283] As experimental results, the polyethylene resin compositions of Examples 1 to 8 had an NCD index of 0 or more and had a bimodal molecular weight distribution, indicating that they had an NCD structure and a low molecular weight region had a high SCB content derived from the comonomer.
[0284] In contrast, Comparative Examples 1 to 3 and 5 showed a bimodal molecular weight distribution, but the NCD index was a negative value less than 0, indicating that they had a broad orthogonal comonomer distribution (BOCD) structure in which the SCB content from the comonomer was low in the low molecular weight region and the SCB content was high in the high molecular weight region, or had a flat structure in which the SCB was uniformly distributed.
[0285] Furthermore, the polyethylene resin composition of Comparative Example 4 showed a unimodal molecular weight distribution and a flat comonomer distribution.
[0286] Furthermore, since the polyethylene resin composition of Comparative Example 6 was prepared by a solution polymerization process, it showed a low Mz value and a low high crystalline fraction content.
[0287] Experimental Example 2
[0288] For the polyethylene resin compositions prepared in Examples 3 and 6 and Comparative Example 1, changes in loss modulus of the specimens according to temperature were measured by dynamic mechanical analysis (DMA).
[0289] Specifically, each of the polyethylene resin compositions of Examples 3 and 6 and Comparative Example 1 was pressed at 190° C. to prepare a rectangular test piece having a thickness of 0.5 mm, a width of 6 mm, and a length of 30 mm.
[0290] Each of the prepared samples was mounted on the film tension fixture (gap: 10 mm) of TAInstruments Q850 DMA, heated from -50°C to 140°C at a rate of 3°C / min, and after applying a sinusoidal vibration with an input frequency of 1 Hz and a shear deformation with a deformation amplitude of 5%, the loss modulus (MPa) was measured from the output response characteristics shown on the board. From the results, a graph of the change in loss modulus according to temperature was obtained and plotted in Figure 1 Shown in.
[0291] like Figure 1 As shown in the graph of the loss modulus according to temperature, a peak appears in the range of -40°C to 10°C, which is caused by the movement of polymer chains between lamellar crystals (β relaxation).
[0292] Generally, at similar density, the higher the content of the comonomer-derived structure in the low molecular weight region, the greater the chain mobility between the lamellar crystals. Compared with Comparative Example 1, the polyethylene resin compositions of Examples 3 and 6 exhibit β relaxation peaks in the corresponding regions. From these results, it can be expected that the polyethylene resin compositions of Examples 3 and 6 having NCD structures are more conducive to biaxial stretching in film production.
[0293] Experimental Example 3
[0294] Biaxially stretched films were produced using each of the polyethylene resin compositions prepared in Examples 1 to 8 and Comparative Examples 1 to 6, and stretchability was evaluated.
[0295] (1) Production of biaxially stretched films
[0296] - Cast sheets of the polyethylene resin composition having a thickness of 0.72 mm were produced using a laboratory extruder line from Bruckner (L / D ratio: 42, screw diameter: 25 mm, melt / T-die temperature: 250°C).
[0297] - Biaxial stretching was performed using a KARO 5.0 machine to produce a polyethylene resin composition sheet having a width x height of 90 mm x 90 mm.
[0298] - After preheating at 120°C for 100 seconds, stretching (MD→TD) was performed sequentially.
[0299] -When stretching, the speed is 300% / s.
[0300] - Final film thickness (based on a stretch ratio of 5×8): 20 μm.
[0301] (2) Evaluation of stretchability
[0302] As shown in Table 5 below, the cast film produced in (1) was biaxially stretched while changing the stretching ratio in the MD / TD directions, and the stretchability was evaluated according to the following criteria.
[0303] <Evaluation Criteria>
[0304] O: Stretchable, excellent appearance without defects
[0305] △: Stretchable, but poor appearance due to changes in film thickness
[0306] X: Not stretchable due to breaking
[0307] [Table 5]
[0308]
[0309] (3) Evaluation of film properties (evaluation of elastic tensile modulus, haze and shrinkage)
[0310] Each biaxially stretched film having a stretch ratio of 5×8 and a thickness of 20 μm was manufactured in the same manner as in (1) using the polyethylene resin compositions of Examples 1 to 6 and Comparative Example 6, and then the elastic tensile modulus (1% elastic modulus) of each film was measured according to ASTM D882.
[0311] Furthermore, the haze of each film was measured according to the ISO 13468 standard, and the shrinkage was evaluated according to the ASTM D1204 standard.
[0312] [Table 6]
[0313]
[0314] As an experimental result, the polyethylene resin compositions of Examples 1 to 6 of the present invention exhibited significantly improved stretchability compared to the resin compositions of Comparative Examples 1 to 5 except Comparative Example 6. The stretched films manufactured using the polyethylene resin compositions of Examples 1 to 6 also exhibited improved tensile strength characteristics and excellent shrinkage characteristics and transparency.
[0315] In contrast, when producing a stretched film, the resin composition of Comparative Example 6 exhibited the same level of stretchability as that of Example 1. However, due to the low content of the high crystalline fraction, the stretched film produced using the resin composition of Comparative Example 6 exhibited significant deterioration in tensile strength, haze, and shrinkage characteristics compared to the stretched films of the Examples.
Claims
1. A polyethylene resin composition, which meets the following requirements (a1) to (a6): (a1) Density measured according to ASTM D792: 0.940 g / cm 3 Up to 0.965g / cm 3 , (a2) NCD index calculated according to the following equation 1: 0 or above, (a3) In gel permeation chromatography analysis, when a molecular weight distribution curve is plotted with the logarithmic value (log M) of the weight average molecular weight (M) (g / mol) as the x-axis and the molecular weight distribution relative to the logarithmic value (dwt / dlog M) as the y-axis, the type of the molecular weight distribution curve: bimodal, (a4) in the temperature rising elution fractionation analysis, the content of the highly crystalline fraction eluted at an elution temperature of 100° C. or higher, based on the total weight of all eluted fractions: 35% by weight or higher, (a5) Z average molecular weight (Mz): 500000 g / mol to 800000 g / mol, (a6) Number of SCBs per 1000 carbon atoms: greater than 3 and less than 8, [Equation 1] NCD index = - (SCB number per 1000 carbon atoms at logMw of 5.5 - SCB number per 1000 carbon atoms at logMw of 4.5) In Equation 1, Mw represents a weight average molecular weight (g / mol), and SCB represents a short chain branch having 2 to 7 carbon atoms attached to a polyethylene main chain.
2. The polyethylene resin composition according to claim 1, wherein In dynamic mechanical analysis, the polyethylene resin composition exhibits a β relaxation peak at -40°C to 10°C in a graph of loss modulus versus temperature.
3. The polyethylene resin composition according to claim 1, wherein The polyethylene resin composition has a melt index (MI) measured at 190° C. under a load of 2.16 kg according to ASTM D1238. 2.16 ) is 0.5g / 10min to 3.0g / 10min.
4. The polyethylene resin composition according to claim 1, wherein The MFRR (MI5 / MI 2.16 ) is 3 to 5, which is the melt index (MI5) measured at a temperature of 190° C. under a load of 5 kg according to ASTM D1238 divided by the melt index (MI5) measured at a temperature of 190° C. under a load of 2.16 kg 2.16 ) and the ratio obtained.
5. The polyethylene resin composition according to claim 1, wherein The polyethylene resin composition has a weight average molecular weight (Mw) of 80,000 g / mol to 130,000 g / mol.
6. The polyethylene resin composition according to claim 1, wherein The number average molecular weight (Mn) of the polyethylene resin composition is greater than or equal to 5000 g / mol and less than 11000 g / mol.
7. The polyethylene resin composition according to claim 1, wherein The polyethylene resin composition has a polydispersity index [Mw / Mn] of 8 to 20.
8. The polyethylene resin composition of claim 1, comprising an ethylene / C4 to C10 α-olefin copolymer.
9. The polyethylene resin composition according to claim 8, wherein The ethylene / C4 to C10 α-olefin copolymer is an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, an ethylene / 1-octene copolymer or an ethylene / 1-butene / 1-octene copolymer.
10. A method for preparing the polyethylene resin composition of claim 1, comprising: a first step of preparing a first polyethylene by conducting a first slurry polymerization of ethylene and a first comonomer of C4 to C10 alpha olefins in a first reactor while introducing hydrogen in the presence of a Ziegler-Natta catalyst; as well as The first polyethylene is transferred to a second reactor connected to the first reactor, and then ethylene alone or ethylene and a C4 to C10 alpha-olefin second comonomer are introduced and a second slurry polymerization is carried out in a second step, The input amount of the first comonomer introduced during the first slurry polymerization reaction is greater than the input amount of the second comonomer introduced during the second slurry polymerization reaction.
11. The method of claim 10, wherein: A weight ratio of the second comonomer introduced during the second slurry polymerization reaction to the first comonomer introduced during the first slurry polymerization reaction is greater than 0 and less than 1.
12. The method of claim 10, wherein: The polymerization temperature (T1) and pressure (P1) during the first slurry polymerization reaction are higher than the polymerization temperature (T2) and pressure (P2) during the second slurry polymerization reaction.
13. The method of claim 12, wherein: The polymerization temperature (T1) during the first slurry polymerization reaction was 70°C to 90°C, and the polymerization temperature (T2) during the second slurry polymerization reaction was 70°C to 90°C.
14. The method of claim 12, wherein: The pressure (P1) during the first slurry polymerization reaction was 5 kgf / cm 2 Up to 10kgf / cm 2 , and the pressure (P2) during the second slurry polymerization reaction is 1 kgf / cm 2 Up to 5kgf / cm 2 .
15. The method of claim 10, wherein: The Ziegler-Natta catalyst used in the first slurry polymerization process is a magnesium-supported titanium catalyst.
16. The method of claim 10, wherein: The Ziegler-Natta catalyst used in the first slurry polymerization process further comprises a halogenated hydrocarbon.
17. The method of claim 16, wherein: The halogenated hydrocarbons are bromoform, tetrachloroethane, hexachloroethane, pentachloroethane, 1,1,2,2-tetrachloroethane, 1-bromo-1-chloroethane, 1,2-dibromoethane, 1,2-dichloroethane, bromoethane, hexachloropropane, 1,2,3-trichloropropane, 1,2-dichloropropane, 1-chloropropane, 2-chloropropane, chlorobutane, dichlorobutane, 1-chloro-2-methylpropane, n-butyl chloride, tert-butyl chloride, 1-chloro-3-methylbutane, 1-chloropentane , 1,5-dichloropentane, bromopentane, neopentyl chloride, 1-chloroheptane, cyclopropyl bromide, cyclobutyl chloride, cyclohexyl chloride, cyclohexyl bromide, vinylidene chloride, 1,2,3,3-tetrachloropropene, 1,2-dibromo-1-propene, 1,3-dichloropropene, hexachloro-1,3-butadiene, 2-bromo-2-butene, propargyl chloride, chlorobenzene, tetrachlorobenzene, trichlorobenzene, dichlorobenzene, 4-chlorobenzyl chloride, benzyl chloride, or 1,1-dichloro-2-phenylcyclopropane.
18. A stretched film comprising the polyethylene resin composition according to claim 1.
19. The stretched film according to claim 18, wherein The stretched film has a stretch ratio of 4 to 7 in the machine direction (MD), and a stretch ratio of 4 to 9 in the transverse direction (TD).
20. The stretched film according to claim 18, wherein When stretched at a stretch ratio of 5×8 and having a thickness of 20 μm, the stretched film satisfies the following requirements (b1) to (b3): (b1) Haze measured according to ISO 13468: 20% or less, (b2) a tensile modulus of elasticity in the MD direction of 1000 MPa to 1500 MPa and a tensile modulus of elasticity in the TD direction of 2000 MPa to 2500 MPa when measured according to ASTM D882, and (b3) When measured according to ASTM D1204, at 120° C., the shrinkage in the MD direction is 3 to 5, and the shrinkage in the TD direction is 7 to 10.