Ink composition, light-shielding member, and image display device
By adding a light shielding agent, a cationic polymerizable compound, a photoacid generator and a sensitizer to the ink composition, the problem of adhesion and light shielding balance of the ink composition during photocuring is solved, and an image display device is realized High-efficiency light-shading components in.
Patent Information
- Application Number
- CN202380031815.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-02-09
- Publication Date
- 2024-11-15
AI Technical Summary
The conventional ink compositions are difficult to achieve substrate adhesion while maintaining curability and light shielding properties, and there is a problem that light shielding materials are difficult to cure when light curing.
The ink composition containing a sunscreen, a cationic polymerizable compound, a photoacid generator and a sensitizer is adopted. The volume concentration of the sunscreen is 0.3% or less than 12%. The cationic polymerizable compound contains a metal element compound and a sensitizer. Contains anthracene skeleton and promotes polymerization reaction through photoacid generators.
It is achieved while maintaining the curability of the ink composition, and is excellent substrate adhesion and light-shielding properties are obtained, and is suitable for light-shielding components in an image display device, thereby improving the stability and light-shielding effect for long-term use.
Smart Images

Figure CN118974186A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to an ink composition, a light shielding component and an image display device. Background Art
[0002] In recent years, image display devices capable of displaying clearer images are being developed. For example, Patent Document 1 discloses a display module having a plurality of LED chips mounted on a substrate. Patent Document 1 also shows a structure in which a light reflection wall is provided between the LED chips to prevent interference of output light between the LED chips (see Patent Document 1; paragraph
[0043] , FIG. 4, etc.).
[0003] In this regard, a resin composition capable of forming light-shielding partition walls is disclosed in Patent Document 2. According to the resin composition disclosed in Patent Document 2, thick film partition walls having both tack-free properties after prebaking and heat resistance after curing can be formed.
[0004] Patent Document 3 discloses a curable composition that is suitable for use in an inkjet process and has a glossiness that is suppressed as a black matrix used in LED products. Prior art literature Patent Literature
[0005] Patent Document 1: Japanese Patent Publication No. 2018-026517 Patent Document 2: Japanese Patent Publication No. 2021-161401 Patent Document 3: International Publication No. 2021 / 049331 Summary of the invention Technical problem to be solved by the invention
[0006] However, in order to use the image display device for a long time, the light shielding material such as the light reflecting wall needs to have sufficient substrate adhesion. Although the light shielding material can also be formed by a photocurable ink composition, the material formed by the existing ink composition cannot meet such substrate adhesion. In addition, the ink composition for forming the light-shielding material generally has light-shielding properties itself and therefore has a side that it is difficult to be cured by light.
[0007] In view of the above circumstances, the present invention provides an ink composition capable of obtaining a cured product having an excellent balance between substrate adhesion and light shielding properties while maintaining the curability of the ink composition. Technical means of solving problems
[0008] According to one aspect of the present invention, an ink composition is provided. The ink composition includes a light-shielding agent (A), a cationically polymerizable compound (B), a photoacid generator (C), and a sensitizer (D). The volume concentration of the light-shielding agent (A) is 0.3% to 12% with respect to the total solid content volume of the ink composition. The cationically polymerizable compound (B) includes a metal element-containing compound (B1) having a cationically polymerizable group and a hydrolyzable group. When the total solid content of the ink composition is 100 parts by mass, the content of the metal element-containing compound (B1) is 5 parts by mass or more and 80 parts by mass or less. The sensitizer (D) includes a compound (D1) containing an anthracene skeleton. Effects of the Invention
[0009] According to this aspect, an ink composition or the like is provided, which can obtain a cured product having an excellent balance between substrate adhesion and light shielding properties while maintaining the curability as an ink composition. BRIEF DESCRIPTION OF THE DRAWINGS
[0010] Figure 1 It is a cross-sectional view of an image display device using a cured product of the ink composition according to this embodiment as a light shielding member. DETAILED DESCRIPTION
[0011] The following describes the embodiments of the present invention. The various features described in the embodiments described below can be combined with each other. In addition, "to" in this specification means above to below unless otherwise specified.
[0012] <Ink Composition> The ink composition of this embodiment is as follows. An ink composition comprising: A sunscreen (A), a cationic polymerizable compound (B), a photoacid generator (C) and a sensitizer (D); wherein: The volume concentration of the light-shielding agent (A) is 0.3% to 12% relative to the total volume of the solid content of the ink composition, The cationically polymerizable compound (B) comprises a metal element-containing compound (B1) having a cationically polymerizable group and a hydrolyzable group, When the total solid content of the ink composition is 100 parts by mass, the content of the metal element-containing compound (B1) is 5 parts by mass or more and 80 parts by mass or less. The sensitizer (D) includes a compound (D1) having an anthracene skeleton. Hereinafter, components constituting the ink composition according to the present embodiment, a method for producing the ink composition, uses, etc. will be described.
[0013] (Sunscreen (A)) The ink composition of this embodiment contains a light shielding agent (A). As described later, the ink composition of this embodiment is typically used when forming a light shielding member, and the inclusion of the light shielding agent (A) in such an ink composition contributes to improving the light shielding property of such a light shielding member.
[0014] The light-shielding agent (A) can be selected from known materials and used. However, from the viewpoint of availability and a high balance between light-shielding properties, the light-shielding agent (A) preferably contains carbon black (A1).
[0015] In addition, as the sunscreen (A), other sunscreens (A2) other than the carbon black (A1) may also be included. As other sunscreens (A2), there may be mentioned: titanium black; iron oxide black; inorganic sunscreens (A2-1) such as sunscreens containing one or more metal elements such as vanadium, silver, copper, and tin; organic black pigments (A2-2) such as aniline black, perylene black, and lactam black; black dyes (A2-3) such as azo compounds or azine compounds, etc. In addition, other sunscreens (A2) may also be composed by combining colored pigments (A2-4) such as red pigments, blue pigments, green pigments, and yellow pigments, or by colored dyes (A2-5) such as red dyes, blue dyes, green dyes, and yellow dyes. In addition, as long as the light-shielding function can be ensured for the obtained cured product, the other light-shielding agent (A2) may be used alone or in combination of two or more.
[0016] In the ink composition of this embodiment, the volume concentration of the light-shielding agent (A) is set in the range of 0.3% to 12% relative to the total volume of the solid content of the ink composition. By setting the volume concentration of the light-shielding agent (A) in such a range, the light-shielding property of the obtained light-shielding component can be improved while ensuring the curability of the ink composition.
[0017] Here, the volume concentration is the ratio of the volume of the light-shielding agent (A) contained in the total solid content volume of the ink composition. The method for determining the volume concentration of the light-shielding agent (A) can be set appropriately, but is typically determined as follows. That is, if the volume of the entire components other than the light-shielding agent (A) in the ink composition can be measured, the bulk density of the light-shielding agent (A) can be calculated by the following formula (X1). Bulk density of sunscreen (A) = Volume of sunscreen (A) / (Volume of sunscreen (A) + Volume of all components other than sunscreen (A))...(X1)
[0018] Note that the volume of the light-shielding agent (A) can be calculated by the following formula (X2). Volume of sunscreen (A) = weight of sunscreen (A) / true density of sunscreen (A)...(X2)
[0019] Similarly, the volume of the entire components other than the sunscreen agent (A) can be calculated by the following formula (X3). The volume of all components other than the sunscreen (A) = the weight of all components other than the sunscreen (A) / the true density of all components other than the sunscreen (A) (X3)
[0020] That is, if the formula of the ink composition is known, the volume concentration of the sunscreen (A) can be calculated as described above based on the types and amounts of the components added. On the other hand, even if the details of the formula of the ink composition are unknown, by separating the sunscreen (A) and other components, the volumes of both components can be calculated, and thus the volume concentration can be calculated.
[0021] Note that the volume concentration of the light-shielding agent (A) is preferably 0.5% or more, more preferably 1% or more, and further preferably 1.5% or more relative to the total volume of the solid content of the ink composition. By setting it to such a range, the light-shielding property of the light-shielding component can be further improved. In addition, the volume concentration of the light-shielding agent (A) is preferably 10% or less, more preferably 9% or less, and further preferably 8% or less relative to the total volume of the solid content of the ink composition. By setting it to such a range, the curability of the ink composition can be further improved.
[0022] In addition, in the present embodiment, when the solid content of the ink composition is set to 100 parts by mass as a whole, the content of the light-shielding agent (A) is preferably 0.6 parts by mass or more and 18 parts by mass or less. In addition, from other aspects, in the ink composition of the present embodiment, the content of the light-shielding agent (A) is preferably 3 parts by mass or more and 14 parts by mass or less when the solid content of the ink composition is set to 100 parts by mass as a whole. By setting the content of the light-shielding agent (A) to such a range, the light-shielding property of the obtained light-shielding component can be improved while ensuring the curability of the ink composition. When the total solid content of the ink composition is 100 parts by mass, the content of the light shielding agent (A) is preferably 5 parts by mass or more, and more preferably 7 parts by mass or more. By setting the content within such a range, the light shielding property of the light shielding member can be further improved. In addition, when the solid content of the ink composition is set to 100 parts by mass, the content of the light-shielding agent (A) is preferably 13 parts by mass or less, and more preferably 11 parts by mass or less. By setting it to such a range, the curability of the ink composition can be further improved. In addition, in order to improve the curability of the ink composition, the content of the light-shielding agent (A) can also be set to 8 parts by mass or less or 5 parts by mass or less relative to 100 parts by mass of the solid content of the ink composition. In other aspects, when the total solid content of the ink composition is 100 parts by mass, the content of the light shielding agent (A) may be 0.8 parts by mass or more, 1 part by mass or more, or 1.2 parts by mass or more.
[0023] The mass ratio of carbon black (A1) in the sunscreen (A) as a whole is preferably 80 mass % or more, more preferably 90 mass % or more, further preferably 95 mass % or more, and particularly preferably 98 mass % or more. In addition, the sunscreen (A) may also be substantially composed of carbon black (A1) only. In this way, it is easier to exert the above-mentioned effects.
[0024] In addition, the sunscreen (A) may be composed of other sunscreens (A2) other than carbon black (A1). The mixing ratio of other sunscreens (A2) is arbitrary. As an example, the sunscreen (A) is substantially composed of only inorganic sunscreens containing one or more metal elements such as titanium black or iron oxide black, vanadium, silver, copper, tin, etc.
[0025] (Cationically polymerizable compound (B)) The ink composition of the present embodiment includes a cationically polymerizable compound (B). The cationically polymerizable compound (B) is a compound containing a cationically polymerizable group in its chemical structure. Specifically, as the cationically polymerizable group, in addition to cyclic ether groups such as epoxy or oxetane, vinyl ether groups, etc. can also be cited. In addition, as the cationically polymerizable compound (B) of the present embodiment, in addition to epoxy compounds and oxetane compounds, compounds such as oxetane compounds (tetrahydrofuran, substituted tetrahydrofuran, etc.) are also included.
[0026] The ink composition of this embodiment includes a metal element-containing compound (B1) having a cationic polymerizable group and a hydrolyzable group as the cationic polymerizable compound (B). In addition, the ink composition of this embodiment may also contain other cationic polymerizable compounds (B2) that are not included in the metal element-containing compound (B1). These components are further described below.
[0027] The metal element-containing compound (B1) in the present embodiment contains the cationically polymerizable group and the metal element in its chemical structure. Specifically, the metal element-containing compound (B1) can be represented by the following structural formula (1). M(R)x(X)y···(1) Here, M in the structural formula (1) is a metal element, R is an organic group containing a cationic polymerizable group in its structure, and the carbon atom possessed by R is bonded to M. X is a group selected from the group consisting of a hydrogen atom, a halogen atom, a hydroxyl group, an alkoxy group, and a phenoxy group. x and y are integers greater than 1, and the sum of x and y is the number of combinations of M.
[0028] As the metal element, silicon, aluminum, titanium, zirconium, tin, lead, boron and the like can be cited. Among them, from the viewpoint of high ease of handling and excellent operability, the metal element is preferably silicon, that is, the metal element-containing compound (B1) is preferably a silicon-containing compound. In addition, as described above, the metal element-containing compound (B1) contains a cationically polymerizable group in the structure of R. In this regard, from the viewpoint of its high reactivity, it is preferred that an epoxy group is contained in the structure of R, that is, the cationically polymerizable group possessed by the metal element-containing compound (B1) is preferably an epoxy group. In addition, the cationically polymerizable group contained in the structure of R may also be an oxetane group. When X is an alkoxy group, the carbon number of the alkoxy group is, for example, 1 to 8, preferably 1 to 6, and more preferably 1 to 4. When X is a phenoxy group, the hydrogen atoms of the benzene ring constituting the phenoxy group may be substituted by various substituents. Note that when M is silicon, x is 1 or 2 and y is 2 or 3.
[0029] The metal element-containing compound (B1) of this embodiment undergoes cationic polymerization using the acid generated by the photoacid generator (C) described later, and the metal element contained in its structure can form a chemical bond with the surface of the substrate to which the ink composition is applied. Due to this contribution, the ink composition of this embodiment can exhibit high substrate adhesion.
[0030] Particularly preferred compounds of the metal element-containing compound (B1) include 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxysilane, 3-glycidyloxypropylmethyldimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, 3-[(3-ethyloxetane-3-yl)methoxy]propyl(trimethoxy)silane, 3-[(3-ethyloxetane-3-yl)methoxy]propyl(triethoxy)silane, 3-[(3-methyloxetane-3-yl)methoxy]propyl(trimethoxy)silane, and 3-[(3-methyloxetane-3-yl)methoxy]propyl(trimethoxy)silane.
[0031] In addition, other cationically polymerizable compounds (B2) that can be included in the ink composition of this embodiment are preferably epoxy compounds, oxetane compounds, vinyl ether compounds, etc., from the perspective of availability and high reactivity. Note that other cationically polymerizable compounds do not contain the metal element in their chemical structure.
[0032] The epoxy compound is a compound having an epoxy group, and examples thereof include a glycidyl ether epoxy compound and an alicyclic epoxy compound. Note that the number of epoxy groups in the epoxy compound may be 1 or more, but a compound having 2 or more epoxy groups may be contained. That is, the epoxy compound in the other cationically polymerizable compound (B2) of this embodiment may be a monofunctional epoxy compound or a polyfunctional epoxy compound.
[0033] Specific examples of epoxy compounds include phenyl glycidyl ether, 2-ethylhexyl glycidyl ether, 3,3-bis[(2-oxiranylmethoxy)methyl]oxetane, 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, 3,4,3',4'-diepoxybicyclohexane, 1,2-epoxy-4-vinylcyclohexane, ε-caprolactone-modified 3',4'-epoxycyclohexylmethyl, 3,4-epoxycyclohexanecarboxylate, limonene oxide, 2,2-bis(4-glycidyloxyphenyl)propane, 2-[4-(2, A mixture of 1,3-bis[4-[1-[4-(2,3-epoxypropoxy)phenyl]-1-[4-[1-[4-(2,3-epoxypropoxy)phenyl]-1-methylethyl]phenyl]ethyl]phenoxy]-2-propanol, 2-[4-[1,1-bis[4-([2,3-epoxypropoxy]phenyl)]ethyl]phenyl]propane, and 1,3-bis[4-[1-[4-(2,3-epoxypropoxy)phenyl]-1-[4-[1-[4-(2,3-epoxypropoxy)phenyl]-1-methylethyl]phenyl]ethyl]phenoxy]-2-propanol.
[0034] In addition, the epoxy compound may be any of an epoxy monomer, an epoxy oligomer, and an epoxy resin, and commercially available products shown below may also be used. That is, a polyfunctional epoxy monomer such as Celloxide (registered trademark) CEL2021P, CEL2000, or CEL8000 (manufactured by Daicel Corporation) can be used as the epoxy compound. In addition, glycidyl ether type epoxy resins such as TECHMORE VG3101L (manufactured by Printec Co., Ltd.), EPPN-501H, 502H (manufactured by Nippon Kayaku Co., Ltd.), and JER1032H60 (manufactured by Mitsubishi Chemical Corporation); bisphenol A novolac type epoxy resins such as JER157S65 and 157S70 (manufactured by Mitsubishi Chemical Corporation); and novolac type epoxy resins such as EPPN-201 (manufactured by Nippon Kayaku Co., Ltd.), JER152 and 154 (manufactured by Mitsubishi Chemical Corporation) can also be used as epoxy compounds in this embodiment.
[0035] The oxetane compound may have 1 or more oxetane groups, but may also contain compounds having 2 or more oxetane groups. That is, the oxetane compound in the other cationically polymerizable compound (B2) of the present embodiment may be a monofunctional oxetane compound or a polyfunctional oxetane compound.
[0036] Examples of oxetane compounds include 2-ethylhexyloxetane, 3-ethyl-3-ethoxymethyloxetane, 3-ethyl-3-butoxymethyloxetane, 3-ethyl-3-hexyloxymethyloxetane, 3-ethyl-3-(2-ethylhexyloxymethyl)oxetane, [(1-ethyl-3-oxetane)methoxy]cyclohexane, 3-ethyl-3-(phenoxymethyl)oxetane, 3-ethyl-3-methoxymethyloxetane, and oxetane alcohol. , 3-ethyl-3{[3-ethyloxetan-3-yl]methoxy}methyl)oxetane, bis[(1-ethyl-3-oxetan-3-yl]methoxy]cyclohexane, bis[(1-ethyl-3-oxetan-3-yl)methoxy]norbornane, 1,4-bis((1-ethyl-3-oxetan-3)methoxy)benzene, 1,3-bis((1-ethyl-3-oxetan-3)methoxy)benzene, 4,4'-bis((3-ethyl-3-oxetan-3)methoxy)biphenyl, xylylenebisoxetane, and the like.
[0037] Examples of vinyl ether compounds include divinyl ether compounds or trivinyl ether compounds such as ethylene glycol divinyl ether, diethylene glycol divinyl ether, triethylene glycol divinyl ether, propylene glycol divinyl ether, dipropylene glycol divinyl ether, butanediol divinyl ether, hexanediol divinyl ether, cyclohexanedimethanol divinyl ether, and trimethylolpropane trivinyl ether; and monovinyl ether compounds such as ethyl vinyl ether, n-butyl vinyl ether, isobutyl vinyl ether, octadecyl vinyl ether, cyclohexyl vinyl ether, hydroxybutyl vinyl ether, 2-ethylhexyl vinyl ether, cyclohexanedimethanol monovinyl ether, n-propyl vinyl ether, isopropyl vinyl ether, isopropenyl ether-o-propylene carbonate, dodecyl vinyl ether, diethylene glycol monovinyl ether, and octadecyl vinyl ether.
[0038] When the ink composition of the present embodiment contains another cationically polymerizable compound (B2), the other cationically polymerizable compound (B2) preferably contains a compound having one cationically polymerizable group in its chemical structure. Typically, the ink composition of the present embodiment preferably contains a monofunctional epoxy compound or a monofunctional oxetane compound. These compounds are less likely to shrink upon curing during curing and thus contribute to the adhesion of the cured film to the substrate. As an example, when the other cationic polymerizable compounds (B2) are set to 100 parts by mass as a whole, the content of the monofunctional epoxy compound or the monofunctional oxetane compound can be 5 parts by mass or more, 20 parts by mass or more, or 40 parts by mass or more. There is no particular restriction on the upper limit, and all of the other cationic polymerizable compounds (B2) can be monofunctional epoxy compounds or monofunctional oxetane compounds. When the other cationic polymerizable compounds (B2) are set to 100 parts by mass as a whole, the content of the monofunctional epoxy compound or the monofunctional oxetane compound can also be adjusted to 85 parts by mass or less.
[0039] In addition, when the ink composition of the present embodiment contains other cationic polymerizable compounds (B2), it is preferred that other cationic polymerizable compounds (B2) are two or more components. By adopting this structure, it is easy to achieve an ink composition with excellent curability or adhesion and hardness balance of the cured film.
[0040] In the ink composition of the present embodiment, when the solid content of the ink composition as a whole is set to 100 parts by mass, the content of the cationic polymerizable compound (B) is preferably from 5 parts by mass to 96 parts by mass, more preferably from 7 parts by mass to 95 parts by mass, and further preferably from 10 parts by mass to 94 parts by mass. By setting the content of the cationically polymerizable compound (B) within such a range, the curability of the ink composition can be increased to a high level while ensuring the storage stability of the ink composition.
[0041] In the ink composition of the present embodiment, when the solid content of the ink composition is set to 100 parts by mass as a whole, the content of the metal element compound (B1) is 5 parts by mass or more and 80 parts by mass or less. By setting the content of the compound (B1) containing the metal element within such a range, the adhesion of the substrate can be further improved compared with the prior art. In addition, when the solid content of the ink composition is set to 100 parts by mass as a whole, the content of the metal element compound (B1) is more preferably 8 parts by mass or less and 78 parts by mass, and more preferably 10 parts by mass or less and 78 parts by mass or less. By setting the content of the metal element compound (B1) within such a range, the adhesion of the substrate can be made to a higher level. Note that from the viewpoint of saving manufacturing costs, when the solid content of the ink composition is set to 100 parts by mass as a whole, the content of the metal element compound (B1) can also be set to 70 parts by mass or less, 60 parts by mass or less, or 55 parts by mass or less.
[0042] In the ink composition of the present embodiment, the content of the other cationic polymerizable compound (B2) is preferably 5 to 80 parts by mass, more preferably 10 to 78 parts by mass, and further preferably 15 to 75 parts by mass, when the solid content of the ink composition as a whole is 100 parts by mass. By setting the content of the other cationic polymerizable compound (B2) to such a range, good curability can be exhibited, and the film quality of the obtained light-shielding component can be made good.
[0043] (Photoacid generator (C)) The ink composition of the present embodiment includes a photoacid generator (C). That is, when the ink composition of the present embodiment is exposed to light, the photoacid generator (C) generates an acid to promote the polymerization reaction of the cationically polymerizable compound (B). The photoacid generator (C) can be appropriately selected from known materials, but it is preferred that the photoacid generator (C) contains a sulfonium salt compound (C1). By using the sulfonium salt compound (C1), the ink composition can be effectively cured by light.
[0044] The sulfonium salt compound (C1) is a salt of a sulfonium cation and an anion.
[0045] Here, examples of the sulfonium cation include triphenylsulfonium, (4-tert-butoxyphenyl)diphenylsulfonium, bis(4-tert-butoxyphenyl)phenylsulfonium, tris(4-tert-butoxyphenyl), (3-tert-butoxyphenyl)diphenylsulfonium, bis(3-tert-butoxyphenyl)phenylsulfonium, tris(3-tert-butoxyphenyl)sulfonium, (3,4-di-tert-butoxyphenyl)diphenylsulfonium, bis(3,4-di-tert-butoxyphenyl)phenylsulfonium, tris(3,4-di-tert-butoxyphenyl)sulfonium, diphenylsulfonium, (4-(phenylthio)phenyl)sulfonium, (4-tert-butoxycarbonylmethoxyphenyl)diphenylsulfonium, tris(4-tert-butoxycarbonylmethoxyphenyl)sulfonium, (4-tert-butoxyphenyl)bis(4-dimethylaminophenyl)sulfonium, tris(4-dimethylaminophenyl)sulfonium, 2-naphthyldiphenylsulfonium, dimethyl-2-naphthylsulfonium, 4-hydroxyphenyldimethylsulfonium, 4-methoxyphenyldimethylsulfonium, trimethylsulfonium, 2-oxocyclohexylcyclohexylmethylsulfonium, trinaphthylsulfonium, tribenzylsulfonium and the like.
[0046] In addition, as anions, there can be mentioned anions of BF4-, PF6-, SbF6-, [BX4]- (X represents a phenyl group substituted with at least 2 fluorine or trifluoromethyl groups), [PFnY6-n]- (Y represents a fluorinated alkyl group or a fluorinated phenyl group having 1 to 9 carbon atoms, and n is an integer of 1 to 6), sulfonates, etc.
[0047] In addition, as the photoacid generator (C) (also referred to as other photoacid generator (C2)), an ionic photoacid generator other than sulfonium salts, a nonionic photoacid generator, or the like can be used. Specifically, other photoacid generators (C2) include phenyldiazonium salts of boron tetrafluoride; diphenyliodonium salts of phosphorus hexafluoride; diphenyliodonium salts of antimony hexafluoride; diphenyliodonium salts of tetrakis(pentafluorophenyl)boron; a mixture of aluminum acetylacetonate and o-nitrobenzylsilyl ether; phenylthiopyridinium salt; phosphorus hexafluoride allene-iron complex; sulfonyldiazomethane; N-sulfonyloxyimide-type photoacid generators such as phthalimide-type photoacid generators and naphthalimide-type photoacid generators, oxime-O-sulfonate-type photoacid generators, and the like.
[0048] In the ink composition of this embodiment, the photoacid generator (C) preferably contains a compound having a peak wavelength of 280 nm or more. By using such a compound, it is easy to form an industrially advantageous light-shielding component. Note that the compound having a peak wavelength of 280 nm or more may be equivalent to the sulfonium salt compound (C1) or to a compound of another photoacid generator (C2).
[0049] In the ink composition of the present embodiment, when the solid content of the ink composition as a whole is 100 parts by mass, the content of the photoacid generator (C) is preferably 0.1 parts by mass or more and 15 parts by mass or less, more preferably 0.5 parts by mass or more and 10 parts by mass or less, and even more preferably 1 part by mass or more and 8 parts by mass or less. By setting the content of the photoacid generator (C) to such a range, the curability of the ink composition can be made high while ensuring the storage stability of the ink composition.
[0050] Note that the mass ratio of the sulfonium salt compound (C1) in the entire photoacid generator (C) is preferably 80 mass % or more, more preferably 90 mass % or more, further preferably 95 mass % or more, and particularly preferably 98 mass % or more. In addition, the photoacid generator (C) may also be substantially composed of the sulfonium salt compound (C1). In this way, it is easier to exert the above-mentioned effects.
[0051] (Sensitizer (D)) The ink composition of the present embodiment contains a sensitizer (D). That is, the ink composition of the present embodiment can contain a light shielding agent (A) and ensure good curability by containing the sensitizer (D).
[0052] In addition, in the present embodiment, the sensitizer (D) includes a compound (D1) containing an anthracene skeleton. The present inventors have found that, among various sensitizers (D), by including the compound (D1) containing the anthracene skeleton in the ink composition, it is possible to ensure good curability of the ink composition while containing the light-shielding agent (A).
[0053] Examples of the compound (D1) containing an anthracene skeleton include anthracene, 9-anthracene methanol, 9-anthracene carboxylic acid, 9,10-diphenylanthracene, 9,10-bis(phenylethynyl)anthracene, 2-methoxyanthracene, 1,5-dimethoxyanthracene, 1,8-dimethoxyanthracene, 9,10-diethoxyanthracene, 9,10-dibutoxyanthracene, 9,10-bis(octanoyloxy)anthracene, 6-chloroanthracene, and 1,5-dichloroanthracene. These may be used alone or in combination of two or more.
[0054] The ink composition of the present embodiment may contain another sensitizer (D2) different from the above-mentioned anthracene skeleton-containing compound (D1). Other sensitizers (D2) include aromatic nitro compounds; coumarins; thiazolines; oxazolines; thioxanthones; benzothiazoles; nitroanilines; nitronaphthalene; benzoin alkyl ethers; N-alkylated phthalocyanines; naphthalenes; benzene; pyrene; benzopyran; azoindoline; fluorocoumarin; phenylthiazine; benzo[c]benzothiazine; 7-H-benzo[c]phenylthiazine; triethylenetetracycline; 1,3-dicyanobenzene; phenyl-3-cyanobenzoate, etc.
[0055] In the ink composition of the present embodiment, when the solid content of the ink composition as a whole is set to 100 parts by mass, the content of the sensitizer (D) is preferably from 0.05 parts by mass to 6 parts by mass, more preferably from 0.08 parts by mass to 4 parts by mass, and further preferably from 0.1 parts by mass to 2 parts by mass. By setting the content of the sensitizer (D) within such a range, the curability of the ink composition can be increased to a high level while ensuring the storage stability of the ink composition.
[0056] Note that the mass ratio of the anthracene skeleton-containing compound (D1) in the entire sensitizer (D) is preferably 80 mass % or more, more preferably 90 mass % or more, further preferably 95 mass % or more, particularly preferably 98 mass % or more. Furthermore, the sensitizer (D) may be composed only of the compound (D1) that does not substantially contain an anthracene skeleton. By doing so, it is easier to exert the above-mentioned effects.
[0057] (Solvent(S)) The ink composition of the present embodiment may contain a solvent (S) as a volatile component. By containing a solvent (S) in this way, the coating property of the ink composition of the present embodiment becomes excellent. The solvent (S) may use one or more of the well-known solvents in the field of printing ink. As the organic solvent, for example, one or more of alcohol solvents, ketone solvents, ester solvents, ether solvents, ether ester solvents, glycol ether solvents, amide solvents, carbonate solvents, etc. may be used.
[0058] Examples of the alcohol solvent include methanol, ethanol, isopropanol, 1-butanol, tert-butanol, isobutanol, diacetone alcohol, and 3-methoxy-3-methyl-1-butanol. Examples of the ketone solvent include acetone, methyl ethyl ketone, diethyl ketone, methyl isobutyl ketone, cyclopentanone, cyclohexanone, and diisobutyl ketone. Examples of the ester solvent include ethyl acetate, methyl acetate, butyl acetate, methoxybutyl acetate, cellosolve acetate, amyl acetate, n-propyl acetate, isopropyl acetate, methyl lactate, ethyl lactate, butyl lactate and the like. Examples of the ether solvent include dibutyl ether, tetrahydrofuran, and dioxane. Examples of the ether ester solvent include 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, and methyl methoxypropionate. Examples of the glycol ether solvent include ethylene glycol monomethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, propylene glycol monomethyl ether, and butyl cellosolve (ethylene glycol monobutyl ether). Examples of the amide solvent include N-methylpyrrolidone and N,N-dimethylformamide. Examples of the carbonate-based solvent include propylene carbonate, ethylene carbonate, dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate.
[0059] When the ink composition of the present embodiment contains a solvent (S), the content of the solvent (S) may be arbitrary. For example, the content of the solvent (S) may be set so that the solid content concentration of the ink composition is in the range of 60 to 100% by mass. Note that the ink composition of this embodiment can also be implemented as a method that does not substantially contain the above-mentioned solvent (S). Note that in this specification, "substantially free of" is used to exclude the method of intentionally adding a predetermined component, and the method of inevitably mixing a predetermined component in the manufacturing process should be within the allowable range. In the exemplary process, before exposing the ink composition of this embodiment, it is necessary to heat and remove the solvent (S). When the ink composition does not substantially contain a solvent (S), such a heating process can be omitted, so it is preferred.
[0060] (Other additives) The ink composition of this embodiment may contain additional ingredients other than the above-mentioned ingredients. The additional ingredients include a surface conditioner, such as a silicone compound, wax, a defoamer, a leveling agent, an anti-wrinkle agent (a component that destroys air entrained during the coating process), etc.
[0061] Examples of surface conditioners include Acronal (registered trademark) series such as Acrolein 4F (manufactured by BAS F, (meth) acrylic resin series), BYK series (manufactured by BYK), Polyflow series (manufactured by Kyoeisha Chemical Co., Ltd.), Resiflow series (manufactured by Estrone Chemical), and Modaflow series (manufactured by Mon santo).
[0062] The ink composition of this embodiment may contain only one surface conditioner, or may contain two or more surface conditioners. In addition, the amount of the surface conditioner in the ink composition of this embodiment is not particularly limited and may be appropriately adjusted in consideration of the balance between other properties.
[0063] The ink composition of this embodiment may contain fillers, coupling agents, antioxidants, viscosity modifiers, storage stabilizers, dispersants, etc. as other additives. The amounts of these agents in the ink composition of this embodiment are not particularly limited and can be appropriately adjusted according to the balance between other properties.
[0064] (Method for producing ink composition) The ink composition of the present embodiment is typically prepared by mixing the above-mentioned components.
[0065] As a more specific example, the ink composition of this embodiment can be produced according to the following procedure. (Step 1): A dispersion containing the light-shielding agent (A) is obtained by dispersing the light-shielding agent (A) in a dispersion medium. (Step 2): The obtained dispersion is mixed with other materials.
[0066] That is, in the above-described method, a dispersion containing the light-shielding agent (A) is once obtained in (step 1), and the dispersion is mixed with other materials to obtain a desired ink composition. As the dispersion medium used when obtaining the dispersion liquid, various materials capable of dispersing the light-shielding agent (A) can be used. For example, when the cationically polymerizable compound (B) is in liquid form, the cationically polymerizable compound (B) may be used as a dispersion medium. In addition, a dispersant (sometimes also referred to as an anti-settling agent or a dispersing aid) may be coexistent in order to improve the dispersibility of the dispersion. The dispersant may be a known one, and a typical example is a polymer dispersant. Commercially available dispersants may be used, and specific examples thereof include Flowlen DOPA series (manufactured by Kyoeisha Chemical Co., Ltd.), Solsperce series (manufactured by Nippon Lubrizol Co., Ltd.), Ajispur series (manufactured by Ajinomoto Fine-Techno Co., Inc.), Disper BYK series (manufactured by BYK), and Disparlon series (manufactured by Kusumoto Chemicals Co., Ltd.). The mixing ratio of the dispersant in the dispersion can be appropriately set depending on the type etc., and is, for example, in the range of 10 to 100 parts by mass, and preferably in the range of 20 to 70 parts by mass, relative to 100 parts by mass of the light-shielding agent (A).
[0067] Next, the dispersion obtained in the above (Step 1) is mixed with other materials in (Step 2). In the above (Step 2), the mixing method is not particularly limited. In this way, the desired ink composition can be obtained.
[0068] (use) The ink composition of this embodiment is used, for example, to form a light shielding component in an image display device. Examples of the image display device include a liquid crystal display device having a backlight and a liquid crystal unit, or a display device having a light-emitting element such as an OLED (Organic Light Emitting Diode) element, a mini LED (mini Light Emitting Diode; micro LED) element, or a quantum dot. The ink composition of this embodiment is cured by exposure to form a cured film, so that it can function as a shading member in an image display device. Typically, the shading member is arranged in a display area in the image display device to display an image. Here, the display area is an area in the image display device that is defined by connecting pixels that can be recognized by the person opposite to the image display device and the viewpoint of the person opposite to the image display device. That is, although the edge portion of the so-called display is excluded, it is assumed that the black matrix of the RG B pattern of the color filter separated and arranged in the liquid crystal display device exists in the display area. In addition, when the image display device has multiple light-emitting elements, the light-shielding member formed by the ink composition of this embodiment can also be arranged between the multiple light-emitting elements. In this case, the light-shielding member plays a function of alleviating the interference of light between adjacent light-emitting elements when the light-emitting element emits light.
[0069] An example of an image display device having such a light shielding member will be described below with reference to the drawings. Figure 1 It is a cross-sectional view of an image display device using a cured product of the ink composition according to the present embodiment as a light shielding member. Figure 1 The image display device 100 in the figure includes a substrate 10, a light-emitting element 20 and a light-shielding component 30. The substrate 10 of the image display device 100 is made of a material selected from various materials, and can be made of an inorganic material or an organic material. As a typical example, the substrate 10 is a glass substrate, but in addition to this, it can also be a composite material composed of glass fiber and epoxy resin, or a substrate composed of other ceramics. Note that although the details are not described in the figure, a circuit or electrode is typically provided on the substrate 10, which is configured to be able to apply current to the light-emitting element 20. Note that the circuit or the electrode may also be made of copper, indium tin oxide, or the like.
[0070] The light emitting element 20 is typically a mini LED or a micro LED, and the light emitting element 20 (R), the light emitting element 20 (G), and the light emitting element 20 (B) emit red, green, and blue light, respectively. Note that the light emitting element 20 included in the image display device 100 of this embodiment may also be an OLED.
[0071] The light shielding member 30 is formed by curing the ink composition of the present embodiment, and is disposed between a plurality of light emitting elements 20. As described above, the light shielding member 30 has a function of alleviating interference of light with adjacent light emitting elements 20 when the light emitting element 20 emits light. Note that, in the light shielding member 30 of the present embodiment, since it is formed by a specific ink composition, it has excellent adhesion to the substrate 10, and can stably exhibit such a function even in the case of long-term use.
[0072] Such a light shielding member 30 is applied to the substrate 10 on which the light emitting elements 20 are mounted so that the ink composition is arranged between the light emitting elements 20, thereby photocuring the ink composition. Such application is performed using an inkjet printer (i.e., the ink composition of this embodiment may also be inkjet). Figure 1 , the shading member 30 is arranged at a position in contact with the light emitting element 20, but the shading member 30 and the light emitting element 20 may be separated. In addition, the heights of the shading member 30 and the light emitting element 20 (the thickness in the film thickness direction of the substrate 10) may be different. When the light shielding member 30 is obtained from the ink composition of this embodiment, the thickness of the light shielding member 30 may be 25 μm or less, or 20 μm or less, for example, from the viewpoint of easily obtaining a uniform film quality in the film thickness direction. Note that the thickness of the light shielding member 30 may be greater than the above value from the viewpoint of suppressing interference of light emitted from the light emitting elements 20. When forming such a light shielding member 30, for example, the following method may be employed. That is, the ink composition can be adjusted to a film thickness that can be cured by light exposure, temporarily exposed and cured, and a coating film based on the ink composition is further formed on the cured film to form a light-shielding component 30 with a high film thickness (in other words, the light-shielding component 30 can also be formed by stacking cured films of the ink composition). Therefore, the thickness of the light shielding member 30 can be designed to be greater than the above thickness as needed. As an example, the thickness of the light shielding member 30 can be less than 300 μm, or less than 200 μm. In addition, from the perspective of improving the film quality of the light shielding member 30, a heating process can also be performed after the laminated cured film to increase the degree of cross-linking of the film.
[0073] In order to improve the reliability of the image display device 100, the hardness of the light shielding member 30 may be adjusted. As an example, the pencil hardness of the light shielding member 30 may be H or higher, 2H or higher, 3H or higher, or 4H or higher.
[0074] In addition, it can also be provided in various ways as described below. [α1] An ink composition comprising: A sunscreen (A), a cationic polymerizable compound (B), a photoacid generator (C) and a sensitizer (D); wherein: The volume concentration of the light-shielding agent (A) is 0.3% to 12% relative to the total volume of the solid content of the ink composition, The cationically polymerizable compound (B) comprises a metal element-containing compound (B1) having a cationically polymerizable group and a hydrolyzable group, The content of the metal element-containing compound (B1) is 5 parts by mass or more and 80 parts by mass or less based on 100 parts by mass of the total solid content of the ink composition. The sensitizer (D) includes a compound (D1) having an anthracene skeleton. [α2] The ink composition according to [α1], wherein the content of the light-shielding agent (A) is 0.6 parts by mass or more and 18 parts by mass or less based on 100 parts by mass of the total solid content of the ink composition. [α3] The ink composition according to [α1] or [α2], wherein the light-shielding agent (A) includes carbon black (A1) or an inorganic light-shielding agent (A2-1). [α4] The ink composition according to any one of [α1] to [α3], wherein the metal element-containing compound (B1) is a silicon-containing compound. [α5] The ink composition according to any one of [α1] to [α4], wherein the cationically polymerizable group possessed by the metal element-containing compound (B1) is an epoxy group. [α6] The ink composition according to any one of [α1] to [α5], wherein the cationically polymerizable compound (B) further contains another cationically polymerizable compound (B2) that does not belong to the metal element-containing compound (B1). [α7] The ink composition according to any one of [α1] to [α6], wherein the photoacid generator (C) contains a sulfate compound (C1). [α8] The ink composition according to any one of [α1] to [α7] is an ink composition for inkjet. [α9] The ink composition according to any one of [α1] to [α8], which is used to form a light shielding member provided in an image display device. [α10] The ink composition according to [α9], wherein the light shielding member is provided in a display area where an image is displayed in the image display device. [α11] The ink composition according to [α10], wherein the image display device has a plurality of light-emitting elements, and the light-shielding member is provided between the plurality of light-emitting elements. [α12] A light shielding member formed by curing the ink composition described in any one of [α1] to [α11]. [α13] An image display device comprising the light-shielding component described in [α12]. [β1] An ink composition comprising: A sunscreen (A), a cationic polymerizable compound (B), a photoacid generator (C) and a sensitizer (D); wherein: When the total solid content of the ink composition is 100 parts by mass, the content of the metal element-containing compound (A) is 3 parts by mass or more and 14 parts by mass or less, The cationically polymerizable compound (B) comprises a metal element-containing compound (B1) having a cationically polymerizable group and a hydrolyzable group, The sensitizer (D) includes a compound (D1) having an anthracene skeleton. [β2] In the ink composition according to [β1], the light-shielding agent (A) includes carbon black (A1). [β3] The ink composition according to [β1] or [β2], wherein the metal element-containing compound (B1) is a silicon-containing compound. [β4] The ink composition according to any one of [β1] to [β3], wherein the cationically polymerizable group possessed by the metal element-containing compound (B1) is an epoxy group. [β5] The ink composition according to any one of [β1] to [β4], wherein the cationically polymerizable compound (B) further contains another cationically polymerizable compound (B2) that does not belong to the metal element-containing compound (B1). [β6] The ink composition according to any one of [β1] to [β5], wherein the content of the metal element-containing compound (B1) is 3 parts by mass or more and 80 parts by mass or less per 100 parts by mass of the total solid content of the ink composition. [β7] The ink composition according to any one of [β1] to [β6], wherein the photoacid generator (C) contains a sulfate compound (C1). [β8] The ink composition according to any one of [β1] to [β7] is an ink composition for inkjet. [β9] The ink composition according to any one of [β1] to [β8], which is used to form a light shielding member provided in an image display device. [β10] The ink composition according to [β9], wherein the light shielding member is provided in a display area where an image is displayed in the image display device. [β11] The ink composition according to [β10], wherein the image display device has a plurality of light-emitting elements, and the light-shielding member is provided between the plurality of light-emitting elements. [β12] A light shielding member formed by curing the ink composition described in any one of [β1] to [β11]. [β13] An image display device comprising the light-shielding component described in [β12].
[0075] Although the embodiments of the present invention have been described above, these embodiments are only provided as examples, and other various structures may also be adopted. In addition, the present invention is not limited to the above embodiments, and various changes and improvements are included in the scope of the present invention within the scope of achieving the purpose of the present invention. (Example)
[0076] Hereinafter, the present invention will be described in more detail by way of examples and comparative examples. It should be noted that the present invention is not limited to the following examples.
[0077] (Raw materials used) First, the raw materials used in this example are described. The various raw materials used in this example are as follows. ·A1-1: Mitsubishi Carbon Black MA7 (manufactured by Mitsubishi Chemical Corporation) · A2-1: TilackD TM-A (titanium black; manufactured by Ako Chemicals Co., Ltd.) B1-1: KBM-403 (chemical name: 3-glycidoxypropyltrimethoxysilane; manufactured by Shin-Etsu Chemical Co., Ltd.) B1-2: KBM-303 (chemical name: 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; manufactured by Shin-Etsu Chemical Co., Ltd.) B2-1: Aron Oxetane OXT-221 (chemical name: 3-ethyl-3{[3-ethyloxetan-3-il]methoxy}methyl)oxetane; manufactured by Toagosei Co., Ltd.) B2-2: Celloxide 2021P (chemical name: 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate; manufactured by Daicel Co., Ltd.) B2-3: Limonene oxide (manufactured by RENESSENZ, LLC.) ·B2-4: 3,3-Bis[(2-oxophenylmethoxy)methyl]oxetane · B2-5: Decanediol EX-141 (chemical name: phenyl glycidyl ether; manufactured by Nagase Chemtex Co., Ltd.) · B2-6: Decanediol EX-121 (chemical name: 2-ethylhexyl glycidyl ether; manufactured by Nagase Chemtex Co., Ltd.) C1-1: CPI-110P (chemical name: diphenyl[4-(phenylthio)phenyl]sulfonium hexafluorophosphate; manufactured by San-Apro Co., Ltd.) C1-2: CPI-110B (chemical name: diphenyl[4-(phenylthio)phenyl]sulfoniumtetrakis(pentafluorophenyl)borate; manufactured by San-Apro Co., Ltd.) · D1-1: Anthracure (registered trademark) UVS-1331 (chemical name: 9,10-dibutoxyanthracene; manufactured by Air Water Performance Chemical Co., Ltd.) · D1-2: Anthracure (registered trademark) UVS-581 (chemical name: 9,10-bis(octanoyloxy)anthracene; manufactured by AirWater Performance Chemical Co., Ltd.) D2-1: Omnirad DETX (chemical name: 2-methyl-[4-(methylthio)phenyl]-2-morpholine-1-propane; manufactured by IGM RESINS) ·X-1: Ajispur PB824 (pigment dispersant; manufactured by Ajinomoto Fine-Techno Co., Inc.) ·X-2: DISPER BYK-2013 (pigment dispersant; manufactured by BYK) ·X-3: BYK-361N (polyacrylate surface conditioner; manufactured by BYK) ·S-1: Propylene glycol monomethyl ether acetate
[0078] The B2-4 components are synthesized in the order described in Synthesis Example B of Japanese Patent Publication No. 2019-077674.
[0079] (Preparation of ink composition, etc.) The pigment dispersion and ink composition were prepared according to the following steps. (Preparation of Pigment Dispersion) After premixing various materials in the ratios shown in Tables 1 and 2, the materials were processed in a sand mill for 4 hours to obtain a pigment dispersion containing a predetermined light-shielding agent.
[0080] (Manufacturing of ink composition) The pigment dispersion obtained above was fully mixed with the components listed in Tables 1 and 2 to produce an ink composition. Note that each table also lists the content ratio (mass %) of the component (A) and the content ratio (mass %) of the component (B1) relative to the total solid content of the ink composition.
[0081] In addition, Tables 1 and 2 show the specific gravity (solid content only) of the ink composition and the volume concentration of the light shielding agent (A) in the obtained ink composition.
[0082] The specific gravity of the ink composition (solid content only) was determined by adjusting the ink temperature to 20° C. using a constant temperature water tank, and then the true density (true specific gravity) was measured using a float to obtain a numerical value.
[0083] In addition, when obtaining the volume concentration of the light-shielding agent (A), the true density of the pigment used was measured as follows. That is, the true density of the pigment is measured according to Japanese Industrial Standard (JIS standard) JIS Z 8807 (2012). Specifically, 10 g of each pigment is collected in a Gay-Lussac Type (Pycnometer), a solvent having a smaller specific gravity than each pigment is introduced, and the weight of the pycnometer alone, the pycnometer + pigment, the pycnometer + pigment + solvent, and the pycnometer + solvent is measured respectively, and the weight is calculated according to the following formula. [Formula 1] Wherein, d: true density of pigment, d0: density of solvent, Wa: weight of specific gravity bottle, Wb: weight of specific gravity bottle + powder, Wc: weight of specific gravity bottle + powder + solvent, Wd: weight of specific gravity bottle + solvent. Each weight measurement was performed by placing the sample in a constant temperature water bath at 20°C for 1 hour and adjusting the temperature before measurement. Before measuring the weight of the pycnometer + pigment + solvent, an ultrasonic disperser is used to fully degas the voids in the pigment with the solvent.
[0084] (evaluate) The obtained ink composition was evaluated according to the following items. The obtained evaluation results are shown in Tables 1 and 2.
[0085] <Curing Properties> As an inkjet printer, an inkjet printer (Tritek Co., Ltd., Stage JET) equipped with a piezoelectric inkjet head (Konica Minolta, KM1024iMHE, ink droplet volume 13pL) was prepared. Each ink composition was filled with the printer and ejected at a nozzle temperature of 35°C. Eagle XG (Display Grade Glass made by Corning (registered trademark)) was used for the coating substrate. In addition, the coating amount was set to a coating amount that could form a film thickness of 550nm with a transmittance of less than 0.1%. Next, ultraviolet rays were irradiated under the following conditions using a UV irradiation device (USHIO (model) UVX-516, lamp: USHIO (TYPE) UVH-0501C-1200). In addition, the irradiation intensity and cumulative irradiation amount at this time were measured using a digital illuminometer (Igraphics, model: UVPF-A1, photoreceiver: PD-365). Condition 1: Irradiation at an output of 120 W for 15 seconds. The irradiation intensity is 30mW / cm2 and the cumulative irradiation is 450mJ / cm2. Condition 2: Irradiation at an output of 120 W for 30 seconds. The irradiation intensity is 30mW / cm2 and the cumulative irradiation is 900mJ / cm2. Condition 3: Irradiation at an output of 120 W for 45 seconds. The irradiation intensity is 30mW / cm2 and the cumulative irradiation is 1350mJ / cm2.
[0086] Furthermore, within 10 seconds after the irradiation, the curing state of the coated material was evaluated according to the following evaluation criteria. A···Fully cured, no tack. B···It is sticky and leaves fingerprints when touched with fingers, but the ink component does not adhere to fingers. C···It is sticky. When you touch the coating with your fingers, the ink components will adhere to your fingers.
[0087] <Concealment> The coated substrates obtained in each of the Examples and Comparative Examples after ultraviolet irradiation were heated in a vault-type oven set at an internal temperature of 130°C for 10 minutes to obtain evaluation substrates. In addition, the ultraviolet irradiation amount of each Example and Comparative Example was the minimum ultraviolet irradiation amount for which the curability evaluation value was A. Note that even when 1350mJ / cm2 was irradiated, the sample A was not evaluated. The transmittance in the 540 to 560 nm region was measured using an ultraviolet visible spectrophotometer (using an integrating sphere, manufactured by Shimadzu Corporation, SolidSpec-3700), and the average value was defined as the transmittance at 550 nm. The concealment was evaluated according to the following evaluation criteria. A: Transmittance ≤ 1% B: Transmittance>1%
[0088] <Appearance> In the evaluation substrate, the appearance was evaluated according to the following evaluation criteria. A: No abnormality B: Wrinkles appear near the edges C: Wrinkles appear on the entire coating film
[0089] <Workability> In the curability test described above, the number of coating passes required to achieve a film thickness of 1% or less in transmittance at 550 nm was determined. Tables 1 and 2 show the film thickness formed by one coating pass, the number of coating passes, and the total film thickness. In the primary coating, inkjet coating is performed, followed by exposure and heating to obtain a cured film. In the case of double coating, inkjet coating is performed once and then light exposure is performed, and after this exposure, inkjet coating and light exposure are further performed, and heating is further performed. In the case of triple coating, the combination of inkjet coating and light exposure is performed three times, and finally a cured film is obtained by heating.
[0090] The workability was evaluated according to the following evaluation criteria, and the results are shown in Tables 1 and 2. Generally, when the number of processes increases, the tact time increases, the probability of abnormal phenomena such as foreign matter mixing increases, and the yield rate tends to decrease. A: 1 coating B: 2nd coating C: 3 or more coats
[0091] In the ink composition of Comparative Example 1, the film thickness of one coating was set to 50 μm, and the coating was repeated until the transmittance described above was satisfied. However, in this case, the number of coatings was 4, and the evaluation of <Workability> became C (see Comparative Example 1A in Table 1). Therefore, when the number of coatings was limited to 2 times while maintaining the condition of the film thickness of one coating being 50 μm, the evaluation of <Hiddenness> became low (see Comparative Example 1B in Table 1). When the film thickness of one coating increases to 90 μm, although the balance between <hiding property> and <workability> is relatively good, the evaluation of <appearance> deteriorates (see Comparative Example 1C in Table 1). Therefore, the ink composition of Comparative Example 1 still has problems in effectively producing a material with high light-shielding properties.
[0092] <Adhesion> A substrate for evaluating adhesion was prepared in the same manner as the substrate for evaluating concealment. Although Eagle XG was used as the concealment evaluation substrate, the adhesion evaluation substrate was further coated and cured in the same manner on a glass epoxy substrate (manufactured by Sunhayato; single-sided glass epoxy resin FR-4) and a glass substrate with a transparent conductive film (ITO film) (manufactured by Hiraoka Special Glass Co., Ltd.; variety 25Ω) to produce an adhesion evaluation substrate. In addition, the ITO film glass substrate was heated in a vault-type oven set to an internal temperature of 180°C for 10 minutes. Regarding the adhesion, the adhesion between the cured film and the substrate was evaluated by cross-cutting test in accordance with JIS K5600-5-6:1999, with slits opened at 1 mm intervals when the film thickness is less than 60 μm, and with slits opened at 2 mm intervals when the film thickness is 60 μm or more. Regarding this evaluation, 0 to 4 for each substrate is within the practical range, but 0 to 3 is more preferably set. 0: The cut edge is completely smooth, with no peeling of any mesh. 1: There is a small amount of peeling of the coating at the cross-cut point. The affected area at the cross-cut part is obviously not more than 5%. 2: The coating peels off along the cut edges and / or at the intersections. The affected area of the cross-cut portion is significantly more than 5%, but not more than 15%. 3: The coating peels off partially or completely along the cut edge and / or peels off partially or completely in various parts of the point. The area affected in the cross-cut section is significantly more than 15%, but not more than 35%. 4: Extensive partial or full flaking of the coating along the cut edge and / or partial or full flaking at multiple locations. The affected area in the cross-cut section will not exceed 65% significantly. 5: Any degree of peeling that cannot be classified in category 4.
[0093] <Pencil Hardness> The same method as the concealment evaluation substrate was used to prepare a pencil hardness evaluation substrate. The evaluation substrate was used to evaluate pencil hardness according to the test method of JIS-K5600-5-4. The pencil was made by MITSU-BISHI and the test machine was a pencil scratch hardness tester manufactured by Toyo Seiki Seisakusho.
[0094]
Table 1
[0095]
Table 2
[0096] The results of this example show that the ink composition of this example can provide a cured product having an excellent balance between substrate adhesion and light shielding properties while maintaining the curability of the ink composition. Description of Reference Numerals
[0097] 10: Substrate 20: Light-emitting element 30: Light shielding parts 100: Image display device
Claims
1. An ink composition, It is characterized in that It comprises: a light shielding agent (A), a cationic polymerizable compound (B), a photoacid generator (C) and a sensitizer (D); wherein: The volume concentration of the light-shielding agent (A) is 0.3% to 12% relative to the total volume of the solid content of the ink composition, The cationically polymerizable compound (B) comprises a metal element-containing compound (B1) having a cationically polymerizable group and a hydrolyzable group, When the total solid content of the ink composition is 100 parts by mass, the content of the metal element-containing compound (B1) is 5 parts by mass or more and 80 parts by mass or less. The sensitizer (D) includes a compound (D1) containing an anthracene skeleton.
2. The ink composition according to claim 1, It is characterized in that When the total solid content of the ink composition is 100 parts by mass, the content of the light shielding agent (A) is 0.6 parts by mass or more and 18 parts by mass or less.
3. The ink composition according to claim 1 or 2, It is characterized in that The sunscreen agent (A) contains carbon black (A1) or an inorganic sunscreen agent (A2-1).
4. The ink composition according to any one of claims 1 to 3, It is characterized in that The metal element-containing compound (B1) is a silicon-containing compound.
5. The ink composition according to any one of claims 1 to 4, It is characterized in that The cationically polymerizable group possessed by the metal element-containing compound (B1) is an epoxy group.
6. The ink composition according to any one of claims 1 to 5, It is characterized in that The cationically polymerizable compound (B) further contains another cationically polymerizable compound (B2) which does not belong to the metal element-containing compound (B1).
7. The ink composition according to any one of claims 1 to 6, It is characterized in that The photoacid generator (C) contains a sulfate compound (C1).
8. The ink composition according to any one of claims 1 to 7, It is characterized in that This is an ink composition for inkjet.
9. The ink composition according to any one of claims 1 to 8, It is characterized in that Used to form a light shielding member provided in an image display device.
10. The ink composition according to claim 9, It is characterized in that The light shielding member is disposed in a display area of the image display device where an image is displayed.
11. The ink composition according to claim 10, It is characterized in that The image display device includes a plurality of light emitting elements, and the light shielding member is provided between the plurality of light emitting elements.
12. A light shielding component, It is characterized in that The ink composition according to any one of claims 1 to 11 is cured.
13. An image display device, It is characterized in that A light shielding member according to claim 12 is provided.