Polishing composition

By using sodium permanganate and transition metal salt in the grinding composition, a multi-component composition is formed, and the problem of insufficient removal speed in grinding of high-hardness materials is solved, and efficient grinding effect and stability improvement are achieved.

CN118974199APending Publication Date: 2024-11-15FUJIMI INCORPORATED
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380031724.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2023-03-13
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The conventional polishing compositions are insufficient in the removal rate of high-hardness materials, and the solubility of oxidants such as potassium permanganate is low, making it difficult to form high-concentration compositions, which affects the grinding efficiency.

Method used

Sodium permanganate is used as an oxidant, combining transition metal salts and abrasive particles to form a multi-component grinding composition, improving the content and stability of the oxidant, inhibiting pH changes, and optimizing grinding conditions.

Benefits of technology

The grinding removal speed is significantly improved, the storage stability and grinding efficiency of the composition are enhanced, and suitable for the grinding of high-hardness materials such as silicon carbide, improving productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005066511390000301
    Figure BDA0005066511390000301
  • Figure BDA0005066511390000331
    Figure BDA0005066511390000331
Patent Text Reader

Abstract

Provided is a polishing composition capable of achieving an excellent polishing removal rate with respect to an object to be polished. The polishing composition provided by the invention is used for polishing an object to be polished. The polishing composition contains water, sodium permanganate as an oxidizing agent, and a transition metal salt different from the oxidizing agent, and contains more than 10 wt% of the oxidizing agent. In some preferred ways, the transition metal salt is an oxygen transition metal salt, or a polynuclear transition metal complex comprising a transition metal and oxygen and / or hydrogen. The polishing composition is also preferably applied to polishing of an object to be polished comprising a high-hardness material having a Vickers hardness of 1500 Hv or more.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a polishing composition. This application claims priority based on Japanese Patent Application No. 2022-056781 filed on March 30, 2022, the entire contents of which are incorporated herein by reference. Background Art

[0002] Use grinding composition to grind the surface of materials such as metal, semimetal, nonmetal, its oxide.For example, for the surface consisting of compound semiconductor materials such as silicon carbide, boron carbide, tungsten carbide, silicon nitride, titanium nitride, gallium nitride, by supplying diamond abrasive between its surface and the grinding plate and grinding (grinding (lapping)) to process.But, in the grinding using diamond abrasive, easily due to the generation of scratches, dents, residual etc. and produce defects, deformation.Therefore, after the grinding using diamond abrasive or instead of this grinding, the grinding (polishing (polishing)) using abrasive pad and grinding composition is studied.As the document of disclosing such prior art, patent documentation 1 can be cited.

[0003] Prior art literature

[0004] Patent Literature

[0005] Patent Document 1: International Publication No. 2016 / 072370 Summary of the invention

[0006] Usually, from the perspective of manufacturing efficiency and cost-effectiveness, it is expected that the grinding removal rate is fast enough in practical aspects. For example, in the grinding of the surface composed of high hardness materials such as silicon carbide, it is strongly desired to improve the grinding removal rate. In the grinding of substrates composed of such high hardness materials, in order to improve the grinding removal rate, in addition to using abrasive grains that play a physical grinding effect, it is also effective to chemically deteriorate the grinding object surface and make it brittle. Sometimes it is expected that this effect can be obtained so that the grinding composition contains an oxidant. For example, a grinding composition is proposed in patent document 1, which comprises oxidants such as abrasive grains, water and potassium permanganate, and is used for the grinding of substrates composed of high hardness materials.

[0007] In the grinding of various grinding objects including substrates composed of high hardness materials such as those described above, it is practically meaningful if a higher grinding removal rate can be obtained. In order to further increase the grinding removal rate, for example, it is considered effective to increase the concentration of the oxidant contained in the grinding composition. However, the oxidants such as potassium permanganate used in the past in this field tend to have a low solubility in water, and it is difficult to obtain a grinding composition containing a high concentration of oxidant.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a polishing composition that can achieve an excellent polishing removal rate for an object to be polished.

[0009] The present inventors have noted that sodium permanganate has higher solubility in water than other permanganates conventionally used in this field, and have found that the content of the oxidant in the polishing composition can be suitably increased by using sodium permanganate as the oxidant.

[0010] The polishing composition provided in this specification comprises water, sodium permanganate as an oxidant, and a transition metal salt different from the oxidant, and comprises more than 10% by weight of the oxidant. According to the polishing composition, the polishing removal rate can be stably increased while suppressing the performance change of the polishing composition during polishing (for example, the decrease of the polishing removal rate, etc.).

[0011] In some embodiments, the transition metal salt is an oxytransition metal salt or a polynuclear transition metal complex containing a transition metal and oxygen and / or hydrogen. By using the above metal salt, it is easy to suppress the pH change of the polishing composition during polishing of the polishing object.

[0012] In some embodiments, the polishing composition further comprises abrasive grains. The use of abrasive grains can increase the polishing removal rate.

[0013] In some embodiments, the pH of the polishing composition is 1.0 or higher and less than 6.0. In this pH range, the polishing composition disclosed herein tends to exhibit a high polishing removal rate.

[0014] The grinding composition disclosed herein is, for example, used for grinding materials with a Vickers hardness of 1500 Hv or more. In the grinding of such high-hardness materials, the effect produced by the technology disclosed herein can be preferably exerted. The application effect of the present invention can be more suitably exerted. In some embodiments, the material with a Vickers hardness of 1500 Hv or more is a non-oxide (i.e., a compound that is not an oxide). In the grinding of a non-oxide grinding object material, it is easy to suitably exert the effect of increasing the grinding removal rate produced by the grinding composition disclosed herein.

[0015] The polishing composition disclosed herein is used, for example, for polishing silicon carbide. In the polishing of silicon carbide, the effect of the technology disclosed herein can be preferably exerted.

[0016] According to the specification, a grinding method for a grinding object is also provided. The grinding method includes a process of grinding the grinding object using any grinding composition disclosed herein. According to the grinding method, even when grinding the grinding object composed of a high hardness material, the grinding removal rate can be increased. Thus, the productivity of the target product (grinding object, for example, a compound semiconductor substrate such as a silicon carbide substrate) obtained by grinding using the above-mentioned grinding method can be improved.

[0017] In addition, the polishing composition provided in this specification is a multi-component polishing composition, which comprises: Part A, which comprises sodium permanganate and water as an oxidant; Part B, which comprises a transition metal salt different from the oxidant and water, and the multi-component polishing composition comprises more than 10% by weight of the oxidant. According to the multi-component polishing composition, the storage stability of the polishing composition can be improved.

[0018] In some embodiments, the transition metal salt is an oxytransition metal salt or a polynuclear transition metal complex containing a transition metal, oxygen and hydrogen. By using the above metal salt, it is easy to suppress the pH change of the polishing composition during polishing of the polishing object.

[0019] In some embodiments, part A or part B contains abrasive particles.

[0020] In some embodiments, a part C different from part A and part B is further included, and part C contains abrasive particles.

[0021] The multi-component grinding composition disclosed herein is, for example, used for grinding materials with a Vickers hardness of 1500 Hv or more. In the grinding of such high-hardness materials, the effect produced by the technology disclosed herein can be preferably exerted. The application effect of the present invention can be more suitably exerted. In some embodiments, the material with a Vickers hardness of 1500 Hv or more is a non-oxide (i.e., a compound that is not an oxide). In the grinding of a non-oxide grinding object material, it is easy to suitably exert the effect of increasing the grinding removal rate produced by the grinding composition disclosed herein.

[0022] The multi-component polishing composition disclosed herein is used, for example, for polishing silicon carbide. In the polishing of silicon carbide, the effect of the technology disclosed herein can be preferably exerted.

[0023] According to the specification, a grinding method for a grinding object is also provided. The grinding method includes a process of grinding the grinding object using any multi-component grinding composition disclosed herein. The multi-component grinding composition is obtained, for example, by mixing part A and part B, and when part C is also included, the part C is also mixed. The grinding is performed using the grinding composition mixed in this way. According to the grinding method, even when grinding an object to be ground consisting of a high hardness material, the grinding removal rate can be increased. Thus, the productivity of the target product (grinding material, for example, a compound semiconductor substrate such as a silicon carbide substrate) obtained by grinding using the above-mentioned grinding method can be improved. DETAILED DESCRIPTION

[0024] The preferred embodiments of the present invention are described below. It should be noted that, for the contents necessary for the implementation of the present invention other than the matters specifically described in this specification, they can be mastered as conventional technical means based on the prior art in the field by those skilled in the art. The present invention can be implemented based on the contents disclosed in this specification and the technical common sense in the field.

[0025] <Polishing composition>

[0026] (Oxidant)

[0027] The grinding composition disclosed herein includes an oxidant. The oxidant is effective in reducing the hardness of the grinding object material (for example, a non-oxide material with high hardness such as silicon carbide) and making the material brittle. Therefore, in the polishing of the grinding object material, the oxidant can play an effect of increasing the grinding removal rate. In this specification, the oxidant does not include the transition metal salt C, metal salt A and metal salt B described later.

[0028] The grinding composition disclosed herein is characterized in that it contains sodium permanganate as an oxidant. Compared with other permanganates such as potassium permanganate, sodium permanganate has a tendency to show high solubility in water. Therefore, according to the composition containing sodium permanganate as an oxidant, it is easy to appropriately increase the content of the oxidant in the grinding composition. If such sodium permanganate, it is easy to increase the grinding removal rate.

[0029] From the perspective of improving the grinding removal rate, the content of sodium permanganate in the grinding composition exceeds 10 weight %. From making full use of the feature that sodium permanganate shows high solubility in water, it is easy to realize the perspective of higher grinding removal rate, in some ways, the content of sodium permanganate can be more than 15 weight %, can be more than 20 weight %, or can be more than 22 weight %. In addition, in some ways, it is appropriate that the content of sodium permanganate in the grinding composition is set to about 45 weight %, preferably set to less than 40 weight %, more preferably less than 35 weight %, further preferably less than 30 weight %, can be less than 25 weight %, can be less than 20 weight %, or can be less than 15 weight %. From the perspective of reducing the generation of defects caused by the sodium that may remain after grinding, it is advantageous to reduce the content of sodium permanganate.

[0030] The polishing composition disclosed herein may further contain an oxidant other than sodium permanganate (hereinafter referred to as "other oxidants"). Specific examples of compounds that can be selected as other oxidants include peroxides such as hydrogen peroxide; permanganic acids such as permanganate and its salts other than sodium permanganate (e.g., potassium permanganate); periodic acids such as periodic acid and its salts of sodium periodate and potassium periodate; iodic acids such as iodic acids such as ammonium iodate; bromic acids such as bromic acids such as its salts of potassium bromate; ferric acids such as ferric acids such as its salts of potassium ferrate; perchromic acid, chromic acid and its salts of potassium chromate; dichromic acids such as chromic acids and dichromic acids such as its salts of vanadium; Acid, vanadic acid, ammonium vanadate, sodium vanadate, potassium vanadate and other vanadic acids such as its salts; ruthenic acids such as perruthenic acid or its salts; permolybdic acid, molybdic acid, ammonium molybdate, disodium molybdate and other molybdic acids such as its salts; rhenic acid such as perrhenic acid or its salts; pertungstic acid, tungstic acid, disodium tungstate and other tungstic acids such as its salts; persulfuric acid such as permonosulfuric acid and peroxydisulfuric acid, ammonium persulfate, potassium persulfate and other persulfuric acids such as its salts; chloric acid, its salts, perchloric acid, potassium perchlorate and other chloric acids and perchloric acids such as its salts; osmic acids such as perosmic acid and osmic acid; selenic acids such as perselenic acid and selenic acid; ammonium cerium nitrate. As other oxidants, one of such compounds can be used or two or more of them can be used in combination. In some embodiments, from the perspective of performance stability of the polishing composition (for example, preventing deterioration caused by long-term storage), other oxidants are preferably inorganic compounds.

[0031] In the polishing composition disclosed herein, as other oxidants, a composite metal oxide may be included, which is a salt of a cation selected from an alkali metal ion and an anion selected from a transition metal oxyacid ion. The above-mentioned composite metal oxide is effective, for example, in reducing the hardness of high-hardness materials such as silicon carbide and making the material brittle. The above-mentioned composite metal oxide can be used alone or in combination of two or more. As specific examples of transition metal oxyacid ions in the above-mentioned composite transition metal oxide, permanganate ion, ferrate ion, chromate ion, dichromate ion, vanadate ion, ruthenate ion, molybdate ion, rhenate ion, tungstate ion, etc. can be cited. Among them, the oxyacids of the transition metal elements of the 4th period of the periodic table are more preferred. As preferred examples of the transition metal elements of the 4th period of the periodic table, Fe, Mn, Cr, V, and Ti can be cited. Among them, Fe, Mn, Cr are more preferred, and Mn is further preferred. The alkali metal ion in the above-mentioned composite transition metal oxide is preferably K. + In some embodiments, potassium permanganate may be preferably used as another oxidizing agent.

[0032] When the compound used as the oxidizing agent is a salt (eg, permanganate), the compound may be present in the polishing composition in the form of ions.

[0033] (Transition Metal Salt C)

[0034] The polishing composition disclosed herein comprises a transition metal salt C selected from salts comprising cations and anions of transition metals, i.e., metals belonging to Groups 3 to 12 of the periodic table. One transition metal salt C may be used alone or two or more may be used in combination. In a polishing composition comprising sodium permanganate as an oxidant, by using a transition metal salt C, it is possible to suppress the degradation of the performance of the polishing composition (e.g., a decrease in the polishing removal rate, etc.) caused by a pH change of the polishing composition during the polishing of the polishing object.

[0035] As the above transition metal, transition metals belonging to Groups 4 to 11 of the periodic table are preferred, and transition metals belonging to Periods 4 to 6 of the periodic table are suitable, transition metals belonging to Periods 4 to 5 are preferred, and transition metals belonging to Period 4 are more preferred.

[0036] In some embodiments, the transition metal salt C is preferably a salt of a cation and an anion of a metal containing a hydrated metal ion having a pKa of less than about 7. The transition metal salt C, which is a salt of such a cation and anion, forms a hydrated metal cation in water. The hydrated metal cation acts as a pH buffer due to the protons on the coordinated water being in an adsorption de-equilibrium state, thereby easily suppressing the performance degradation of the polishing composition caused by time. From this perspective, as the transition metal salt C, a salt of a cation and anion of a metal containing a pKa of a hydrated metal ion, for example, less than 7 or less than 6, can be preferably used. Examples of metal cations having a pKa of less than 6 for the hydrated metal ion include Cr 3+ (the pKa of hydrated metal ions is 4.2), Fe 3+ (the pKa of hydrated metal ions is 2.2), Hf 4+ (the pKa of hydrated metal ions is 0.2), Zr 4+ (the pKa of hydrated metal ions is -0.3), Ti 4+ (the pKa of the hydrated metal ion is -4.0), etc., but not limited thereto.

[0037] Examples of cations constituting the transition metal salt C include Cr 3+ , Fe 3+ , Hf 4+ 、Zr 4+ 、Ti 4+ Single-atom transition metal cations such as ZrO 2+ 、ZrO + , HfO + 、TiO + 、TiO 2+ Isooxo transition metal cations; ZrOH + , HfOH + etc. transition metal hydroxide cations; etc. cations, but not limited thereto.

[0038] The type of salt in the transition metal salt C is not particularly limited, and may be an inorganic salt or an organic salt. Examples of inorganic salts include hydrohalic acids such as hydrochloric acid, hydrobromic acid, and hydrofluoric acid, inorganic acid salts such as nitric acid, sulfuric acid, carbonic acid, silicic acid, boric acid, and phosphoric acid; sulfides; oxides; halogen oxides such as chlorine oxides, bromine oxides, and fluorine oxides; oxynitrates, oxysulfates, oxycarbonates, oxysilicates, oxyborates, and oxyphosphates; oxysulfides; and other compounds. Examples of organic salts include carboxylic acids such as formic acid, acetic acid, propionic acid, benzoic acid, glycine, butyric acid, citric acid, tartaric acid, and trifluoroacetic acid; organic sulfonic acids such as methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and toluenesulfonic acid; organic phosphonic acids such as methylphosphonic acid, phenylphosphonic acid, and toluenephosphonic acid; organic phosphoric acids such as ethylphosphonic acid; oxyorganic acid salts such as oxyacetates; and other organic acid salts. Among them, salts of hydrochloric acid, nitric acid, sulfuric acid, and phosphoric acid are preferred, and salts of hydrochloric acid and nitric acid are more preferred. The technology disclosed herein can be preferably implemented in a manner where an oxygen transition metal salt is used as the transition metal salt C, and the oxygen transition metal salt is a salt of an oxygen transition metal cation and an anion. As some preferred embodiments, ZrO 2+ 、ZrO + , HfO + 、TiO + 、TiO 2+ Any oxygen transition metal cation and nitrate ion (NO3 - ), sulfate ion (SO4 2- ) or chloride ion (Cl - ) is implemented in the form of salt.

[0039] Transition metal salt C generates a polynuclear transition metal complex comprising a transition metal and an oxygen atom and / or hydrogen by being dissolved in a solvent. For example, if transition metal salts C such as zirconium oxynitrate, zirconium sulfate, zirconium chloride are dissolved in water, a polynuclear transition metal complex comprising zirconium and an oxygen atom and / or hydrogen will be generated. In the technology disclosed herein, transition metal salt C may also be preferably implemented in a manner such as a polynuclear transition metal complex comprising a transition metal and an oxygen atom and / or hydrogen generated by being dissolved in a solvent. As a preferred polynuclear transition metal complex, a polynuclear transition metal complex comprising zirconium and an oxygen atom and / or hydrogen may be enumerated.

[0040] The transition metal salt C is preferably a compound that is not oxidized by the oxidant. From this perspective, by appropriately selecting the oxidant and the transition metal salt C, the deactivation of the oxidant due to the oxidation of the transition metal salt C by the oxidant can be prevented, and the performance degradation of the polishing composition caused by the passage of time (for example, a decrease in the polishing removal rate, etc.) can be suppressed. From this perspective, examples of preferred transition metal salts C include zirconium oxynitrate and the like.

[0041] In the case where the polishing composition includes a transition metal salt C, the concentration (content) of the transition metal salt C in the polishing composition is not particularly limited, and can be appropriately set according to the purpose of use and the method of use of the polishing composition to achieve the desired effect. The concentration of the transition metal salt C can be, for example, about 1000mM or less (i.e., 1 mol / L or less), can be 500mM or less, or can be 300mM or less. In some embodiments, it is appropriate that the concentration of the transition metal salt C is set to 200mM or less, preferably 100mM or less, more preferably 50mM or less, can be 30mM or less, can be 20mM or less, or can be 10mM or less. When the polishing composition contains a transition metal salt C, the lower limit of the concentration of the transition metal salt C may be, for example, 0.1 mM or more. From the perspective of properly exerting the effect of the use of the transition metal salt C, it is advantageous to set the lower limit of the concentration of the transition metal salt C to be 1 mM or more, preferably 5 mM or more, more preferably 10 mM or more (for example 15 mM or more), and may be 18 mM or more, 20 mM or more, or 30 mM or more.

[0042] In the case where the polishing composition contains a transition metal salt C, although not particularly limited, from the perspective of better exerting the effect of making the polishing composition containing an oxidant contain a transition metal salt C, the ratio (CC / Wx) of the concentration of the transition metal salt C in the polishing composition (when multiple transition metal salts C are included, their total concentration) CC [mM] to the content of the oxidant (when multiple oxidants are included, their total content) Wx [wt%] is usually greater than 0, preferably 0.01 or more, more preferably 0.025 or more, can be 0.05 or more, can be 0.1 or more, and can also be 0.5 or more. In some embodiments, CC / Wx can be, for example, 0.8 or more, can be 1.0 or more, can be 2.0 or more, can be 2.5 or more, and can also be 3.0 or more. The upper limit of CC / Wx is not particularly limited, and is appropriately about 500 or less, can be 300 or less, can be preferably 200 or less, more preferably 100 or less, and further preferably 50 or less. In some preferred embodiments, CC / Wx may be less than 25, less than 20, less than 10, less than 5, less than 4, less than 3, less than 2, or less than 1.

[0043] It should be noted that in the above "CC / Wx", "CC" is the numerical part when the concentration (content) of the transition metal salt C in the polishing composition is expressed in "mM", and "Wx" is the numerical part when the content of the oxidant in the polishing composition is expressed in "weight %", and both CC and Wx are dimensionless numbers.

[0044] (Metal Salt A)

[0045] In some preferred embodiments, the polishing composition may include a metal salt A, which is selected from salts containing cations and anions of poor metals, i.e., metals belonging to Groups 13 to 16 of the periodic table. The metal salt A may be used alone or in combination of two or more. In the polishing composition containing sodium permanganate as an oxidant, by further using the metal salt A, it is possible to suppress the degradation of the performance of the polishing composition caused by the pH change of the polishing composition during the polishing of the polishing object (for example, a decrease in the polishing removal rate, etc.).

[0046] As the above-mentioned poor metal, preferably it is a poor metal belonging to the 13th to 15th groups of the periodic table, more preferably it is a poor metal belonging to the 13th to 14th groups. In addition, it is preferably a poor metal belonging to the 3rd to 5th periods of the periodic table, more preferably it is a poor metal belonging to the 3rd to 4th periods, and particularly preferably it is a poor metal belonging to the 3rd period, i.e., aluminum.

[0047] In some embodiments, the metal salt A is preferably a salt of a cation and an anion of a metal containing a hydrated metal ion having a pKa of less than about 7. The metal salt A, which is a salt of such a cation and anion, forms a hydrated metal cation in water. Since the protons on the coordinated water are in adsorption-desorption equilibrium, the hydrated metal cation acts as a pH buffer, and it is easy to suppress the performance degradation of the polishing composition caused by the passage of time. From this perspective, as the metal salt A, a salt of a cation and anion of a metal containing a pKa of less than 7 or 6 or less can be preferably used. As the cation of the metal containing the hydrated metal ion having a pKa of 6 or less, for example, Al 3+ (pKa of hydrated metal ions is 5.0), Ga 3+ (the pKa of hydrated metal ions is 2.6), In 3+ (The pKa of hydrated metal ions is 4.0), but is not limited thereto.

[0048] The type of salt in the metal salt A is not particularly limited, and it can be an inorganic acid salt or an organic acid salt. Examples of inorganic acid salts include salts of hydrohalic acids such as hydrochloric acid, hydrobromic acid, and hydrofluoric acid, nitric acid, sulfuric acid, carbonic acid, silicic acid, boric acid, and phosphoric acid. Examples of organic acid salts include salts of carboxylic acids such as formic acid, acetic acid, propionic acid, benzoic acid, glycine, butyric acid, citric acid, tartaric acid, and trifluoroacetic acid; organic sulfonic acids such as methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and toluenesulfonic acid; organic phosphonic acids such as methylphosphonic acid, phenylphosphonic acid, and toluenephosphonic acid; organic phosphoric acids such as ethylphosphonic acid; and the like. Among them, salts of hydrochloric acid, nitric acid, sulfuric acid, and phosphoric acid are preferred, and salts of hydrochloric acid and nitric acid are more preferred. The technology disclosed herein can, for example, preferably be used with Al 3+ , Ga 3+ 、In 3+Any cation and nitrate ion (NO3 - ) or chloride ion (Cl - ) is implemented as a metal salt A.

[0049] The metal salt A is preferably a compound that is not oxidized by an oxidant. From this perspective, by appropriately selecting an oxidant and a metal salt A, the inactivation of the oxidant caused by the oxidation of the metal salt A by the oxidant can be prevented, and the performance degradation of the grinding composition caused by the passage of time (for example, the decline of the grinding removal rate, etc.) can be suppressed. From this perspective, as preferred metal salts A, aluminum nitrate, aluminum chloride, etc. can be cited. The metal salt A can be used in combination with the aforementioned transition metal salt C and the metal salt B described later to increase the grinding removal rate. As some preferred modes, it can be preferably implemented in a manner using zirconium nitrate as the transition metal salt C and aluminum nitrate as the metal salt A.

[0050] In the case where the grinding composition includes a metal salt A, the concentration (content) of the metal salt A in the grinding composition is not particularly limited, and can be appropriately set according to the purpose of use and the method of use of the grinding composition to achieve the desired effect. The concentration of the metal salt A can be, for example, about 1000mM or less (i.e., 1 mol / L or less), can be 500mM or less, or can be 300mM or less. In some ways, it is appropriate that the concentration of the metal salt A is set to 200mM or less, preferably 100mM or less, more preferably 50mM or less, can be 30mM or less, can be 20mM or less, or can be 10mM or less. When the polishing composition contains metal salt A, the lower limit of the concentration of metal salt A can be, for example, 0.1 mM or more. From the perspective of properly exerting the effect of the use of metal salt A, it is advantageous to set the lower limit of the concentration of metal salt A to be 1 mM or more, preferably 5 mM or more, more preferably 10 mM or more (for example 15 mM or more), and can be 18 mM or more, 20 mM or more, or 30 mM or more.

[0051] In the case where the polishing composition contains a metal salt A, although not particularly limited, from the perspective of better exerting the effect of making the polishing composition containing an oxidant contain a metal salt A, the ratio (CA / Wx) of the concentration of the metal salt A in the polishing composition (when multiple metal salts A are included, their total concentration) CA [mM] to the content of the oxidant (when multiple oxidants are included, their total content) Wx [wt%] is usually greater than 0, preferably 0.01 or more, more preferably 0.025 or more, can be 0.05 or more, can be 0.1 or more, and can also be 0.5 or more. In some embodiments, CA / Wx can be, for example, 0.8 or more, can be 1.0 or more, can be 2.0 or more, can be 2.5 or more, and can also be 3.0 or more. The upper limit of CA / Wx is not particularly limited, and is appropriately about 500 or less, can be 300 or less, can be preferably 200 or less, more preferably 100 or less, and further preferably 50 or less. In some preferred embodiments, CA / Wx may be less than 25, less than 20, less than 10, less than 5, less than 4, less than 3, less than 2, or less than 1.

[0052] It should be noted that in the above-mentioned "CA / Wx", "CA" is the numerical part when the concentration (content) of the metal salt A in the polishing composition is expressed in "mM", and "Wx" is the numerical part when the content of the oxidant in the polishing composition is expressed in "weight %". Both CA and Wx are dimensionless numbers.

[0053] (Metal Salt B)

[0054] In some preferred embodiments, the polishing composition may include a metal salt B selected from alkaline earth metal salts. As the metal salt B, one alkaline earth metal salt may be used alone, or two or more alkaline earth metal salts may be used in combination. When the metal salt B is used, the polishing removal rate is easily increased. As an element belonging to alkaline earth metals, the metal salt B preferably includes any one or more than two of Mg, Ca, Sr, and Ba. Among them, any one of Ca and Sr is preferred, and Ca is more preferred.

[0055] The type of salt in the metal salt B is not particularly limited, and it can be an inorganic acid salt or an organic acid salt. Examples of inorganic acid salts include salts of hydrohalic acids such as hydrochloric acid, hydrobromic acid, and hydrofluoric acid, nitric acid, sulfuric acid, carbonic acid, silicic acid, boric acid, and phosphoric acid. Examples of organic acid salts include carboxylic acids such as formic acid, acetic acid, propionic acid, benzoic acid, glycine, butyric acid, citric acid, tartaric acid, and trifluoroacetic acid; organic sulfonic acids such as methanesulfonic acid, trifluoromethanesulfonic acid, benzenesulfonic acid, and toluenesulfonic acid; organic phosphonic acids such as methylphosphonic acid, benzenephosphonic acid, and toluenephosphonic acid; organic phosphoric acids such as ethyl phosphoric acid; and the like. Among them, salts of hydrochloric acid, nitric acid, sulfuric acid, and phosphoric acid are preferred, and salts of hydrochloric acid and nitric acid are more preferred. The technology disclosed herein can be preferably implemented, for example, by using nitrates or chlorides of alkaline earth metals as metal salt B.

[0056] Specific examples of alkaline earth metal salts that can be options for the metal salt B include chlorides such as magnesium chloride, calcium chloride, strontium chloride, and barium chloride; bromides such as magnesium bromide; fluorides such as magnesium fluoride, calcium fluoride, strontium fluoride, and barium fluoride; nitrates such as magnesium nitrate, calcium nitrate, strontium nitrate, and barium nitrate; sulfates such as magnesium sulfate, calcium sulfate, strontium sulfate, and barium sulfate; carbonates such as magnesium carbonate, calcium carbonate, strontium carbonate, and barium carbonate; carboxylates such as calcium acetate, strontium acetate, calcium benzoate, and calcium citrate, etc.

[0057] The metal salt B is preferably a water-soluble salt. By using the water-soluble metal salt B, a good surface with few defects such as scratches can be formed efficiently.

[0058] In addition, the metal salt B is preferably a compound that is not oxidized by the oxidant. From this perspective, by appropriately selecting the oxidant and the metal salt B, the deactivation of the oxidant due to oxidation of the metal salt B by the oxidant can be prevented, and the performance degradation of the polishing composition caused by the passage of time (for example, a decrease in the polishing removal rate, etc.) can be suppressed. From this perspective, calcium nitrate can be cited as a preferred metal salt B.

[0059] In the case where the grinding composition includes a metal salt B, the concentration (content) of the metal salt B in the grinding composition is not particularly limited, and can be appropriately set according to the purpose of use and the method of use of the grinding composition to achieve the desired effect. The concentration of metal salt B can be, for example, about 1000mM or less (i.e., 1 mol / L or less), can be 500mM or less, or can be 300mM or less. In some ways, it is appropriate for the concentration of metal salt B to be set to 200mM or less, preferably 100mM or less, more preferably 50mM or less, can be 30mM or less, can be 20mM or less, or can be 10mM or less. The lower limit of the concentration of metal salt B can be, for example, more than 0.1mM, and from the perspective of the effect of the use of metal salt B, the lower limit of the concentration of metal salt B is preferably set to more than 0.5mM, more preferably 1mM or more, can be more than 2.5mM, can be more than 5mM, can be more than 10mM, can be more than 20mM, or can be more than 30mM.

[0060] In the case where the polishing composition includes a metal salt B, although not particularly limited, from the perspective of better exerting the effect of making the polishing composition containing an oxidant contain a metal salt B, the ratio (CB / Wx) of the concentration of the metal salt B in the polishing composition (when multiple metal salts B are included, their total concentration) CB [mM] and the content of the oxidant (when multiple oxidants are included, their total content) Wx [wt %] is usually greater than 0, preferably 0.01 or more, more preferably 0.025 or more, can be 0.05 or more, can be 0.1 or more, and can also be 0.5 or more. In some embodiments, CB / Wx can be, for example, 0.8 or more, can be 1.0 or more, can be 2.0 or more, can be 2.5 or more, and can also be 3.0 or more. The upper limit of CB / Wx is not particularly limited, for example, it can be set to 300 or less, about 100 or less is appropriate, can be preferably 75 or less, more preferably 50 or less, and further preferably 25 or less. In some preferred embodiments, CB / Wx may be less than 20, less than 10, less than 5, less than 4, less than 3, less than 2, or less than 1.

[0061] It should be noted that in the above "CB / Wx", "CB" is the numerical part when the concentration (content) of the metal salt B in the polishing composition is expressed in "mM", and "Wx" is the numerical part when the content of the oxidant in the polishing composition is expressed in "weight %". Both CB and Wx are dimensionless numbers.

[0062] In some preferred embodiments, the polishing composition may include a combination of a metal salt A and a metal salt B. In some preferred embodiments of the case where the combination of a metal salt A and a metal salt B is included, the anion species of the metal salt A and the metal salt B are the same. The anion species common to the metal salt A and the metal salt B may be, for example, nitric acid, hydrochloric acid, phosphoric acid, etc. From the perspective of obtaining a higher effect, a polishing composition in which both the metal salt A and the metal salt B are nitrates is particularly preferred.

[0063] In the case where the polishing composition comprises a combination of a metal salt A and a metal salt B, the relationship between the concentration CA [mM] of the metal salt A in the polishing composition and the concentration CB [mM] of the metal salt B is not particularly limited, and can be set to appropriately exert the effect of using them in combination. For example, CA / CB can range from 0.001 to 1000. From the perspective of increasing the polishing removal rate, in some embodiments, it is appropriate for CA / CB to be about 0.01 or more, preferably 0.05 or more (e.g., 0.1 or more). In addition, it is appropriate for CA / CB to be about 100 or less, preferably 50 or less, 30 or less, and more preferably 25 or less (e.g., 10 or less).

[0064] (Abrasive particles)

[0065] In some aspects of the technology disclosed herein, the polishing composition contains abrasive grains. According to the polishing composition containing abrasive grains, in addition to the main chemical polishing action by the oxidant, etc., the main mechanical polishing action of the abrasive grains can be exerted, thereby achieving a higher polishing removal rate.

[0066] The material and properties of the abrasive grains are not particularly limited. For example, the abrasive grains may be any of inorganic particles, organic particles, and organic-inorganic composite particles. For example, the abrasive grains may be substantially composed of oxide particles such as silica particles, alumina particles, cerium oxide particles, chromium oxide particles, titanium dioxide particles, zirconium oxide particles, magnesium oxide particles, manganese dioxide particles, zinc oxide particles, and iron oxide particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; carbonates such as calcium carbonate and barium carbonate; etc. Abrasive grains may be used alone or in combination of two or more. Among them, oxide particles such as silica particles, alumina particles, cerium oxide particles, chromium oxide particles, zirconium oxide particles, manganese dioxide particles, and iron oxide particles can form a good surface, so they are preferred. Among them, silica particles, alumina particles, zirconium oxide particles, chromium oxide particles, and iron oxide particles are more preferred, and silica particles and alumina particles are further preferred, and alumina particles are particularly preferred. In the embodiment using aluminum oxide particles as abrasive particles, the effect of increasing the polishing removal rate by applying the technology disclosed herein can be preferably exerted.

[0067] It should be noted that, in the present specification, regarding the composition of the abrasive grains, "substantially formed of X" or "substantially composed of X" means that the proportion of X in the abrasive grains (the purity of X) is 90% or more on a weight basis. In addition, the proportion of X in the abrasive grains is preferably 95% or more, more preferably 97% or more, further preferably 98% or more, for example, 99% or more.

[0068] The average primary particle size of the abrasive is not particularly limited. From the perspective of increasing the grinding removal rate, the average primary particle size of the abrasive can be, for example, 5 nm or more, 10 nm or more is appropriate, preferably 20 nm or more, and 30 nm or more. From the perspective of further increasing the grinding removal rate, in some embodiments, the average primary particle size of the abrasive can be 50 nm or more, 80 nm or more, 150 nm or more, 250 nm or more, or 350 nm or more. In addition, from the perspective of the surface quality after grinding, the average primary particle size of the abrasive can be, for example, 5 μm or less, preferably 3 μm or less, more preferably 1 μm or less, 750 nm or less, or 500 nm or less. From the perspective of further improving the surface quality after grinding, in some embodiments, the average primary particle size of the abrasive can be 350 nm or less, 180 nm or less, 85 nm or less, or 50 nm or less.

[0069] It should be noted that the average primary particle size in this specification refers to the specific surface area (BET value) measured by the BET method, which is obtained by average primary particle size (nm) = 6000 / (true density (g / cm 3 )×BET value (m 2 The above-mentioned specific surface area can be measured using, for example, a surface area measuring device manufactured by Micromeritics under the trade name "Flow Sorb II 2300".

[0070] The average secondary particle size of the abrasive particles can be, for example, more than 10 nm. From the perspective of easily increasing the grinding removal rate, it is preferably more than 50 nm, more preferably more than 100 nm, more than 250 nm, or more than 400 nm. From the perspective of fully ensuring the number per unit weight, it is appropriate to set the upper limit of the average secondary particle size of the abrasive particles to about 10 μm or less. In addition, from the perspective of the surface quality after grinding, the above-mentioned average secondary particle size is preferably less than 5 μm, more preferably less than 3 μm, for example, less than 1 μm. From the perspective of further improving the surface quality after grinding, in some embodiments, the average secondary particle size of the abrasive particles can be less than 600 nm, less than 300 nm, less than 170 nm, or less than 100 nm.

[0071] For particles having an average secondary particle size of less than 500 nm, for example, the volume average particle size (arithmetic mean diameter based on volume; Mv) can be measured by a dynamic light scattering method using a model "UPA-UT151" manufactured by Nikkiso Co., Ltd. In addition, for particles having a size of 500 nm or more, the volume average particle size can be measured by a pore resistance method using a model "Multisizer 3" manufactured by BECKMAN COULTER Co., Ltd.

[0072] When alumina particles (alumina abrasives) are used as abrasives, they can be appropriately selected from various known alumina particles. Examples of such known alumina particles include α-alumina and intermediate alumina. Here, intermediate alumina is a general term for alumina particles other than α-alumina, and specifically, γ-alumina, δ-alumina, θ-alumina, η-alumina, κ-alumina, χ-alumina, etc. can be cited. In addition, based on the classification according to the manufacturing method, alumina called fumed alumina (typically alumina particles produced when alumina salt is calcined at a high temperature) can be used. Furthermore, alumina called colloidal alumina or alumina sol (for example, alumina hydrates such as boehmite) is also included in the examples of the above-mentioned known alumina particles. From the perspective of processability, it is preferred to contain α-alumina. The alumina abrasive in the technology disclosed herein may contain one of such alumina particles alone or two or more of such alumina particles in combination.

[0073] When aluminum oxide particles are used as abrasive particles, it is generally advantageous if the proportion of aluminum oxide particles in the total abrasive particles used is relatively high. For example, the proportion of aluminum oxide particles in the total abrasive particles is preferably 70% by weight or more, more preferably 90% by weight or more, further preferably 95% by weight or more, and can be substantially 100% by weight.

[0074] The particle size of the aluminum oxide abrasive is not particularly limited and can be selected to exert the desired grinding effect. From the perspective of improving the grinding removal rate, the average primary particle size of the aluminum oxide abrasive is preferably 50 nm or more, more preferably 80 nm or more, 150 nm or more, 250 nm or more, or 300 nm or more. The upper limit of the average primary particle size of the aluminum oxide abrasive is not particularly limited. From the perspective of the surface quality after grinding, it is appropriate to set it to about 5 μm or less. From the perspective of further improving the surface quality after grinding, it is preferably 3 μm or less, more preferably 1 μm or less, 750 nm or less, 500 nm or less, 400 nm or less, or 350 nm or less.

[0075] When aluminum oxide particles are used as abrasive particles, the polishing composition disclosed herein may further contain abrasive particles formed of a material other than the above-mentioned aluminum oxide (hereinafter also referred to as non-aluminum oxide abrasive particles) within the range that does not impair the effect of the present invention. Examples of such non-aluminum oxide abrasive particles include abrasive particles substantially composed of any of oxide particles such as silicon dioxide particles, cerium oxide particles, chromium oxide particles, titanium dioxide particles, zirconium oxide particles, magnesium oxide particles, manganese oxide particles, zinc oxide particles, and iron oxide particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; and carbonates such as calcium carbonate and barium carbonate.

[0076] The content of the non-aluminum oxide abrasive grains in the total weight of the abrasive grains contained in the polishing composition is, for example, appropriately 30 wt % or less, preferably 20 wt % or less, and more preferably 10 wt % or less.

[0077] In another preferred embodiment of the technology disclosed herein, the grinding composition comprises silica particles (silica abrasive grains) as abrasive grains. The silica abrasive grains can be appropriately selected from various known silica particles for use. As such known silica particles, colloidal silica, dry silica, etc. can be cited. Among them, colloidal silica is preferably used. According to the silica abrasive grains comprising colloidal silica, good surface accuracy can be suitably achieved.

[0078] The shape (outer shape) of the silica abrasive grains may be spherical or non-spherical. For example, as specific examples of non-spherical silica abrasive grains, there may be mentioned peanut-shaped (i.e., the shape of peanut shells), cocoon-shaped, candy-shaped, rugby-shaped, etc. In the technology disclosed herein, the silica abrasive grains may be in the form of primary particles or in the form of secondary particles formed by the association of multiple primary particles. In addition, silica abrasive grains in the form of primary particles and silica abrasive grains in the form of secondary particles may also be mixed. In a preferred embodiment, at least a portion of the silica abrasive grains are contained in the grinding composition in the form of secondary particles.

[0079] As silica abrasive grains, silica abrasive grains having an average primary particle size greater than 5 nm can be preferably used. From the perspective of grinding efficiency, the average primary particle size of the silica abrasive grains is preferably 15 nm or more, more preferably 20 nm or more, further preferably 25 nm or more, and particularly preferably 30 nm or more. The upper limit of the average primary particle size of the silica abrasive grains is not particularly limited, and it is appropriate to set it to about 120 nm or less, preferably 100 nm or less, and more preferably 85 nm or less. For example, from the perspective of taking into account grinding efficiency and surface quality at a higher level, silica abrasive grains having a BET diameter of 12 nm or more and 80 nm or less are preferred, and silica abrasive grains having a BET diameter of 15 nm or more and 75 nm or less are preferred.

[0080] The average secondary particle size of the silica abrasive is not particularly limited, but is preferably 20 nm or more, more preferably 50 nm or more, and further preferably 70 nm or more from the perspective of grinding efficiency. In addition, from the perspective of obtaining a higher quality surface, the average secondary particle size of the silica abrasive is appropriately 500 nm or less, preferably 300 nm or less, more preferably 200 nm or less, further preferably 130 nm or less, and particularly preferably 110 nm or less (e.g., 100 nm or less).

[0081] The true specific gravity (true density) of silica particles is preferably more than 1.5, more preferably more than 1.6, and further preferably more than 1.7. By increasing the true specific gravity of silica particles, physical grinding ability tends to increase. The upper limit of the true specific gravity of silica particles is not particularly limited, typically less than 2.3, for example, less than 2.2, less than 2.0, less than 1.9. As the true specific gravity of silica particles, a measured value obtained by a liquid displacement method using ethanol as a displacement fluid can be used.

[0082] The shape (outer shape) of the silica particles is preferably spherical. Although not particularly limited, the average value (average aspect ratio) of the major diameter / minor diameter ratio of the particles is theoretically more than 1.00, and from the perspective of improving the grinding removal rate, for example, it can be more than 1.05, or more than 1.10. In addition, it is appropriate that the average aspect ratio of the particles is less than 3.0, or less than 2.0. From the perspective of improving the smoothness of the ground surface and reducing scratches, the average aspect ratio of the particles is preferably less than 1.50, can be less than 1.30, or less than 1.20.

[0083] The shape (outer shape) and average aspect ratio of the particles can be grasped, for example, by electron microscope observation. As a specific step to grasp the average aspect ratio, for example, a scanning electron microscope (SEM) is used to extract the shapes of a specified number of particles (for example, 200 particles). Draw the smallest rectangle that circumscribes the shape of each extracted particle. Then, for the rectangle drawn for the shape of each particle, the value obtained by calculating the length of its long side (the value of the long diameter) divided by the length of the short side (the value of the short diameter) is used as the long diameter / short diameter ratio (aspect ratio). The average aspect ratio can be calculated by arithmetically averaging the aspect ratios of the above-mentioned specified number of particles.

[0084] In the embodiment in which the polishing composition includes silica abrasive grains, the polishing composition may further include abrasive grains formed of a material other than silica (hereinafter also referred to as non-silica abrasive grains). Examples of particles constituting such non-silica abrasive grains include particles substantially composed of oxide particles such as aluminum oxide particles, cerium oxide particles, chromium oxide particles, titanium dioxide particles, zirconium oxide particles, magnesium oxide particles, manganese oxide particles, zinc oxide particles, and iron oxide particles; nitride particles such as silicon nitride particles and boron nitride particles; carbide particles such as silicon carbide particles and boron carbide particles; diamond particles; carbonates such as calcium carbonate and barium carbonate; and the like.

[0085] The content of the non-silica abrasive grains in the total weight of the abrasive grains contained in the polishing composition is, for example, appropriately 30 wt % or less, preferably 20 wt % or less, and more preferably 10 wt % or less.

[0086] From the perspective of surface quality after grinding, it is appropriate that the content of abrasive grains (such as aluminum oxide abrasive grains, etc.) in the grinding composition disclosed herein is less than 10% by weight, and it is advantageous to be less than 6% by weight, preferably less than 3% by weight, more preferably less than 2% by weight, and can be less than 1.5% by weight, can be less than 1.3% by weight, can be less than 1.2% by weight, can be less than 1.1% by weight, and can also be less than 1.0% by weight. In some embodiments, the content of abrasive grains in the grinding composition can be less than 0.5% by weight or less than 0.5% by weight, can be less than 0.1% by weight or less than 0.1% by weight, can be less than 0.05% by weight or less than 0.05% by weight, can be less than 0.04% by weight or less than 0.04% by weight. The lower limit of the content of abrasive grains is not particularly limited, for example, it can be more than 0.000001% by weight (i.e., more than 0.01ppm). From the perspective of improving the use effect of the abrasive, in some embodiments, the content of the abrasive in the polishing composition can be 0.00001% by weight or more, 0.0001% by weight or more, 0.001% by weight or more, 0.002% by weight or more, or 0.005% by weight or more. In some embodiments, the content of the abrasive in the polishing composition can be 0.01% by weight or more, 0.02% by weight or more, 0.03% by weight or more, more than 0.1% by weight, more than 0.3% by weight, more than 0.5% by weight, or more than 0.8% by weight. When the polishing composition disclosed herein contains multiple abrasives, the content of the abrasive in the polishing composition refers to the total content of the multiple abrasives.

[0087] The grinding composition disclosed herein preferably does not substantially comprise diamond particles as particles. The hardness of diamond particles is high, so it is likely to become the limiting factor for improving smoothness. In addition, generally speaking, diamond particles are more expensive, so they are not favorable materials from the aspect of cost effect, and from the practical aspect, the degree of dependence on high-priced materials such as diamond particles can be reduced. Here, particle does not substantially comprise diamond particles, and refers to that the ratio of diamond particles in the entire particle is below 1 weight %, more preferably below 0.5 weight %, typically below 0.1 weight %, and the ratio comprising diamond particles is the situation of 0 weight %. In such a mode, the application effect of the present invention can be brought into play suitably.

[0088] In the polishing composition containing abrasive grains, the relationship between the content of the oxidant and the content of the abrasive grains is not particularly limited, and can be appropriately set according to the purpose of use and the method of use to achieve the desired effect. The ratio of the content Wx [weight %] of the oxidant to the content Wp [weight %] of the abrasive grains, that is, Wx / Wp, can be set to about 0.01 or more, and it is appropriate to set it to 0.025 or more, and it can be 0.05 or more, 0.1 or more, 0.2 or more, 1 or more, and 1.4 or more is advantageous, preferably 2.5 or more, and more preferably 3.5 or more. When Wx / Wp becomes larger, the contribution of chemical polishing tends to become larger relative to the contribution of mechanical polishing. In some embodiments, Wx / Wp can be 5 or more, 6 or more, 6.5 or more, 7 or more, 8 or more, or 9 or more. In some preferred embodiments, Wx / Wp may be, for example, about 10 or more, 30 or more, 50 or more, 70 or more, 90 or more, 120 or more, 150 or more, or 180 or more. The upper limit of Wx / Wp is not particularly limited. From the perspective of storage stability of the polishing composition, for example, it may be about 5000 or less, 1500 or less, 1000 or less, 800 or less, 400 or less, 250 or less, 100 or less, 80 or less, or 40 or less. In some embodiments, Wx / Wp may be 30 or less, 20 or less, or 10 or less.

[0089] It should be noted that in the above-mentioned "Wx / Wp", "Wx" is the numerical part when the content of the oxidant in the polishing composition is expressed in "weight %", and "Wp" is the numerical part when the content of the abrasive in the polishing composition is expressed in "weight %", and both Wx and Wp are dimensionless numbers.

[0090] In the polishing composition comprising abrasive grains and the above-mentioned transition metal salt C, the relationship between the concentration of the transition metal salt C and the content of the abrasive grains is not particularly limited, and can be appropriately set according to the purpose of use and the mode of use to achieve the desired effect. The ratio of the concentration CC of the transition metal salt C (when multiple transition metal salts C are included, it is their total concentration) [mM] to the content Wp of the abrasive grains (when multiple abrasive grains are included, it is their total content) [wt%], that is, CC / Wp, can be set to 0.05 or more, and it is appropriate to set it to 0.1 or more, and it can be 0.2 or more, preferably 1 or more, more preferably 3 or more, 5 or more, or 10 or more. When CC / Wp becomes larger, the contribution of chemical polishing tends to become larger relative to the contribution of mechanical polishing. In some embodiments, CC / Wp can be 12 or more, 15 or more, or 18 or more. In other embodiments, CC / Wp can be 50 or more, 100 or more, 150 or more, 200 or more, or 250 or more. The upper limit of CC / Wp is not particularly limited. From the perspective of storage stability of the polishing composition, for example, it can be set to about 20,000 or less, 10,000 or less, 5,000 or less, 2,500 or less, or 1,000 or less. In some embodiments, CC / Wp can be 100 or less, 50 or less, 40 or less, or 30 or less.

[0091] It should be noted that in the above "CC / Wp", "CC" is the numerical part when the concentration of the transition metal salt C in the polishing composition is expressed in "mM", and "Wp" is the numerical part when the content of the abrasive in the polishing composition is expressed in "weight %", and both Wp and CC are dimensionless numbers.

[0092] In the polishing composition comprising abrasive grains and metal salt A, the relationship between the concentration of metal salt A and the content of abrasive grains is not particularly limited and can be appropriately set according to the purpose of use and the mode of use to achieve the desired effect. The ratio of the concentration CA of metal salt A (when comprising multiple metal salts A, it is their total concentration) [mM] to the content Wp of abrasive grains (when comprising multiple abrasive grains, it is their total content) [wt %], i.e. CA / Wp, can be set to 0.05 or more, and it is appropriate to set it to 0.1 or more, and it can be 0.2 or more, preferably 1 or more, more preferably 3 or more, 5 or more, or 10 or more. When CA / Wp becomes larger, the contribution of chemical polishing tends to become larger relative to the contribution of mechanical polishing. In some embodiments, CA / Wp can be 12 or more, 15 or more, or 18 or more. The upper limit of CA / Wp is not particularly limited. From the perspective of storage stability of the polishing composition, for example, it can be set to about 20,000 or less, 10,000 or less, 5,000 or less, 2,500 or less, or 1,000 or less. In some embodiments, CA / Wp can be 100 or less, 50 or less, 40 or less, or 30 or less.

[0093] It should be noted that in the above-mentioned "CA / Wp", "CA" is the numerical part when the concentration of the metal salt A in the polishing composition is expressed in "mM", and "Wp" is the numerical part when the content of the abrasive in the polishing composition is expressed in "weight %", and both Wp and CA are dimensionless numbers.

[0094] In the polishing composition comprising abrasive grains and metal salt B, the relationship between the concentration of metal salt B and the content of abrasive grains is not particularly limited, and can be appropriately set according to the purpose of use and the method of use to achieve the desired effect. The ratio of the concentration CB of metal salt B (when multiple metal salts B are included, their total concentration) [mM] to the content Wp of abrasive grains (when multiple abrasive grains are included, their total content) [wt%], i.e., CB / Wp, can be set to 0.05 or more, and it is appropriate to set it to 0.1 or more, and it can be 0.2 or more, preferably 1 or more, more preferably 3 or more, 5 or more, or 10 or more. When CB / Wp becomes larger, the contribution of chemical polishing tends to become larger relative to the contribution of mechanical polishing. In some embodiments, CB / Wp can be 20 or more, 50 or more, 100 or more, or 300 or more. The upper limit of CB / Wp is not particularly limited. From the perspective of the storage stability of the polishing composition, for example, it can be set to about 10,000 or less, 5000 or less, or 2500 or less. In some embodiments, CB / Wp may be 1000 or less, 800 or less, or 600 or less.

[0095] It should be noted that in the above "CB / Wp", "CB" is the numerical part when the concentration of the metal salt B in the polishing composition is expressed in "mM", and "Wp" is the numerical part when the content of the abrasive in the polishing composition is expressed in "weight %", and both CB and Wp are dimensionless numbers.

[0096] The polishing composition disclosed herein may also be preferably implemented in an embodiment not containing abrasive grains. In this embodiment, the effect of increasing the polishing removal rate by using sodium permanganate as an oxidizing agent can also be well exerted.

[0097] (water)

[0098] The polishing composition disclosed herein includes water. As water, ion exchange water (deionized water), pure water, ultrapure water, distilled water, etc. can be preferably used. The polishing composition disclosed herein can also include an organic solvent (lower alcohol, lower ketone, etc.) that can be uniformly mixed with water as required. Usually, it is appropriate that 90% by volume or more of the solvent contained in the polishing composition is water, preferably 95% by volume or more is water, and more preferably 99 to 100% by volume is water.

[0099] (acid)

[0100] For the purpose of pH adjustment, improving the grinding removal speed, etc., the grinding composition may contain an acid as required. As an acid, any kind of an inorganic acid and an organic acid can be used. Examples of inorganic acids include sulfuric acid, nitric acid, hydrochloric acid, carbonic acid, etc. Examples of organic acids include aliphatic carboxylic acids such as formic acid, acetic acid, propionic acid, aromatic carboxylic acids such as benzoic acid and phthalic acid, citric acid, oxalic acid, tartaric acid, malic acid, maleic acid, fumaric acid, succinic acid, organic sulfonic acid, organic phosphonic acid, etc. These can be used alone or in combination of two or more. When using an acid, its usage is not particularly limited and can be set to an usage that meets the purpose of use (e.g., pH adjustment). Alternatively, in some embodiments of the grinding composition disclosed herein, it can also be a composition that does not substantially contain an acid.

[0101] (Basic Compounds)

[0102] For the purpose of pH adjustment, improving the polishing removal rate, etc., the polishing composition may contain an alkaline compound as needed. Here, the alkaline compound refers to a compound having the function of increasing the pH of the composition by adding it to the polishing composition. As examples of alkaline compounds, alkali metal hydroxides such as potassium hydroxide and sodium hydroxide can be cited; carbonates and bicarbonates such as ammonium bicarbonate, ammonium carbonate, potassium bicarbonate, potassium carbonate, sodium bicarbonate, and sodium carbonate; ammonia; quaternary ammonium compounds, such as quaternary ammonium hydroxides such as tetramethylammonium hydroxide, tetraethylammonium hydroxide, and tetrabutylammonium hydroxide; and amines, phosphates, hydrogen phosphates, organic acid salts, etc. The alkaline compound can be used alone or in combination of two or more. When using an alkaline compound, its usage is not particularly limited and can be set to an amount that meets the purpose of use (such as adjusting pH). Alternatively, in some embodiments of the polishing composition disclosed herein, it can also be a composition that does not substantially contain an alkaline compound.

[0103] (Other ingredients)

[0104] The polishing composition disclosed herein may further include known additives such as chelating agents, thickeners, dispersants, surface protective agents, wetting agents, surfactants, rust inhibitors, preservatives, and mildew inhibitors that can be used for polishing compositions (e.g., polishing compositions used in the grinding of high-hardness materials such as silicon carbide) as needed, within the scope of not impairing the effects of the present invention. The content of the above-mentioned additives can be appropriately set according to the purpose of their addition, and the feature of the present invention is not this, so a detailed description is omitted.

[0105] (pH)

[0106] It is appropriate that the pH of the polishing composition is set to about 1 to 12. When the pH is within the above range, a practical polishing removal rate is easily achieved. In some embodiments, the pH may be below 12.0, below 11.0, below 10.0, below 9.0, below 9.0, below 8.0, below 8.0, below 7.0, below 7.0, or below 6.0. From the perspective of making it easier to exert the effect of increasing the polishing removal rate by using the metal salt A, in some embodiments, the pH of the polishing composition is preferably less than 6.0, below 5.0, below 5.0, below 4.0, or below 4.0. The pH may be, for example, above 1.0, above 1.5, above 2.0, or above 2.5.

[0107] The preparation method of the polishing composition disclosed herein is not particularly limited. For example, the various components contained in the polishing composition can be mixed using a known mixing device such as a blade stirrer, an ultrasonic disperser, a homogenizer, etc. The manner of mixing these components is not particularly limited, for example, all the components can be mixed at once, or they can be mixed in an appropriately set order.

[0108] The polishing composition disclosed herein may be a single-component type or a multi-component type headed by a two-component type. For example, it may be constituted as follows: Part A containing a portion of the components of the polishing composition (e.g., components other than water) and Part B containing the remaining components are mixed and used for polishing the polishing object. The above-mentioned multi-component polishing composition may also contain Part C in addition to the above-mentioned Part A and Part B. For example, they may be stored separately before use and mixed during use to prepare a single-liquid polishing composition. During mixing, water for dilution may be further mixed. In a preferred embodiment, the multi-component polishing composition disclosed herein contains an oxidant and water in Part A, and a transition metal salt C and water in Part B. In this way, the storage stability of the polishing composition can be improved. The arbitrarily used Part C may contain abrasive particles or may not contain abrasive particles.

[0109] <Object to be polished>

[0110] The polishing object of the polishing composition disclosed herein is not particularly limited. For example, the polishing composition disclosed herein can be applied to the polishing of a substrate having a surface composed of a compound semiconductor material, that is, a compound semiconductor substrate. The constituent material of the compound semiconductor substrate is not particularly limited, for example, it can be a II-VI group compound semiconductor such as cadmium telluride, zinc selenide, cadmium sulfide, cadmium mercury telluride, cadmium zinc telluride; a III-V group compound semiconductor such as gallium nitride, gallium arsenide, gallium phosphide, indium phosphide, aluminum gallium arsenide, gallium indium arsenide, gallium indium arsenide, and aluminum gallium indium phosphide; a IV-IV group compound semiconductor such as silicon carbide and silicon germanium; etc. It can also be a polishing object composed of a variety of these materials. In a preferred embodiment, the polishing composition disclosed herein can be applied to the polishing of a substrate having a surface composed of a compound semiconductor material that is not an oxide (that is, a non-oxide). In the polishing of a substrate having a surface composed of a non-oxide compound semiconductor material, it is easy and appropriate to exert the polishing promotion effect of the oxidant contained in the polishing composition disclosed herein.

[0111] The grinding composition disclosed herein can be preferably used for example for grinding the surface of the grinding object with a Vickers hardness of more than 500Hv. The above-mentioned Vickers hardness is preferably more than 700Hv, for example, it can be more than 1000Hv or more than 1500Hv. The Vickers hardness of the grinding object material can be more than 1800Hv, can be more than 2000Hv, and can also be more than 2200Hv. The upper limit of the Vickers hardness of the grinding object surface is not particularly limited, for example, it can be about 7000Hv or less, can be 5000Hv or less, and can also be 3000Hv or less. It should be noted that in this specification, the Vickers hardness can be measured based on JISR1610:2003. The international standard corresponding to the above-mentioned JIS standard is ISO 14705:2000.

[0112] As materials having a Vickers hardness of more than 1500 Hv, silicon carbide, silicon nitride, titanium nitride, gallium nitride, etc. can be cited. The grinding object in the technology disclosed herein can have a single crystal surface of the above-mentioned material that is mechanically and chemically stable. Among them, the surface of the grinding object is preferably composed of any of silicon carbide and gallium nitride, and more preferably composed of silicon carbide. Silicon carbide is expected to be used as a compound semiconductor substrate material with low power loss and excellent heat resistance, and the practical advantage of improving productivity by increasing the grinding removal rate is particularly large. The technology disclosed herein is particularly preferably applied to the grinding of the single crystal surface of silicon carbide.

[0113] <Grinding method>

[0114] The polishing method disclosed herein can be used for polishing an object to be polished in a mode including the following operations, for example.

[0115] That is, prepare a polishing liquid (slurry) containing any grinding composition disclosed herein. The preparation of the above-mentioned polishing liquid may include the operation of preparing the polishing liquid by applying concentration adjustment (e.g., dilution) and pH adjustment to the grinding composition. Alternatively, the above-mentioned grinding composition may be directly used as a polishing liquid. In addition, in the case of a multi-component grinding composition, when preparing the above-mentioned grinding liquid, the operation of mixing these components, the operation of diluting one or more components before the mixing, the operation of diluting the mixture after the mixing, etc. may be included.

[0116] Then, the lapping liquid is supplied to the object to be polished, and the object to be polished is polished by the common method commonly used by those skilled in the art. For example, the object to be polished is mounted on a common polishing device, and the method of supplying the above-mentioned lapping liquid to the polishing object surface of the object to be polished by the lapping pad of the lapping device. Typically, the above-mentioned lapping liquid is continuously supplied while the lapping pad is pressed against the polishing object surface of the object to be polished and the two are moved relatively (for example, rotated). After this polishing process, the polishing of the object to be polished is completed.

[0117] It should be noted that, for each component that may be included in the polishing composition in the technology disclosed herein, the above-mentioned content (concentration) and content (concentration) ratio typically refer to the content and content ratio in the polishing composition when it is actually supplied to the polishing object (i.e., at the point of use), and therefore can be renamed as the content and content ratio in the polishing liquid.

[0118] According to the present specification, a grinding method for grinding a grinding object (typically a grinding object material) and a method for manufacturing a grinding object using the grinding method are provided. The above-mentioned grinding method is characterized in that it includes a process of grinding the grinding object using the grinding composition disclosed herein. A preferred grinding method includes: a process of performing preliminary polishing (preliminary polishing process) and a process of performing final polishing (final polishing process). In a typical embodiment, the preliminary polishing process is a polishing process arranged before the final polishing process. The preliminary polishing process can be a polishing process of one stage, or a polishing process of more than two stages. In addition, the final polishing process here is a process of final polishing of the grinding object that has been subjected to preliminary polishing, and is a polishing process that is arranged at the end (i.e., on the most downstream side) of the polishing process performed using a polishing slurry containing abrasive grains. In such a grinding method including a preliminary polishing process and a final polishing process, the grinding composition disclosed herein can be used in the preliminary polishing process, can be used in the final polishing process, or can be used in both the preliminary polishing process and the final polishing process.

[0119] Preliminary polishing and fine polishing can be applied to any of the grinding performed by a single-sided grinding device and the grinding performed by a double-sided grinding device. In a single-sided grinding device, the grinding object is attached to a ceramic plate with wax, or a retainer called a carrier is used to hold the grinding object, and a polishing composition is supplied while a grinding pad is pressed on a single side of the grinding object and the two are moved relative to each other, thereby grinding a single side of the grinding object. The above-mentioned movement is, for example, rotational movement. In a double-sided grinding device, a retainer called a carrier is used to hold the grinding object, and a polishing composition is supplied from above while a grinding pad is pressed on the opposite side of the grinding object, so that they rotate in relative directions, thereby simultaneously grinding both sides of the grinding object.

[0120] The conditions of the above-mentioned polishing are appropriately set based on the kind of the material ground, the surface properties (specifically smoothness) as the target, the grinding removal rate, etc., and are therefore not limited to specific conditions. For example, about processing pressure, the grinding composition disclosed herein can be used in a wide pressure range of more than 10kPa and less than 150kPa. From the perspective of improving the grinding removal rate, in some ways, the above-mentioned processing pressure can be, for example, more than 5kPa, more than 10kPa, more than 20kPa, more than 30kPa or more than 40kPa, in addition, it can be set to less than 100kPa, less than 80kPa or less than 60kPa. The grinding composition disclosed herein can also be preferably used for grinding under, for example, more than 30kPa or higher processing conditions, and the productivity of the target product (ground product) obtained through the grinding can be improved. It should be noted that the processing pressure mentioned here is the same as the meaning of grinding pressure.

[0121] The grinding pad used in each polishing process disclosed herein is not particularly limited. For example, any type of nonwoven type, suede type, and rigid foamed polyurethane type can be used. In some embodiments, a grinding pad of a rigid foamed polyurethane type can be preferably used. It should be noted that the grinding pad used in the technology disclosed herein is a grinding pad that does not contain abrasive particles.

[0122] The object to be polished by the method disclosed herein is typically cleaned after polishing. A suitable cleaning solution can be used for the cleaning. The cleaning solution used is not particularly limited, and a known, commonly used cleaning solution can be appropriately selected and used.

[0123] It should be noted that, in the grinding method disclosed herein, in addition to the above-mentioned preliminary polishing process and the fine polishing process, any other process may be included. As such a process, a mechanical grinding process and a grinding process performed before the preliminary polishing process may be cited. In the above-mentioned mechanical grinding process, a liquid in which diamond abrasive grains are dispersed in a solvent is used to grind the grinding object. In some preferred embodiments, the above-mentioned dispersion does not contain an oxidant. The above-mentioned grinding process is a process in which a grinding plate, such as the surface of a cast iron plate, is pressed against the grinding object for grinding. Therefore, a grinding pad is not used in the grinding process. In the grinding process, typically, abrasive grains are supplied between the grinding plate and the grinding object. The above-mentioned abrasive grains are typically diamond abrasive grains. In addition, the grinding method disclosed herein may also include additional processes before the preliminary polishing process and between the preliminary polishing process and the fine polishing process. The additional process is, for example, a cleaning process and a polishing process.

[0124] <Method for producing ground material>

[0125] The technology disclosed herein may include: providing a method for manufacturing a grinding object including a polishing process based on any of the above-mentioned grinding methods and a grinding object manufactured by the method. The above-mentioned method for manufacturing a grinding object is, for example, a method for manufacturing a silicon carbide substrate. That is, according to the technology disclosed herein, a method for manufacturing a grinding object including a process of grinding a grinding object having a surface composed of a high-hardness material using any of the grinding methods disclosed herein and a grinding object manufactured by the method are provided. According to the above-mentioned manufacturing method, a substrate manufactured by grinding, such as a silicon carbide substrate, can be efficiently provided.

[0126] Example

[0127] Hereinafter, some examples related to the present invention will be described, but the present invention is not intended to be limited to the contents shown in these examples. It should be noted that "%" in the following description is based on weight unless otherwise specified.

[0128] Experiment 1

[0129] <Preparation of polishing composition>

[0130] (Example S1)

[0131] Silica abrasive, sodium permanganate as an oxidizing agent, zirconium oxynitrate as a transition metal salt C, and deionized water were mixed to prepare a polishing composition containing 0.1% silica abrasive, 12.0% sodium permanganate, and 30 mM zirconium oxynitrate (Zr conversion). It should be noted that when preparing the polishing composition of this example, no pH adjuster was used. The pH of the polishing composition involved in this example is shown in Table 1.

[0132] (Example S2 to Example S4)

[0133] The polishing composition of each example was prepared in the same manner as in Example S1 except that the concentration of sodium permanganate was as shown in Table 1. The pH of the polishing composition of each example is shown in Table 1.

[0134] (Example S5)

[0135] Silica abrasive, potassium permanganate as an oxidizing agent, aluminum nitrate as metal salt A, and deionized water were mixed to prepare a polishing composition containing 0.1% of silica abrasive, 4.0% of potassium permanganate, and 30 mM aluminum nitrate (based on Al).

[0136] (Example S6)

[0137] The polishing composition of this example was prepared in the same manner as in Example S5 except that the types of the metal salts were as shown in Table 1. The pH of the polishing composition of this example is as shown in Table 1.

[0138] (Example S7)

[0139] Silica abrasive, potassium permanganate as an oxidizing agent, and deionized water were mixed to try to prepare a polishing composition containing 0.1% silica abrasive and 12.0% potassium permanganate. However, since the mixed potassium permanganate was not completely dissolved, a polishing composition of the above composition could not be prepared. For Example S7, "Unable" is displayed in the "Composition" column of Table 1.

[0140] (Example S8)

[0141] The polishing composition of this example was prepared in the same manner as in Example S1 except that the types of the metal salts were as shown in Table 1. The pH of the polishing composition of this example is shown in Table 1.

[0142] In the polishing compositions of Examples S1 to S8, colloidal silica having an average primary particle size of 35 nm was used as the silica abrasive grains.

[0143] <Polishing of polishing object>

[0144] A SiC wafer was pre-polished using a pre-polishing composition containing aluminum oxide abrasive grains, and the pre-polished SiC wafer was used as a polishing object, and the polishing composition according to each example was used as a polishing liquid as it was, and the polishing object was polished under the following polishing conditions.

[0145] [Polishing conditions]

[0146] Grinding machine: Fujikoshi Machinery Co., Ltd., model "RDP-500"

[0147] Polishing pad: Nitta Dupont "IC-1000" (made of hard polyurethane)

[0148] Processing pressure: 490gf / cm 2

[0149] Plate speed: 130 rpm

[0150] Grinding head speed: 130 rpm

[0151] Polishing liquid supply rate: 20mL / min

[0152] How to use the grinding fluid: one-time use

[0153] Grinding time: 5 minutes

[0154] Polishing object: 4-inch SiC wafer (conductive type: n-type, crystalline type 4H-SiC, deviation angle of the main surface (0001) relative to the C axis: 4°), 1 piece / batch

[0155] Grinding fluid temperature: 23°C

[0156] As a polishing pad, a polishing pad was used in which the polishing surface of the pad was subjected to brush conditioning for 5 minutes, diamond conditioning for 3 minutes, and brush conditioning for 5 minutes. The brush conditioning and diamond conditioning were performed before the above-mentioned polishing.

[0157] <Measurement and evaluation>

[0158] (Grinding removal rate)

[0159] Based on the above polishing conditions, the SiC wafer was polished using the polishing composition of each example, and then the polishing removal rate was calculated according to the following calculation formulas (1) and (2).

[0160] (1) Polishing removal [cm] = Difference in weight of SiC wafer before and after polishing [g] / SiC density [g / cm 3 ](=3.21g / cm 3 ) / grinding object area [cm 2 ](=78.54cm 2 )

[0161] (2) Grinding removal rate [nm / h] = Grinding allowance [cm] × 10 7 / Grinding time (=5 / 60 hours)

[0162] The obtained results were converted into relative values ​​with the polishing removal rate of Example S5 being 100%. A larger value indicates a better polishing removal rate.

[0163] The polishing removal rate obtained for each example is shown in the corresponding column of Table 1.

[0164] [Table 1]

[0165]

[0166] From the results shown in Table 1, it can be clearly confirmed that the polishing removal rate tends to increase when the content of sodium permanganate as an oxidant is increased. It is also confirmed that by further adding a transition metal salt C to a polishing composition containing sodium permanganate as an oxidant, the polishing removal rate tends to increase compared to adding a metal salt A other than the transition metal salt C. In Example S7 using 12% potassium permanganate as an oxidant, no polishing composition was obtained.

[0167] Experiment 2

[0168] <Preparation of polishing composition>

[0169] (Example A1)

[0170] Alumina abrasive grains, sodium permanganate as an oxidizing agent, zirconium oxynitrate as a transition metal salt C, and deionized water were mixed to prepare a polishing composition containing 0.1% of aluminum oxide abrasive grains, 12.0% of sodium permanganate, and 40 mM zirconium oxynitrate (Zr conversion). It should be noted that when preparing the polishing composition of this example, no pH adjuster was used. The pH of the polishing composition involved in this example is shown in Table 2.

[0171] (Example A2 to Example A6)

[0172] The polishing composition of each example was prepared in the same manner as in Example A1 except that the concentration of sodium permanganate and the concentration of zirconium oxynitrate were as shown in Table 2.

[0173] (Example A7)

[0174] Alumina abrasive, potassium permanganate as an oxidizing agent, aluminum nitrate as metal salt A, and deionized water were mixed to prepare a polishing composition containing 0.1% of aluminum oxide abrasive, 4.0% of potassium permanganate, and 30 mM aluminum nitrate (in terms of Al). It should be noted that no pH adjuster was used when preparing the polishing composition of this example. The pH of the polishing composition involved in this example is shown in Table 2.

[0175] (Example A8)

[0176] The polishing composition of this example was prepared in the same manner as in Example A7 except that the types and amounts of the metal salts were as shown in Table 2. The pH of the polishing composition of this example is shown in Table 2.

[0177] (Example A9)

[0178] Alumina abrasive grains, potassium permanganate as an oxidizing agent, and deionized water were mixed to attempt to prepare a polishing composition containing 0.1% of aluminum oxide abrasive grains and 12.0% of potassium permanganate. However, since the mixed potassium permanganate was not completely dissolved, a polishing composition of the above composition could not be prepared. For Example A9, "Unable" is displayed in the "Composition" column of Table 2.

[0179] (Example A10)

[0180] The polishing composition of this example was prepared in the same manner as in Example A1 except that the types of the metal salts were as shown in Table 2. The pH of the polishing composition of this example is shown in Table 2.

[0181] In the polishing compositions of Examples A1 to A10, α-alumina abrasive grains having an average primary particle size of 310 nm were used as the alumina abrasive grains.

[0182] <Polishing of polishing object>

[0183] A SiC wafer was pre-polished using a pre-polishing composition containing aluminum oxide abrasive grains, and the pre-polished SiC wafer was used as a polishing object, and the polishing composition according to each example was used as a polishing liquid as it was, and the polishing object was polished under the following polishing conditions.

[0184] [Polishing conditions]

[0185] Grinding machine: Fujikoshi Machinery Co., Ltd., model "RDP-500"

[0186] Polishing pad: Nitta Dupont "IC-1000" (made of hard polyurethane)

[0187] Processing pressure: 490gf / cm 2

[0188] Plate speed: 130 rpm

[0189] Grinding head speed: 130 rpm

[0190] Polishing liquid supply rate: 20mL / min

[0191] How to use the grinding fluid: one-time use Grinding time: 5 minutes

[0192] Polishing object: 4-inch SiC wafer (conductive type: n-type, crystalline type 4H-SiC, deviation angle of the main surface (0001) relative to the C axis: 4°), 1 piece / batch

[0193] Grinding fluid temperature: 23°C

[0194] As a polishing pad, a polishing pad was used in which the polishing surface of the pad was subjected to brush conditioning for 5 minutes, diamond conditioning for 3 minutes, and brush conditioning for 5 minutes. The brush conditioning and diamond conditioning were performed before the above-mentioned polishing.

[0195] <Measurement and evaluation>

[0196] (Grinding removal rate)

[0197] Based on the above polishing conditions, the SiC wafer was polished using the polishing composition of each example, and then the polishing removal rate was calculated according to the following calculation formulas (1) and (2).

[0198] (1) Polishing removal [cm] = Difference in weight of SiC wafer before and after polishing [g] / SiC density [g / cm 3 ](=3.21g / cm 3 ) / grinding object area [cm 2 ](=78.54cm2 )

[0199] (2) Grinding removal rate [nm / h] = Grinding allowance [cm] × 10 7 / Grinding time (=5 / 60 hours)

[0200] The obtained results were converted into relative values ​​with the polishing removal rate of Example A7 being 100%. A larger value indicates a better polishing removal rate.

[0201] The polishing removal rate obtained for each example is shown in the corresponding column of Table 2.

[0202] [Table 2]

[0203]

[0204] From the results shown in Table 2, it can be clearly confirmed that the polishing removal rate tends to increase when the content of sodium permanganate as an oxidant is increased. It is also confirmed that by further adding a transition metal salt C to a polishing composition containing sodium permanganate as an oxidant, the polishing removal rate tends to increase compared to adding a metal salt A other than the transition metal salt C. In Example A9 using 12% potassium permanganate as an oxidant, no polishing composition was obtained.

[0205] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the claims. The technology described in the claims includes various modifications and changes to the specific examples described above.

Claims

1. A polishing composition comprising: Sodium permanganate as an oxidizing agent, a transition metal salt different from the oxidizing agent, and water, The polishing composition contains more than 10 wt % of the oxidizing agent.

2. The polishing composition according to claim 1, wherein The transition metal salt is an oxygen transition metal salt, or a polynuclear transition metal complex containing a transition metal and oxygen and / or hydrogen. The polishing composition according to claim 1 or 2, further comprising abrasive grains. 4 . The polishing composition according to claim 1 , wherein the pH thereof is 1.0 or more and less than 6.

0. 5 . The polishing composition according to claim 1 , which is used for polishing a material having a Vickers hardness of 1500 Hv or more. 6 . The polishing composition according to claim 1 , which is used for polishing silicon carbide. 7 . A polishing method comprising the step of polishing an object to be polished using the polishing composition according to claim 1 .

8. A multi-component polishing composition comprising: Part A, which contains sodium permanganate as an oxidizing agent and water; Part B, which comprises a transition metal salt different from the oxidant and water, The multi-component polishing composition contains more than 10 wt % of the oxidizing agent.

9. The multi-component polishing composition according to claim 8, wherein: The transition metal salt is an oxygen transition metal salt or a multinuclear transition metal complex containing a transition metal, oxygen and hydrogen.

10. The multi-component polishing composition according to claim 8 or 9, wherein: The A part or the B part contains abrasive particles. 11 . The multi-component polishing composition according to claim 8 , further comprising a part C different from the part A and the part B, wherein the part C contains abrasive grains. 12 . The multi-component polishing composition according to claim 8 , which is used for polishing a material having a Vickers hardness of 1500 Hv or more. 13 . The multi-component polishing composition according to claim 8 , which is used for polishing silicon carbide. 14 . A polishing method comprising the step of polishing an object to be polished using the multi-component polishing composition according to claim 8 .

15. The grinding method according to claim 14, wherein: The part A and the part B are mixed, and when the multi-component polishing composition further includes a part C, the part C is also mixed, and the mixed polishing composition is supplied to an object to be polished to perform polishing.