High-load positive electrode, slurry for positive electrode, and lithium secondary battery

By using fluorine-containing adhesives and high-molecular-weight hydrogenated nitrile rubber in lithium secondary batteries, the structure of lithium iron phosphate is optimized, and the problem of insufficient positive electrode adhesion and flexibility in lithium secondary batteries is solved, and the problem of improved The energy density and capacity of the battery.

CN118974975APending Publication Date: 2024-11-15LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380034180.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-26
Filing Date
2023-10-26
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

When lithium iron phosphate is used as the positive electrode active material in the existing lithium secondary batteries, there are problems of poor adhesion and insufficient flexibility, resulting in electrode disengagement and reduced battery capacity.

Method used

Using fluorine-containing adhesive and high molecular weight hydrogenated nitrile rubber as adhesives, combined with conductive materials such as carbon nanotubes, optimize the particle size and structure of lithium iron phosphate to form a positive electrode active material layer with high load capacity, and improve the positive electrode Adhesion and flexibility to current collector.

Benefits of technology

It significantly improves the adhesion and flexibility of the positive electrode, prevents the electrode from falling apart, reduces the battery resistance, and increases the energy density and capacity of the secondary battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
  • Figure SMS_4
    Figure SMS_4
Patent Text Reader

Abstract

The positive electrode according to the present invention comprises a positive electrode active material layer having a loading amount of 450 mg / 25 cm2 or more, the positive electrode active material layer comprising a lithium iron phosphate, a fluorine-containing binder, a rubber-based binder, and a conductive material, in which the rubber-based binder comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and the content of the second hydrogenated nitrile rubber is 0.2 wt% to 0.8 wt% based on the total weight of the positive electrode active material layer.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] This application claims the benefit of priority to Korean Patent Application Nos. 10-2022-0139395, 10-2022-0139469, 10-2022-0139490, and 10-2022-0139418 filed on October 26, 2022.

[0002] The present invention relates to a positive electrode including lithium iron phosphate as a positive electrode active material, a slurry for the positive electrode and a lithium secondary battery, and more particularly, to a high-load positive electrode with improved adhesion and flexibility, a slurry for the positive electrode and a lithium secondary battery including the same. Background Art

[0003] As the technology of electric vehicles and energy storage systems (ESS) develops and the demand increases, the demand for batteries as energy sources is rapidly increasing, and research is being conducted on batteries that can meet various needs. In particular, lithium secondary batteries with high energy density and excellent life and cycle characteristics are being actively studied as power sources for these devices.

[0004] As a positive electrode active material in a lithium secondary battery, lithium cobalt oxide (LCO), lithium nickel cobalt manganese oxide (LNCMO), and lithium iron phosphate (LFP) are used.

[0005] Because lithium iron phosphate contains iron, which is a material that is abundant in resources and low in cost, its cost is low. In addition, the low toxicity of lithium iron phosphate reduces the environmental impact of using lithium iron phosphate. In addition, because lithium iron phosphate has an olivine structure, it can stably maintain the active material structure at high temperatures compared to lithium transition metal oxides with a layered structure. Therefore, it has the advantages of excellent high temperature stability and high temperature life characteristics of the battery.

[0006] However, compared with lithium transition metal oxides such as lithium nickel cobalt manganese oxide, lithium iron phosphate has poor lithium mobility and low conductivity. Therefore, lithium iron phosphate with a small average particle size is used to form a short lithium migration path, the surface of the lithium iron phosphate is coated with carbon to improve conductivity, and an excess of conductive material is used.

[0007] However, as the particle size of lithium iron phosphate particles decreases, the specific surface area increases, and the lithium iron phosphate coated with carbon on the surface has poor solvent wetting ability. As a result, the particles of lithium iron phosphate are seriously aggregated, which reduces the stability and coating processability of the positive electrode slurry, and the binder cannot be effectively mixed with the lithium iron phosphate, thereby reducing the adhesion between the positive electrode collector and the positive electrode active material layer when manufacturing the positive electrode (hereinafter referred to as positive electrode adhesion). This phenomenon may be exacerbated in a high-load positive electrode.

[0008] If the positive electrode adhesion is deteriorated, detachment of the positive electrode active material layer may occur during electrode manufacturing or charge and discharge, which increases battery resistance and reduces the capacity of the secondary battery.

[0009] Korean Patent Publication No. 10-2020-0008066 discloses a binder composition for a secondary battery electrode, the binder composition comprising an alkylene structural unit and a nitrile group-containing monomer unit, and a copolymer having a predetermined Mooney viscosity, thereby dispersing a conductive material in a good manner, but when applied to a positive electrode using lithium iron phosphate as a positive electrode active material, it is unsatisfactory in terms of improving adhesion and flexibility.

[0010] As the demand for high energy density batteries increases, it is necessary to achieve 600 mg / 25 cm in cathodes containing lithium iron phosphate. 2 Technology to improve positive electrode adhesion and flexibility while achieving the above loading amounts. Summary of the invention

[0011] [Technical issues]

[0012] An object of the present invention is to provide a positive electrode and a lithium secondary battery having improved adhesion between a positive electrode current collector and a positive electrode active material layer and improved flexibility in a high-load positive electrode comprising lithium iron phosphate, thereby preventing electrode detachment, reducing battery resistance, and improving battery capacity.

[0013] [Technical solution]

[0014] According to one embodiment of the present invention, a positive electrode is provided. The positive electrode is a positive electrode having a positive electrode active material layer disposed on one side or both sides of a current collector, wherein

[0015] The positive electrode active material layer comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder and a conductive material, wherein

[0016] The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and

[0017] The second hydrogenated nitrile rubber is included in an amount of 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

[0018] In the positive electrode according to an exemplary embodiment, the positive electrode active material layer has a carbon content of 450 mg / 25 cm 2 Up to 700 mg / 25 cm 2 load within the range.

[0019] In the positive electrode according to one exemplary embodiment, the second hydrogenated nitrile rubber has a weight average molecular weight (Mw) of about 150,000 g / mol to about 1,000,000 g / mol.

[0020] In the positive electrode according to an exemplary embodiment, the first hydrogenated nitrile rubber is included in an amount of 0.1 wt % to 0.6 wt % based on the total weight of the positive electrode active material layer.

[0021] In the positive electrode according to one exemplary embodiment, the content of the lithium iron phosphate is 92.7 wt % to 98.4 wt % based on the total weight of the positive electrode active material layer.

[0022] In the positive electrode according to one exemplary embodiment, the content of the fluorine-containing binder in the positive electrode active material layer is 1.0 wt % to 4.0 wt %.

[0023] In the positive electrode according to one exemplary embodiment, the content of the rubber-based binder in the positive electrode active material layer is 0.5 wt % to 1.5 wt %.

[0024] In the positive electrode according to an exemplary embodiment, the content of the second hydrogenated nitrile rubber in the positive electrode active material layer is 0.3 wt % to 0.7 wt %.

[0025] In the positive electrode according to one exemplary embodiment, the second hydrogenated nitrile rubber is 33 wt % or less based on the total weight of the fluorine-containing binder and the second hydrogenated nitrile rubber.

[0026] In the positive electrode according to one exemplary embodiment, the lithium iron phosphate is a compound represented by Chemical Formula 1 below.

[0027] [Chemical formula 1]

[0028] Li 1+a Fe 1-x M x (PO 4-b )X b

[0029] (In Chemical Formula 1,

[0030] M comprises one or more elements selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn and Y,

[0031] X contains one or more elements selected from F, S and N, and

[0032] a, b and x are -0.5≤a≤0.5, 0≤b≤0.1 and 0≤x≤0.5 respectively)

[0033] In the positive electrode according to an exemplary embodiment, the positive electrode adhesion measured in an adhesion test in which the positive electrode active layer is peeled from the aluminum thin film at 90° is greater than or equal to 19 gf / 20 mm.

[0034] In the positive electrode according to an exemplary embodiment, in a flexibility test in which a phi-dedicated measuring bar was contacted on the positive electrode active material layer and the cross section of the positive electrode was lifted, cracks occurred in the case of a measuring bar of 5 phi (ø) or less.

[0035] In the positive electrode according to one exemplary embodiment, the fluorine-containing binder has a weight average molecular weight (Mw) of 800,000 g / mol or more.

[0036] In the positive electrode according to an exemplary embodiment, the conductive material is a carbon nanotube.

[0037] In the positive electrode according to one exemplary embodiment, the content of the conductive material is 0.3 wt % to 2.0 wt % based on the total weight of the positive electrode active material layer.

[0038] In the positive electrode according to one exemplary embodiment, the total weight of the binder included in the positive electrode active material layer is 2.0 wt % to 4.5 wt % based on the total weight of the positive electrode active material.

[0039] In the positive electrode according to one exemplary embodiment, the lithium iron phosphate has an average particle size D of 0.3 μm to 20.0 μm. 50 .

[0040] In the positive electrode according to one exemplary embodiment, the lithium iron phosphate has a single body structure composed of primary particles.

[0041] According to another exemplary embodiment of the present invention, a lithium secondary battery is provided. The lithium secondary battery comprises a positive electrode, a negative electrode, a separator and an electrolyte, wherein

[0042] The positive electrode has a positive electrode active material layer disposed on one or both sides of the current collector,

[0043] The positive electrode active material layer comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder and a conductive material.

[0044] wherein the rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and

[0045] The second hydrogenated nitrile rubber is included in an amount of 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

[0046] According to another exemplary embodiment of the present invention, a positive electrode slurry is provided. The positive electrode slurry comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder, a conductive material and a solvent, wherein

[0047] The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and

[0048] The second hydrogenated nitrile rubber is included in an amount of 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

[0049] In the slurry for a positive electrode according to an exemplary embodiment, the second hydrogenated nitrile rubber has a weight average molecular weight (Mw) of about 150,000 g / mol to about 1,000,000 g / mol.

[0050] In the slurry for a positive electrode according to an exemplary embodiment, the fluorine-containing binder has a weight average molecular weight (Mw) of 800,000 g / mol or more.

[0051] In the slurry for a positive electrode according to an exemplary embodiment, the solid content of the slurry for a positive electrode ranges from 50 wt % to 75 wt %.

[0052] In the slurry for a positive electrode according to an exemplary embodiment, the viscosity of the slurry for a positive electrode measured at 25° C. and a shear rate of 2.5 / s is 5,000 cps to 25,000 cps.

[0053] In the slurry for a positive electrode according to an exemplary embodiment, the content of the fluorine-containing binder is 1.0 wt % to 4.0 wt % based on the total weight of the solid matter in the slurry for a positive electrode.

[0054] In the positive electrode slurry according to an exemplary embodiment, the first hydrogenated nitrile rubber is contained in an amount of 0.1 wt % to 0.6 wt % based on the total weight of solids in the positive electrode slurry.

[0055] In the positive electrode slurry according to an exemplary embodiment, the content of the lithium iron phosphate is 92.7 wt % to 98.4 wt % based on the total weight of the solid matter in the positive electrode slurry.

[0056] In the slurry for a positive electrode according to an exemplary embodiment, the second hydrogenated nitrile rubber is 33 wt % or less based on the total weight of the fluorine-containing binder and the second hydrogenated nitrile rubber.

[0057] In the slurry for a positive electrode according to an exemplary embodiment, the content of the rubber-based binder is 0.5 wt % to 1.5 wt % based on the total weight of solids in the slurry for a positive electrode.

[0058] In the slurry for a positive electrode according to an exemplary embodiment, the lithium iron phosphate is a compound represented by Chemical Formula 1 below.

[0059] [Chemical formula 1]

[0060] Li 1+a Fe 1-x M x (PO 4-b )X b

[0061] (In Chemical Formula 1,

[0062] M comprises one or more elements selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn and Y,

[0063] X contains one or more elements selected from F, S and N, and

[0064] a, b and x are -0.5≤a≤0.5, 0≤b≤0.1 and 0≤x≤0.5 respectively)

[0065] In the slurry for a positive electrode according to an exemplary embodiment, the conductive material is a carbon nanotube.

[0066] In the slurry for a positive electrode according to an exemplary embodiment, the content of the conductive material is 0.3 wt % to 2.0 wt % based on the total weight of the solid matter in the slurry for a positive electrode.

[0067] In the positive electrode slurry according to an exemplary embodiment, the total weight of the fluorine-containing binder and the rubber-based binder is 2.0 wt % to 4.5 wt % based on the total weight of the solid matter in the positive electrode slurry.

[0068] [Beneficial Effects]

[0069] According to the present invention, the present invention has significantly improved the 2 Up to 700 mg / 25 cm 2 Effect of high loading amount of positive electrode active material layer on the flexibility of positive electrode.

[0070] According to the present invention, by controlling the contents of the fluorine-containing binder, the first hydrogenated nitrile rubber and the second hydrogenated nitrile rubber within a predetermined range, good coating stability of the slurry for the positive electrode and good flexibility of the positive electrode can be simultaneously obtained.

[0071] The positive electrode according to the present invention has excellent adhesion and flexibility even when the content of the binder contained in the positive electrode active material layer is reduced due to improved adhesion, and the content of the positive electrode active material can be increased by reducing the content of the binder, thereby making the energy density of the secondary battery excellent.

[0072] According to an exemplary embodiment of the present invention, by including the fluorine-containing binder and the second hydrogenated nitrile rubber in an appropriate weight ratio, a positive electrode slurry that is easily mixed and has excellent coating stability may be prepared.

[0073] According to the present invention, a positive electrode slurry can be provided in which a positive electrode active material, a binder and a conductive material are well dispersed despite a high solid content, and in particular, aggregation of the positive electrode active material and the conductive material is suppressed, thereby enabling the manufacture of a positive electrode having excellent conductivity. DETAILED DESCRIPTION

[0074] Reference to the detailed description of the embodiments will make the advantages and features of the present invention and the methods for achieving them become apparent. However, the present invention is not limited to the embodiments disclosed herein and can be implemented in many different forms, and these embodiments are provided only to make the content of the present invention complete and to fully disclose the scope of the present invention to those skilled in the art, and the present invention is limited by the scope of the claims.

[0075] Unless otherwise defined, all terms (including technical and scientific terms) used herein are intended to be used in the sense that they would be understood by one of ordinary skill in the art to which the invention belongs, and terms defined in commonly used dictionaries should not be ideally or over-interpreted unless explicitly and specifically defined.

[0076] The terms used herein are intended to describe embodiments, rather than to limit the present invention. In this specification, unless the context otherwise mentions, the singular includes the plural. The words "comprising" and / or "including" used in the specification do not exclude the presence or addition of one or more other components other than the above components.

[0077] In the present specification, when any part is referred to as including any component, unless there is a specific description to the contrary, it does not mean to exclude any other component but includes additional components.

[0078] In this specification, the description of "A and / or B" means A, or B, or A and B.

[0079] In this specification, "%" means weight % unless otherwise specified.

[0080] In this manual, D 50It refers to the particle size corresponding to 50% volume accumulation in the particle size distribution curve. For example, D 50 This can be measured using laser diffraction, which is typically capable of measuring particle sizes from the submicron range to several millimeters and can produce highly reproducible and highly resolvable results.

[0081] In this specification, the "specific surface area" is measured by the BET method and can be calculated using the nitrogen adsorption amount at liquid nitrogen temperature (77 K) using BELSORP-minoII of BEL Japan.

[0082] In this specification, "Mw" refers to the weight average molecular weight of standard polystyrene measured by gel permeation chromatography (GPC). Specifically, Mw is a conversion of a value measured by GPC under the following conditions, and is calibrated using standard polystyrene in an Agilent system.

[0083] <Measurement conditions>

[0084] Measuring instrument: Agilent GPC (Agulent 1200 series, USA)

[0085] Column: Two connected PL Mix B

[0086] Column temperature: 40°C

[0087] Eluent: Tetrahydrofuran

[0088] Flow rate: 1.0 mL / min

[0089] Concentration: ~1 mg / mL (100 μL injection)

[0090] In the present invention, the positive electrode adhesion can be measured in the following manner. A positive electrode cut into a length of 150 mm and a width of 20 mm is prepared, and the positive electrode active material layer is placed to face a slide glass having a length of 75 mm and a width of 25 mm, and the positive electrode is pasted to the slide glass in the longitudinal direction with a double-sided tape. That is, the slide glass is pasted to an area corresponding to half of the longitudinal direction of the positive electrode. Then, the evaluation sample is prepared by rubbing the roller 10 times so that the double-sided tape is evenly pasted. Next, the slide glass portion of the evaluation sample is fixed to the sample stage of a universal testing machine (Universal Testing Machine) (UTM) (LS5, AMETEK), and the half of the positive electrode without the slide glass pasted is connected to the load sensor of the UTM machine. By applying a force at 90 °, the load sensor is moved to 50 mm at a speed of 100 mm / min, and the load applied to the load sensor is measured. Here, the average value of the load was measured at a portion of 20 mm to 40 mm of the stroke, repeated five times, and the average value thereof was evaluated as the positive electrode adhesion force (gf / 20 mm) of each sample.

[0091] In this specification, the positive electrode flexibility can be measured in the following manner. A measuring rod of each phi (ø) is prepared and a loading amount of 600 mg / 25 cm 2 The positive electrode was cut into a length of 10 cm and a width of 30 cm. The cut positive electrode was bent in half to contact the measuring rod, and both ends of the positive electrode were lifted at a speed of 10 mm / min. Here, it was lifted until the force measured on the universal testing machine (UTM) was 5 N. Each phi was measured to observe whether the electrode had cracks under an optical microscope, and if there were no cracks, a smaller phi was used for the test.

[0092] Hereinafter, the present invention will be described in detail.

[0093] positive electrode

[0094] The positive electrode according to an exemplary embodiment of the present invention is a positive electrode having a positive electrode active material layer disposed on one side or both sides of a current collector, wherein

[0095] The positive electrode active material layer comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder and a conductive material, wherein

[0096] The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and

[0097] The second hydrogenated nitrile rubber is included in an amount of 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

[0098] Because lithium iron phosphate has poor lithium mobility and low conductivity compared to lithium transition metal oxides such as lithium nickel cobalt manganese oxide, lithium iron phosphate with a small average particle size is generally used as a positive electrode active material. However, the small size of lithium iron phosphate particles increases the specific surface area, which leads to severe particle aggregation, which hinders the effective mixing of lithium iron phosphate with the binder, thereby reducing the positive electrode adhesion. As a result, the detachment of the positive electrode active material layer occurs during electrode manufacturing or charging and discharging, increasing the battery resistance and reducing the capacity of the secondary battery.

[0099] To solve these problems, the present inventors have conducted research and have found that when the rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, the dispersibility of lithium iron phosphate particles is improved and aggregation thereof is suppressed, while the molecular weight of the second hydrogenated nitrile rubber having a weight average molecular weight of 450 mg / 25 cm 2 Up to 700 mg / 25 cm 2 The adhesion and flexibility of the high-load positive electrode with a certain loading amount are improved, thereby completing the present invention.

[0100] The positive electrode according to one embodiment of the present invention has a structure in which the positive electrode active material layer is in direct contact with the positive electrode collector because the interfacial adhesion between the positive electrode active material layer and the positive electrode collector is excellent, and a separate layer for improving the adhesion between the positive electrode active material layer and the positive electrode collector may not be included. In other words, the positive electrode according to one embodiment of the present invention may exhibit excellent interfacial adhesion between the positive electrode collector and the positive electrode active material layer without including a separate layer such as a bonding layer or an adhesion layer or a bonding layer or a primer layer that may be inserted to improve adhesion.

[0101] The positive electrode according to one embodiment of the present invention may include a positive electrode active material layer. Specifically, the positive electrode according to the present invention may include a positive electrode current collector and a positive electrode active material layer located on at least one side of the positive electrode current collector.

[0102] In one embodiment, the loading amount of the positive electrode active material layer may be at least 450 mg / 25 cm 2 , more particularly 450 mg / 25 cm 2 Up to 700 mg / 25 cm 2 , more particularly 500 mg / 25 cm 2 Up to 700 mg / 25 cm 2, more particularly 550 mg / 25 cm 2 Up to 650 mg / 25 cm 2 Here, the loading amount is the loading amount of the positive electrode active material layer stacked on one side of the current collector.

[0103] The positive electrode current collector may be, but is not limited to, any current collector that is conductive and does not cause chemical changes in the battery. As the current collector, for example, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used.

[0104] The positive electrode current collector may have a thickness of 3 μm to 500 μm, and fine concavoconvexities may be formed on the surface of the positive electrode current collector to increase the adhesion to the positive electrode active material layer. For example, it may be used in various forms such as films, sheets, foils, nets, porous materials, foams, nonwoven fabrics, etc.

[0105] The positive electrode active material layer may include a positive electrode active material. In addition, the positive electrode active material layer may further include a conductive material, a binder, and a dispersant as needed in addition to the positive electrode active material.

[0106] Hereinafter, each component contained in the positive electrode active material layer will be described in detail.

[0107] (1) Positive electrode active material

[0108] The present invention includes lithium iron phosphate as a positive electrode active material. Because the lithium iron phosphate has an olivine structure, the active material structure remains stable at high temperatures compared to lithium transition metal oxides having a layered structure. As a result, when the lithium iron phosphate is used as a positive electrode active material, the high temperature stability and high temperature life characteristics of the positive electrode can be significantly improved, thereby reducing the fire hazard of a lithium secondary battery including the positive electrode, etc.

[0109] The lithium iron phosphate may be a compound of Chemical Formula 1 below.

[0110] [Chemical formula 1]

[0111] Li 1+a Fe 1-x M x (PO 4-b )X b

[0112] (In Chemical Formula 1,

[0113] M comprises one or more elements selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn and Y,

[0114] X contains one or more elements selected from F, S and N, and

[0115] a, b and x are -0.5≤a≤0.5, 0≤b≤0.1 and 0≤x≤0.5 respectively)

[0116] For example, the lithium iron phosphate may be LiFePO 4 .

[0117] The lithium iron phosphate may be a secondary particle in which primary particles are aggregated together, and preferably has a single body structure composed of primary particles.

[0118] In the context of the present invention, the term "monolith structure" refers to a structure in which particles exist as independent phases that are not aggregated to form a morphological shape. As a particle structure in contrast to such a monolithic structure, a structure in which smaller particles ("primary particles") are physically and / or chemically aggregated to form relatively larger particles ("secondary particles") can be exemplified.

[0119] Compared with when the lithium iron phosphate particles are secondary particles, when the lithium iron phosphate has a single body structure composed of primary particles, the lithium iron phosphate particles are less likely to crack during the rolling process, thereby reducing the capacity due to the detachment of the cracked particles, which is desirable. In addition, when the lithium iron phosphate is a primary particle with a single body structure, the migration of the binder during the drying process of the positive electrode slurry can be alleviated, which may be desirable in terms of the interfacial adhesion between the positive electrode collector and the positive electrode active material layer.

[0120] The lithium iron phosphate may include a carbon coating on its surface. When the carbon coating is formed on the surface of the lithium iron phosphate, the electrical conductivity is enhanced, which can improve the resistance characteristics of the positive electrode.

[0121] The carbon coating layer can be formed using at least one raw material selected from the group consisting of glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, polymers of furfuryl alcohol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, asphalt resins, and tar resins. Specifically, the carbon coating layer can be formed by mixing the raw materials with lithium iron phosphate, followed by heat treatment.

[0122] Average particle size D of lithium iron phosphate 50 The average particle size D of the positive electrode active material may be 0.3 μm to 20.0 μm, more particularly 0.4 μm to 10.0 μm, and more particularly 0.5 μm to 3.0 μm. 50 When the above range is met, the mobility of lithium in lithium iron phosphate can be improved, thereby improving the charge and discharge characteristics of the battery.

[0123] The BET specific surface area of ​​lithium iron phosphate can be 5 m2 / g to 20 m 2 / g, more specifically 7 m 2 / g to 18 m 2 / g, more specifically 9 m 2 / g to 16 m 2 / g. Compared with conventional lithium iron phosphate, the above range corresponds to a lower value. When this range is satisfied, even in a positive electrode slurry composition with a relatively low dispersant content, aggregation of lithium iron phosphate can be effectively suppressed.

[0124] In one embodiment of the present invention, the lithium iron phosphate may include 50 In this case, the first lithium iron phosphate particles may have an average particle size D in the range of 0.5 μm to 2 μm. 50 , and the second lithium iron phosphate particles may have an average particle size D in the range of 3.5 μm to 15 μm 50 .

[0125] The binder contained in the positive electrode active material layer, especially the PVdF-based polymer binder, tends to adhere to the lithium iron phosphate rather than the current collector at the positive electrode interface, and this phenomenon is aggravated as the specific surface area of ​​the lithium iron phosphate particles increases.

[0126] Average particle size D 50 The second lithium iron phosphate particles in the range of 3.5 μm to 15 μm have an average particle size larger than that of the first lithium iron phosphate particles, and thus have a smaller specific surface area than that of the first lithium iron phosphate particles. Therefore, the second lithium iron phosphate particles contained in the predetermined range have the effect of reducing the sum of the specific surface areas of the lithium iron phosphate particles, and within the range in which the sum of the specific surface areas of the lithium iron phosphate particles is reduced, the PVdF-based binder can adhere to the current collector instead of the lithium iron phosphate to improve the interfacial adhesion between the current collector and the positive electrode active material layer.

[0127] The average particle size D of the first lithium iron phosphate 50 The average particle size D of the second lithium iron phosphate may be 0.5 μm to 2 μm, preferably 0.55 μm to 1.8 μm, and even more preferably 0.6 μm to 1.6 μm. 50 It may be 3.5 μm to 15 μm, preferably 3.8 μm to 12 μm, and even more preferably 4 μm to 10 μm.

[0128] The weight ratio of the first lithium iron phosphate to the second lithium iron phosphate may be 80:20 to 99.9:0.1, preferably 85:15 to 99:1, and more preferably 90:1 to 95:5. When the weight ratio of the first lithium iron phosphate to the second lithium iron phosphate satisfies the above range, the adhesion is excellent. If the second lithium iron phosphate having a relatively large average particle size is excessively included, the viscosity of the positive electrode slurry may rise rapidly, and the rolling performance may deteriorate, which is not desirable.

[0129] The first lithium iron phosphate may be a primary particle, and the second lithium iron phosphate may be a primary particle or a secondary particle.

[0130] Based on the total solids of the positive electrode slurry composition, the content of the lithium iron phosphate may be 92.7 wt % to 98.4 wt %, more particularly 93.5 wt % to 98 wt %, more particularly 94 wt % to 97 wt %. When the content of the lithium iron phosphate satisfies the above range, the battery capacity of the positive electrode can be improved by ensuring sufficient positive electrode energy density.

[0131] (2) Adhesive

[0132] As the adhesive, the present invention comprises a fluorine-containing adhesive and a rubber-based adhesive, wherein the rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more.

[0133] Fluorine-containing adhesives include PVDF-based polymers containing vinylidene fluoride (VDF) as monomers. Specific examples of PVDF-based polymers include PVDF homopolymers, PVDF-HFP (poly(vinylidene fluoride-to-hexafluoropropylene)), PVDF-CTFE (poly(vinylidene fluoride-to-chlorotrifluoroethylene)), PVDF-TFE (poly(vinylidene fluoride-to-tetrafluoroethylene)), PVDF-TrFE (poly(vinylidene fluoride-to-trifluoroethylene)), etc.

[0134] The fluorine-containing binder, together with the rubber-based binder, imparts adhesion between the positive electrode active material and the conductive material, and imparts adhesion between the current collector and the positive electrode active material layer.

[0135] The weight average molecular weight (Mw) of the fluorine-containing adhesive according to the present invention can be 500,000 g / mol or more, more specifically in the range of 550,000 g / mol to 2,000,000 g / mol, more specifically in the range of 600,000 g / mol to 1,500,000 g / mol. When the weight average molecular weight of the fluorine-containing adhesive is within the above numerical range, the coating stability of the positive electrode slurry is more excellent, and the adhesion of the positive electrode is excellent. In particular, in terms of the adhesion of the positive electrode, the weight average molecular weight (Mw) of the fluorine-containing adhesive is 800,000 g / mol or more, preferably 900,000 g / mol to 1,400,000 g / mol, and even more preferably 950,000 g / mol to 1,200,000 g / mol.

[0136] The content of the fluorine-containing binder in the positive electrode active material layer may be 1.0 wt % to 4.0 wt %, preferably 1.4 wt % to 3.5 wt %, more preferably 1.6 wt % to 3.0 wt %, based on the total weight of the positive electrode active material layer.

[0137] Fluorinated binders are commonly used as electrode binders due to their excellent adhesion and chemical stability to electrolytes, but including more fluorinated binders than required can negatively affect the flexibility of the positive electrode due to its crystal structure. On the other hand, the higher the binder content, the higher the adhesion of the positive electrode, so improving the adhesion and flexibility of the positive electrode by simply adjusting the binder content has been a difficult task. In addition, the loading amount of the positive electrode active material layer is 600 mg / 25 cm 2 High-loaded cathodes tend to be less flexible than low-loaded cathodes with the same binder content but smaller loading, and thus improving adhesion and flexibility in high-loaded cathodes has become a more difficult technical challenge.

[0138] Therefore, in addition to the fluorine-containing binder, the positive electrode according to the present invention further includes a rubber-based binder, wherein the rubber-based binder includes a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more.

[0139] The first hydrogenated nitrile rubber not only improves the adhesion and flexibility of the positive electrode, but also improves the dispersibility of the positive electrode slurry, thereby suppressing the aggregation of the conductive material and the positive electrode active material. The inventor of the present invention found that when the positive electrode only includes the first hydrogenated nitrile rubber as a rubber-based binder, if the content is higher than a certain level, the adhesion and flexibility of the positive electrode can no longer be improved, but when the positive electrode includes the second hydrogenated nitrile rubber and the first hydrogenated nitrile rubber, the flexibility and adhesion of the positive electrode are significantly increased. Therefore, the positive electrode according to the present invention has both excellent flexibility and excellent adhesion, and because the flexibility is improved when the load of the positive electrode increases, it has excellent calendering performance. In addition, the improved flexibility helps to prevent the active material layer of the positive electrode from being detached when the positive electrode is physically impacted outside.

[0140] The first hydrogenated nitrile rubber (HNBR) and the second hydrogenated nitrile rubber (HNBR) respectively refer to nitrile rubber (NBR) subjected to a hydrogenation reaction so that double bonds originally contained in the nitrile rubber (NBR) are converted into single bonds.

[0141] The content of repeating units having acrylonitrile (AN) derivatives in the hydrogenated nitrile rubber may be 20 to 50 wt %, more preferably 25 to 45 wt %, most preferably 30 to 40 wt %, based on the total weight of the hydrogenated nitrile rubber.

[0142] The first hydrogenated nitrile rubber may have a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol to improve the solvent wettability and dispersibility of the lithium iron phosphate particles, thereby inhibiting the aggregation of the lithium iron phosphate particles. The weight average molecular weight (Mw) of the first hydrogenated nitrile rubber may be 10,000 g / mol to 100,000 g / mol, preferably 10,000 g / mol to 75,000 g / mol, and more preferably 10,000 g / mol to 50,000 g / mol. When the weight average molecular weight of the first hydrogenated nitrile rubber is within the above numerical range, the particle aggregation of the lithium iron phosphate can be effectively inhibited.

[0143] In addition, the first hydrogenated nitrile rubber improves the positive electrode conductive network by inhibiting the aggregation of the conductive material, and by aggregating the conductive material in a spherical rather than linear manner, the specific surface area of ​​the aggregated conductive material is minimized compared to when the conductive material is linearly aggregated. As a result, the surface area of ​​the positive electrode active material adjacent to the aggregated conductive material that cannot participate in the insertion / extraction reaction of lithium is minimized, thereby reducing the discharge resistance of the lithium secondary battery.

[0144] The weight average molecular weight (Mw) of the second hydrogenated nitrile rubber is at least 150,000 g / mol, preferably 150,000 g / mol to 1,000,000 g / mol, and more preferably 200,000 g / mol to 500,000 g / mol. When the weight average molecular weight (Mw) of the second hydrogenated nitrile rubber is within the above numerical range, the adhesion and flexibility of the positive electrode active material layer can be improved, thereby increasing the calendering density of the positive electrode, and as the calendering density increases, the positive electrode resistance can be reduced.

[0145] The first hydrogenated nitrile rubber may be contained in the positive electrode active material layer at 0.1 wt % to 0.6 wt %, preferably at 0.15 wt % to 0.55 wt %, and more preferably at 0.2 wt % to 0.5 wt %. When the content of the first hydrogenated nitrile rubber is within the above range, the dispersibility of the lithium iron phosphate can be improved, and excellent adhesion and flexibility can be achieved without increasing the total content of the binder.

[0146] The second hydrogenated nitrile rubber can be included in the positive electrode active material layer with 0.2% to 0.8% by weight, preferably with 0.3% to 0.7% by weight, and more preferably with 0.35% to 0.65% by weight. When the content of the second hydrogenated nitrile rubber is greater than 0.8% by weight, this is undesirable because it can significantly increase the viscosity of the slurry, thereby significantly reducing the mixing performance and coating performance in the slurry preparation, and when the content of the second hydrogenated nitrile rubber is less than 0.2% by weight, this is undesirable because the effect of improving the adhesion performance and flexibility of the prepared positive electrode is not significant.

[0147] The rubber-based binder may be contained in the positive electrode active material layer at 0.5 wt % to 1.5 wt %, preferably 0.6 wt % to 1.3 wt %, and most preferably 0.7 wt % to 1.2 wt %. When the content of the rubber-based binder is within the above range, excellent adhesion and flexibility can be achieved without increasing the overall binder content.

[0148] The second hydrogenated nitrile rubber may be in a range of 40 wt % or less, preferably 14 wt % to 33 wt %, and more preferably 15 wt % to 30 wt % relative to the total weight of the fluorine-containing binder and the second hydrogenated nitrile rubber. When the second hydrogenated nitrile rubber is included in the above content relative to the fluorine-containing binder, the flexibility of the positive electrode can be improved while the viscosity of the slurry can be greatly increased to prevent the coating stability from being deteriorated.

[0149] In addition, the total content of the fluorine-containing binder and the rubber-based binder in the positive electrode active material layer can be 2.0 wt % to 4.5 wt %, preferably 2.2 wt % to 4.0 wt %, and most preferably 2.5 wt % to 3.8 wt %. When the content of the binder satisfies the above range, the contact area between the binder and the lithium iron phosphate increases, thereby being able to obtain excellent positive electrode adhesion.

[0150] (3) Conductive materials

[0151] The positive electrode active material layer of the present invention may further contain a conductive material.

[0152] There is no particular limitation on the conductive material as long as it conducts electricity without causing chemical changes in the battery, and for example: graphite; carbon black materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, etc.; conductive fibers such as carbon fibers or metal fibers; fluorocarbons; metal powders such as aluminum powder, nickel powder; conductive whiskers such as zinc oxide, potassium titanate, etc.; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives, etc. Specific examples of commercially available conductive materials include: acetylene black products from Chevron Chemical Company, Denka Singapore Private Limited, or Gulf Oil Company, etc.; Ketjenback, EC series (Armak Company), Vulcan XC-72 (product of Cabot Company), and Super P (MMM). (Armak Company product), Vulcan XC-72 (Cabot Company product), and Super P (Timcal product). Preferably, the conductive material may be carbon nanotubes. A conductive network of carbon nanotubes is preferred as the conductive material contained in the positive electrode of the present invention because it can alleviate the migration phenomenon of the binder during the drying process of the positive electrode slurry.

[0153] The content of the conductive material in the positive electrode active material layer may be 0.3 wt % to 2.0 wt %, more particularly 0.6 wt % to 1.5 wt %, more particularly 0.8 wt % to 1.3 wt %. When the content of the conductive material in the positive electrode active material layer satisfies the above range, the conductivity of the positive electrode can be improved by ensuring a positive electrode conductive network.

[0154] According to one embodiment of the present invention, based on the total weight of the positive electrode active material layer, the positive electrode active material layer may include: 92.7% to 98.4% by weight of lithium iron phosphate; 1.0% to 4.0% by weight of fluorine-containing adhesive; 0.1% to 0.6% by weight of the first hydrogenated nitrile rubber; 0.2% to 0.8% by weight of the second hydrogenated nitrile rubber; and 0.3% to 2.0% by weight of conductive material. When the composition in the positive electrode active material layer meets the above range, the adhesion and conductivity of the electrode are ensured, and by increasing the active material content, the capacity and resistance performance of the lithium secondary battery can be improved, and the flexibility of the positive electrode can be significantly improved.

[0155] The positive electrode can be manufactured according to a conventional method for manufacturing a positive electrode. Specifically, the positive electrode can be manufactured by preparing a positive electrode slurry composition containing a positive electrode active material, a conductive material, a binder and / or a dispersant, applying the positive electrode slurry composition to a positive electrode current collector, and then drying and rolling.

[0156] Alternatively, the positive electrode may be prepared by casting the positive electrode slurry composition onto a separate support and then laminating a film obtained by peeling off the support onto a positive electrode current collector.

[0157] The positive electrode according to one embodiment of the present invention includes the first hydrogenated nitrile rubber and the second hydrogenated nitrile rubber, and because the lithium iron phosphate, the fluorine-containing binder, the first hydrogenated nitrile rubber and the second hydrogenated nitrile rubber are included in the above weight ratio, it is possible to ensure 550 mg / 25 cm 2 Up to 650 mg / 25 cm 2 The invention has excellent positive electrode adhesion and flexibility while having a high loading amount. As a result, a high-load positive electrode can be manufactured, the battery resistance of the secondary battery can be reduced by preventing the detachment of the positive electrode, the capacity and output characteristics of the battery can be improved, and defects in the manufacturing process can be reduced.

[0158] The positive electrode of the present invention has an adhesion force between the positive electrode collector and the positive electrode active material layer measured by a 90° peel test of at least 19 gf / 20mm, more specifically in the range of 19.5 gf / 20mm to 70 gf / 20mm, and more specifically in the range of 20 gf / 20mm to 67 gf / 20mm.

[0159] Furthermore, the positive electrode of the present invention has flexibility such that in a flexibility test in which a cross section of the positive electrode is lifted after a phi-dedicated measuring rod is contacted on the positive electrode active material layer, cracks occur with a measuring rod of 5 phi(ø) or less, more specifically 2 to 4 phi(ø).

[0160] Lithium secondary battery

[0161] Next, a lithium secondary battery according to the present invention will be described.

[0162] A lithium secondary battery according to one embodiment of the present invention may include a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.

[0163] In a lithium secondary battery, the positive electrode is as described above. For example, the positive electrode may include a positive electrode active material layer disposed on one or both sides of the current collector,

[0164] The positive electrode active material layer comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder and a conductive material, wherein

[0165] The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and

[0166] The second hydrogenated nitrile rubber is included in an amount of 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

[0167] The lithium iron phosphate, the fluorine-containing binder, the first hydrogenated nitrile rubber, the second hydrogenated nitrile rubber, and the conductive material have been described in detail previously, and thus redundant description will be omitted.

[0168] The loading amount of the positive electrode active material layer can be at least 450 mg / 25 cm 2 , more particularly 450 mg / 25 cm 2 Up to 700 mg / 25 cm 2 , more particularly 500 mg / 25 cm 2 Up to 700 mg / 25 cm 2 , more particularly 550 mg / 25 cm 2 Up to 650 mg / 25 cm 2 .

[0169] For example, the negative electrode may be prepared by preparing a negative electrode forming composition including a negative electrode active material, a negative electrode binder, and a negative electrode conductive material, and then coating the composition on a negative electrode current collector.

[0170] There is no particular limitation on the negative electrode active material, and any compound capable of reversibly inserting and deinserting lithium can generally be used. Specific examples include: carbonaceous materials such as synthetic graphite, natural graphite, graphitized carbon fiber, amorphous carbon and high crystalline carbon; (semi) metal materials such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy or Al alloy capable of forming an alloy with lithium; or a composite material comprising a (semi) metal material and a carbonaceous material. Low crystalline carbon includes soft carbon and hard carbon, and high crystalline carbon includes natural graphite, condensed graphite and pyrolytic carbon, mesophase pitch carbon fiber, mesophase carbon microspheres, mesophase pitch and high temperature calcined carbon such as coke derived from petroleum or coal tar pitch. A single one of these materials or a mixture of two or more can be used, and a metallic lithium film can also be used as a negative electrode active material.

[0171] The negative electrode material is used to impart conductivity to the electrode, and can be used without particular limitation as long as it has electronic conductivity and does not cause chemical changes in the battery to be constructed. Specific examples include: graphite such as natural or synthetic graphite; carbon materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum and silver; conductive whiskers such as zinc oxide, potassium titanate, etc.; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives, etc., one type thereof or a mixture of two or more types thereof can be used alone. The content of the negative electrode conductive material can generally be 1 to 30% by weight, more particularly 1 to 20% by weight, and more particularly 1 to 10% by weight relative to the total weight of the negative electrode active material layer.

[0172] The negative electrode binder is used to enhance the adhesion between the negative electrode active material particles and the adhesion between the negative electrode active material and the negative electrode collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinyl pyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene propylene diene rubber (EPDM rubber), sulfonated EPDM, styrene butadiene rubber (SBR), fluororubber or its various copolymers, wherein any one thereof or a mixture of two or more thereof may be used alone. Based on the total weight of the negative electrode active material layer, the content of the negative electrode binder may be 1 to 30% by weight, more particularly 1 to 20% by weight, and more particularly 1 to 10% by weight.

[0173] On the other hand, there is no particular limitation on the negative electrode collector as long as it has high conductivity and does not cause chemical changes in the battery, and for example: copper, stainless steel, aluminum, nickel, titanium, calcined carbon; and copper or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. on the surface of the copper or stainless steel; aluminum-cadmium alloy, etc. can be used.

[0174] In addition, the negative electrode current collector may generally have a thickness of 3 μm to 500 μm, and, like the positive electrode current collector, fine concavoconvexities may be formed on the surface of the negative electrode current collector to enhance the binding of the negative electrode active material. For example, it can be used in various forms such as films, sheets, foils, nets, porous materials, foams, nonwoven fabrics, etc.

[0175] On the other hand, in lithium secondary batteries, if the separator is conventionally used as a separator in lithium secondary batteries, the separator can be used without any specific restrictions, and it is particularly desirable to have low resistance to the ion migration of the electrolyte and excellent ability to impregnate the electrolyte. Specifically, it can be used: a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer; or a layered structure of more than two layers thereof. In addition, conventional porous non-woven fabrics can be used, such as non-woven fabrics made of high melting point glass fibers, polyethylene terephthalate fibers, etc. In addition, the separator can also be a porous film with a pore size of 0.01 μm to 10 μm and a thickness of 5 μm to 300 μm.

[0176] On the other hand, in a lithium secondary battery, the electrolyte may include, but is not limited to, an organic solvent and a lithium salt conventionally used in an electrolyte.

[0177] As long as the organic solvent can be used as a medium in which ions participating in the electrochemical reaction of the battery can move, the organic solvent can be used without any particular limitation. Specifically, the organic solvent includes: ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, ε-caprolactone, etc.; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; carbonate solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), propylene carbonate (PC), etc.

[0178] Among them, carbonate solvents are preferred, and more preferably a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery and a linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate or diethyl carbonate, etc.) having a low viscosity.

[0179] As long as the lithium salt is a compound that can provide lithium ions used in lithium secondary batteries, the lithium salt can be used without restriction. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI or LiB(C2O4)2. The lithium salt is preferably contained in the electrolyte at a concentration of about 0.6 mol% to 2 mol%.

[0180] In order to improve the life characteristics of the battery, inhibit the reduction of the battery capacity, improve the discharge capacity of the battery, etc., in addition to the above-mentioned electrolyte components, the electrolyte may also contain one or more additives, such as pyridine, triethyl phosphite, triethanolamine, cyclic ether, ethylenediamine, (condensed) glycol dimethyl ether, hexamethylphosphoric triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted Oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salt, pyrrole, 2-methoxyethanol or aluminum chloride. Here, the content of the additive may be 0.1 wt % to 5 wt % based on the total weight of the electrolyte.

[0181] The lithium secondary battery of the present invention can be manufactured by placing a separator between the positive electrode and the negative electrode to form an electrode assembly, placing the electrode assembly in a cylindrical battery shell or a prismatic battery shell, and then injecting an electrolyte. Alternatively, the lithium secondary battery of the present invention can be manufactured by stacking electrode assemblies, impregnating the electrode assemblies with an electrolyte, and sealing the resulting product in a battery shell.

[0182] When manufacturing the lithium secondary battery of the present invention, the electrode assembly can be dried to remove one or more organic solvents selected from the following: N-methyl-2-pyrrolidone (NMP), acetone, ethanol, propylene carbonate, ethyl methyl carbonate, ethylene carbonate and dimethyl carbonate used in the manufacture of the positive electrode. If an electrolyte having the same composition as the organic solvent used in the preparation of the positive electrode is used as the electrolyte, the process of drying the electrode assembly can be omitted.

[0183] Unlike the above-described lithium secondary battery, a lithium secondary battery according to other embodiments of the present invention may be an all-solid-state battery.

[0184] The battery case may be any one conventionally used in the art, and has no limitation on shape according to the intended use of the battery, for example, it may be a cylindrical shape using a can, a prismatic shape, a pouch type, or a coin type.

[0185] The lithium secondary battery according to the present invention stably exhibits excellent discharge capacity, output characteristics, and capacity retention rate, and thus can be used in: portable devices such as mobile phones, notebook computers, and digital cameras; energy storage systems (ESS); and electric vehicles such as hybrid electric vehicles (HEV).

[0186] Cathode slurry

[0187] According to another embodiment of the present invention, a slurry for a positive electrode is provided.

[0188] The positive electrode slurry according to the present invention comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder, a conductive material and a solvent, wherein:

[0189] The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and

[0190] The second hydrogenated nitrile rubber is included in an amount of 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

[0191] In the positive electrode slurry according to an exemplary embodiment, based on the total weight of the solids in the positive electrode slurry, the content of lithium iron phosphate can be 92.7 wt % to 98.4 wt %; the content of the fluorine-containing binder can be 1.0 wt % to 4.0 wt %; the content of the first hydrogenated nitrile rubber can be 0.1 to 0.6 wt %; the content of the second hydrogenated nitrile rubber can be 0.2 wt % to 0.8 wt %; and the content of the conductive material can be 0.3 wt % to 2.0 wt %.

[0192] The positive electrode slurry according to the present invention includes the second hydrogenated nitrile rubber having a weight average molecular weight within the above range, which significantly increases the flexibility of the high-load positive electrode, and has appropriate viscosity and excellent coating stability by controlling the contents of the fluorine-containing binder and the second hydrogenated nitrile rubber within the above range.

[0193] Since the lithium iron phosphate, the first and second hydrogenated nitrile rubbers, the fluorine-containing adhesive, and the conductive material have been previously described in detail, redundant descriptions will be omitted.

[0194] The solvent is used to mix the lithium iron phosphate, the binder, the conductive material and / or the dispersant. The solvent may be any commonly used solvent in the art, such as dimethyl sulfoxide (DMSO), isopropanol, N-methyl-2-pyrrolidone (NMP), acetone or water, any one of which may be used alone or as a mixture of two or more thereof.

[0195] The solvent may be included in an amount to provide a positive electrode slurry having an appropriate viscosity and solid content. For example, the content of the solvent may be such that the solid content in the slurry is 50% to 75% by weight, more particularly 50% to 70% by weight, and more particularly 55% to 70% by weight. This corresponds to a relatively high solid content compared to conventional positive electrode slurries containing lithium iron phosphate as positive electrode active materials. When the solid content of the positive electrode slurry composition meets the above range, the time required for the slurry drying process during positive electrode manufacturing can be reduced, thereby reducing process costs. In addition, the positive electrode slurry can have a viscosity at a level that can be coated, and the positive electrode active material layer formed by the composition can have a thickness higher than a specific level, thereby ensuring excellent energy density.

[0196] The composition viscosity of the positive electrode slurry according to one embodiment of the present invention measured at a shear rate of 2.5 / s at 25°C may be 5,000 cps to 25,000 cps, more particularly 6,000 cps to 24,000 cps, more particularly 6,500 cps to 23,000 cps. The positive electrode slurry having a viscosity value within the above range may have good storage stability and coating processability. In addition, compared with a conventional slurry of a lithium iron phosphate positive electrode having the same viscosity, the positive electrode slurry may have a high solid content, thereby reducing the time required for the slurry drying process in the manufacture of the positive electrode, thereby reducing the process cost.

[0197] The present invention will now be described in more detail by way of examples. However, the following examples are intended to illustrate the present invention and are not intended to limit the scope of the present invention.

[0198] Example 1: Preparation of positive electrode

[0199] (1) Preparation of positive electrode slurry

[0200] A dispersion was prepared, which contained carbon nanotubes (CNTs) as a conductive material and a first hydrogenated nitrile rubber (first HNBR) having a weight average molecular weight (Mw) of 30,000 g / mol as a rubber-based binder.

[0201] As lithium iron phosphate, LiFePO4 (average particle size D 50A primary particle with a diameter of 1.0 μm and a single body structure), a carbon nanotube (CNT) as a conductive material, a polyvinylidene fluoride (PVdF) with a weight average molecular weight (Mw) of 630,000 g / mol as a fluorine-containing binder, and a second hydrogenated nitrile rubber (second HNBR) with a weight average molecular weight (Mw) of 310,000 g / mol as a rubber-based binder, and the above-mentioned dispersion are introduced into an N-methylpyrrolidone (NMP) solvent, and mixed at 2500 rpm for 90 min using a homogenizer to prepare a positive electrode slurry.

[0202] In the positive electrode slurry, lithium iron phosphate, conductive material, fluorine-containing binder, first hydrogenated nitrile rubber and second hydrogenated nitrile rubber are present in a weight ratio of 95.24:1.2:2.7:0.36:0.5, and the solid content in the positive electrode slurry is 62 wt %.

[0203] (2) Preparation of positive electrode

[0204] The cathode slurry was coated on a 20 μm thick aluminum film to a concentration of 600 mg / 25 cm 2 After that, the positive electrode slurry was hot-air dried at 130° C. for 5 minutes to make the solid content of the positive electrode slurry greater than or equal to 99.0% by weight. Then, the positive electrode was prepared by rolling the dried positive electrode slurry so that the porosity of the positive electrode active material layer was 29%.

[0205] Example 2: Preparation of positive electrode

[0206] A positive electrode was prepared in the same manner as in Example 1, except that the weight ratio of the lithium iron phosphate, the conductive material, the fluorine-containing binder, the first hydrogenated nitrile rubber, and the second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1.

[0207] Example 3 to Example 6: Preparation of positive electrode

[0208] A positive electrode was prepared in the same manner as in Example 1, except that the fluorine-containing binder was replaced with polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 1,000,000 g / mol, and the weight ratio of lithium iron phosphate, conductive material, fluorine-containing binder, first hydrogenated nitrile rubber and second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1.

[0209] Example 7 to Example 10: Preparation of positive electrode

[0210] A positive electrode was prepared in the same manner as in Example 1, except that the fluorine-containing binder was changed to polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 1,000,000 g / mol, the second hydrogenated nitrile rubber was changed to a hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 220,000 g / mol, and the weight ratio of lithium iron phosphate, conductive material, fluorine-containing binder, first hydrogenated nitrile rubber and second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1 (however, the solid content of the positive electrode slurry in Example 9 was also changed).

[0211] Example 11: Preparation of positive electrode

[0212] A positive electrode was prepared in the same manner as in Example 1, except that the fluorine-containing binder was replaced with polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 1,000,000 g / mol, and the weight ratio of lithium iron phosphate, conductive material, fluorine-containing binder, first hydrogenated nitrile rubber and second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1.

[0213] Comparative Example 1: Preparation of positive electrode

[0214] (1) Preparation of positive electrode slurry

[0215] A dispersion was prepared, which contained carbon nanotubes (CNTs) as a conductive material and a first hydrogenated nitrile rubber (first HNBR) having a weight average molecular weight (Mw) of 30,000 g / mol as a rubber-based binder.

[0216] As lithium iron phosphate, LiFePO4 (average particle size D 50 A primary particle with a diameter of 1.0 μm and a single body structure), polyvinylidene fluoride (PVdF) with a weight average molecular weight (Mw) of 630,000 g / mol as a fluorine-containing binder, a first hydrogenated nitrile rubber (first HNBR) with a weight average molecular weight (Mw) of 30,000 g / mol as a rubber-based binder, and the above-mentioned dispersion are introduced into an N-methylpyrrolidone (NMP) solvent and mixed at 2500 rpm for 90 min using a homogenizer to prepare a positive electrode slurry.

[0217] In the positive electrode slurry, the lithium iron phosphate, the conductive material, the fluorine-containing binder and the first hydrogenated nitrile rubber are present in a weight ratio of 95.24:1.2:2.7:0.86, and the solid content in the positive electrode slurry is 62 wt %.

[0218] (2) Preparation of positive electrode

[0219] The cathode slurry was coated on a 20 μm thick aluminum film to a concentration of 600 mg / 25 cm 2After that, the positive electrode slurry was hot-air dried at 130° C. for 5 minutes so that the solid content of the positive electrode slurry was 99.0 wt % or more. Then, the positive electrode was prepared by rolling the dried positive electrode slurry so that the porosity of the positive electrode active material layer was 29%.

[0220] Comparative Example 2: Preparation of positive electrode

[0221] (1) Preparation of positive electrode slurry

[0222] A dispersion was prepared, which contained carbon nanotubes (CNTs) as a conductive material and a first hydrogenated nitrile rubber (first HNBR) having a weight average molecular weight (Mw) of 30,000 g / mol as a rubber-based binder.

[0223] As lithium iron phosphate, LiFePO4 (average particle size D 50 0 μm and having a single body structure), a second hydrogenated nitrile rubber (second HNBR) having a weight average molecular weight (Mw) of 310,000 g / mol as a rubber-based binder, and the above-mentioned dispersion were introduced into an N-methylpyrrolidone (NMP) solvent, and then mixed at 2500 rpm for 90 min by using a homogenizer to prepare a positive electrode slurry.

[0224] In the positive electrode slurry, lithium iron phosphate, the conductive material, the first hydrogenated nitrile rubber, and the second hydrogenated nitrile rubber are present in a weight ratio of 97.44:1.2:0.36:1.0, and the solid content in the positive electrode slurry is 64 wt %.

[0225] (2) Preparation of positive electrode

[0226] The cathode slurry was coated on a 20 μm thick aluminum film to a concentration of 600 mg / 25 cm 2 After that, the positive electrode slurry was hot-air dried at 130° C. for 5 minutes so that the solid content of the positive electrode slurry was 99.0 wt % or more. Then, the positive electrode was prepared by rolling the dried positive electrode slurry so that the porosity of the positive electrode active material layer was 29%.

[0227] Comparative Example 3 to Comparative Example 4: Preparation of Positive Electrode

[0228] A positive electrode was prepared in the same manner as in Example 1, except that the weight ratio of the lithium iron phosphate, the conductive material, the fluorine-containing binder, the first hydrogenated nitrile rubber, and the second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1.

[0229] Comparative Example 5: Preparation of positive electrode

[0230] A positive electrode was prepared in the same manner as in Comparative Example 1, except that the weight ratios of the lithium iron phosphate, the conductive material, the fluorine-containing binder, and the first hydrogenated nitrile rubber in the positive electrode slurry were changed as shown in Table 1.

[0231] Comparative Examples 6 to 8: Preparation of Positive Electrode

[0232] A positive electrode was prepared in the same manner as in Example 1, except that the fluorine-containing binder was replaced by polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 1,000,000 g / mol, the second hydrogenated nitrile rubber was replaced by a hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 220,000 g / mol, and the weight ratio of lithium iron phosphate, conductive material, fluorine-containing binder, first hydrogenated nitrile rubber and second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1.

[0233] Comparative Example 9: Preparation of positive electrode

[0234] A positive electrode was prepared in the same manner as in Comparative Example 1, except that the fluorine-containing binder was changed to polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 530,000 g / mol.

[0235] Comparative Example 10: Preparation of positive electrode

[0236] A positive electrode was prepared in the same manner as in Example 1, except that the fluorine-containing binder was replaced with polyvinylidene fluoride (PVdF) having a weight average molecular weight (Mw) of 1,000,000 g / mol, and the weight ratio of lithium iron phosphate, conductive material, fluorine-containing binder, first hydrogenated nitrile rubber and second hydrogenated nitrile rubber in the positive electrode slurry was changed as shown in Table 1.

[0237] Experimental Example 1: Measuring the viscosity of positive electrode slurry

[0238] The viscosity of the positive electrode slurry prepared in each of Examples 1-11 and Comparative Examples 1-10 was measured, and the results are shown in Table 2.

[0239] Specifically, the positive electrode slurry prepared in each of Examples 1-11 and Comparative Examples 1-10 was cooled at room temperature and 1% relative humidity for 1 hour, and then the viscosity of the positive electrode slurry composition was measured using a viscometer (Brookfield) at a shear rate of 2.5 / s at 25° C. The viscosity measurement was performed within 2 hours after the positive electrode slurry composition was prepared, including the cooling time.

[0240] Experimental Example 2: Testing the Adhesion of the Positive Electrode

[0241] After the positive electrodes prepared in each of Examples 1-11 and Comparative Examples 1-10 were vacuum dried at 130° C. for 2 hours, the adhesion between the positive electrode active material layer and the positive electrode current collector was measured. The results are shown in Table 2.

[0242] Specifically, the positive electrode prepared in each of Examples 1-11 and Comparative Examples 1-10 was cut into a length of 150 mm and a width of 20 mm, and the surface of the positive electrode was pasted on a slide glass having a length of 75 mm and a width of 25 mm in the longitudinal direction using a double-sided tape. That is, the slide glass was pasted to an area corresponding to half of the positive electrode in the longitudinal direction. Then, the evaluation sample was prepared by rubbing the roller 10 times to ensure that the double-sided tape was evenly applied.

[0243] Next, the slide glass portion of the evaluation sample was fixed to the sample stage of the universal testing machine (UTM) (product name: LS5, manufacturer: LLOYD), and the half of the positive electrode that was not attached to the slide glass was connected to the load sensor of the UTM machine. The load sensor was moved to 50 mm at a speed of 100 mm / min using a 90° force, and the load applied to the load sensor was measured. Then, the load applied to the load sensor was averaged in the 20 mm to 40 mm portion of the stroke, and repeated 5 times to evaluate the average value as the positive electrode adhesion force (gf / 20 mm) of each sample.

[0244] Experimental Example 3: Testing the flexibility of the positive electrode

[0245] The positive electrodes prepared in each of Examples 1-11 and Comparative Examples 1-10 were vacuum dried at a temperature of 130° C. for 2 hours, and their flexibility was measured. The results are shown in Table 2.

[0246] Specifically, each positive electrode prepared in Example 1-11 and Comparative Example 1-10 was cut into a length of 10 cm and a width of 30 cm, and a measuring rod with a diameter of 2.5 ø, 3 ø, 4 ø, 5 ø, 6 ø, 7 ø, 8 ø, 9 ø, and 10 ø was prepared, and the positive electrode collector side of each cut positive electrode was facing the measuring rod, and each cut positive electrode was bent in half, and the two ends of the positive electrode were lifted at a speed of 10 mm / min. It was lifted until the force measured by UTM was 5 N. It was measured by each phi, and the electrode was observed by an optical microscope to see if there was a crack. If there was no crack, a smaller phi was used for the test. Accordingly, the diameter (ø) of the measuring rod with cracks is shown in Table 2.

[0247]

[0248]

[0249] Referring to Tables 1 and 2, it is found that the positive electrode slurries according to Examples 1 to 11 all have a relatively high solid content of 62 wt %, but the viscosity of the slurry is in the range of 6,500 cps to 12,500 cps, except for the positive electrode slurry of Example 3, which has a viscosity that is very suitable for coating on the positive electrode collector, and the lithium iron phosphate and the conductive material are not linearly aggregated.

[0250] Furthermore, it was found that the positive electrodes according to Examples 1 to 11 had an adhesion of 20 gf / 20 mm or more while having excellent flexibility of 4 Å or less. Therefore, it is expected that the detachment of the positive electrode active material layer during the production of the positive electrode will be reduced.

[0251] The positive electrodes not including the second hydrogenated nitrile rubber according to Comparative Examples 1, 5, 7, and 9 had flexibility exceeding 10 during the flexibility evaluation, indicating poor flexibility compared to the positive electrode according to any one of Examples 1 to 11.

[0252] The positive electrode according to Comparative Example 2 was found to have the worst adhesion because no fluorine-containing binder was contained, and was also found to have the worst flexibility compared with the positive electrode of the example although it contained the second hydrogenated nitrile rubber.

[0253] It is found that compared with the positive pole of Examples 1 to 11, the positive pole according to Comparative Example 3, Comparative Example 4 and Comparative Example 6 has too high viscosity of positive electrode slurry due to relatively more second hydrogenated nitrile rubber and relatively less fluorine-containing adhesive, resulting in poor coating stability and being difficult to be applied to batch production. It is also found that, compared with the positive pole of the embodiment, these positive poles have lower adhesion. From these results, it can be seen that in terms of the viscosity characteristics of the positive electrode slurry and the adhesion of the positive pole, it is desirable to control the weight ratio of the second hydrogenated nitrile rubber relative to the fluorine-containing adhesive and the second hydrogenated nitrile rubber gross weight within a suitable range, more specifically, it is desirable to control the weight ratio to less than 40%, more specifically less than 33%.

[0254] Since the positive electrode according to Comparative Example 10 did not contain the first hydrogenated nitrile rubber, the lithium iron phosphate and the conductive material were not dispersed and the viscosity was too high to be measured, and thus, the positive electrode slurry could not be coated on the current collector, thereby failing to manufacture the positive electrode.

[0255] Experimental Example 4: Measuring positive electrode resistance

[0256] The resistance values ​​of the positive electrodes prepared in Examples 1-4 were measured and compared.

[0257] Specifically, the positive electrode prepared in each of Examples 1 to 4 was used to measure the multi-probe electrode resistance.

[0258] The resistance was set as the positive electrode active layer resistance and the interface contact resistance between the positive electrode active layer and the current collector, and was calculated as the potential difference measured between the respective probes.

[0259] The measurement conditions are as follows

[0260] - Current: 100 μA

[0261] - Speed: Slow

[0262] - Voltage range: 0.5 V

[0263] - Current collector resistivity value: Al used above 2.82E-06Ω-cm

[0264] The results are shown in Table 3 below.

[0265]

[0266] Referring to Tables 1 to 3 at the same time, it is shown that the positive electrode according to Example 4, although containing less binder than the positive electrode according to Example 2, still has better adhesion than the positive electrode according to Example 2, and also has better resistance performance than the positive electrode according to Example 2 due to the reduced binder content.

[0267] It was found that the positive electrode according to Example 3 had better adhesion than the positive electrode according to Example 1 despite containing less binder than the positive electrode according to Example 1, and had better resistance performance than the positive electrode according to Example 1 due to the reduced binder content.

[0268] Therefore, in the present invention, it is analyzed that the weight average molecular weight of the fluorine-containing binder is preferably 800,000 g / mol or more in terms of adhesion and electrical properties.

Claims

1. A positive electrode having a positive electrode active material layer disposed on one or both sides of a current collector, wherein The positive electrode active material layer comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder and a conductive material, wherein The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and The content of the second hydrogenated nitrile rubber is 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

2. The positive electrode according to claim 1, wherein The positive electrode active material layer has a 2 Up to 700 mg / 25 cm 2 load within the range.

3. The positive electrode according to claim 1, wherein The second hydrogenated nitrile rubber has a weight average molecular weight (Mw) of 150,000 g / mol to 1,000,000 g / mol.

4. The positive electrode according to claim 1, wherein The first hydrogenated nitrile rubber may be present in an amount of 0.1 wt % to 0.6 wt % based on the total weight of the positive electrode active material layer.

5. The positive electrode according to claim 1, wherein The lithium iron phosphate may be present in an amount of 92.7 wt % to 98.4 wt % based on the total weight of the positive electrode active material layer.

6. The positive electrode according to claim 1, wherein The content of the fluorine-containing binder in the positive electrode active material layer is 1.0 wt % to 4.0 wt %.

7. The positive electrode according to claim 1, wherein The content of the rubber-based binder in the positive electrode active material layer is 0.5 wt % to 1.5 wt %.

8. The positive electrode according to claim 1, wherein The content of the second hydrogenated nitrile rubber in the positive electrode active material layer is 0.3 wt % to 0.7 wt %.

9. The positive electrode according to claim 1, wherein The second hydrogenated nitrile rubber is 33 wt % or less based on the total weight of the fluorine-containing adhesive and the second hydrogenated nitrile rubber.

10. The positive electrode according to claim 1, wherein The lithium iron phosphate is a compound represented by the following chemical formula 1: [Chemical formula 1] Li 1+a Fe 1-x M x (PO 4-b )X b (In Chemical Formula 1, M comprises one or more elements selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn and Y, X contains one or more elements selected from F, S and N, and a, b and x are -0.5≤a≤0.5, 0≤b≤0.1 and 0≤x≤0.5 respectively).

11. The positive electrode according to claim 1, wherein The positive electrode adhesion measured in an adhesion test in which the positive electrode active layer is peeled off from an aluminum film at 90° is greater than or equal to 19 gf / 20 mm.

12. The positive electrode according to claim 1, wherein In a flexibility test in which a phi-dedicated measuring rod was brought into contact on the positive electrode active material layer and the cross section of the positive electrode was lifted, cracks occurred in the case of a measuring rod of 5 phi (ø) or less.

13. The positive electrode according to claim 1, wherein The fluorine-containing binder has a weight average molecular weight (Mw) of 800,000 g / mol or more.

14. The positive electrode according to claim 1, wherein The conductive material is carbon nanotube.

15. The positive electrode according to claim 12, wherein The conductive material may be contained in an amount of 0.3 wt % to 2.0 wt % based on the total weight of the positive electrode active material layer.

16. The positive electrode according to claim 1, wherein The total weight of the binder contained in the positive electrode active material layer is 2.0 wt % to 4.5 wt % based on the total weight of the positive electrode active material.

17. The positive electrode according to claim 1, wherein The lithium iron phosphate has an average particle size D of 0.3 μm to 20.0 μm. 50 .

18. The positive electrode according to claim 1, wherein The lithium iron phosphate has a single body structure consisting of primary particles.

19. A lithium secondary battery, comprising: a positive electrode, a negative electrode, a separator and an electrolyte, wherein The positive electrode has a positive electrode active material layer disposed on one side or both sides of the current collector, wherein the positive electrode active material layer comprises lithium iron phosphate, a fluorine-containing binder, a rubber-based binder and a conductive material, wherein the rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and The content of the second hydrogenated nitrile rubber is 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

20. A positive electrode slurry, comprising lithium iron phosphate, a fluorine-containing binder, a rubber-based binder, a conductive material and a solvent, wherein The rubber-based adhesive comprises a first hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 10,000 g / mol to 100,000 g / mol and a second hydrogenated nitrile rubber having a weight average molecular weight (Mw) of 150,000 g / mol or more, and The content of the second hydrogenated nitrile rubber is 0.2 wt % to 0.8 wt % based on the total weight of the positive electrode active material layer.

21. The positive electrode slurry according to claim 20, wherein The second hydrogenated nitrile rubber has a weight average molecular weight (Mw) of 150,000 g / mol to 1,000,000 g / mol.

22. The positive electrode slurry according to claim 20, wherein The fluorine-containing binder has a weight average molecular weight (Mw) of 800,000 g / mol or more.

23. The positive electrode slurry according to claim 20, wherein The solid content of the positive electrode slurry is in a range of 50 wt % to 75 wt %.

24. The positive electrode slurry according to claim 20, wherein The positive electrode slurry has a viscosity of 5,000 cps to 25,000 cps measured at 25° C. and a shear rate of 2.5 / s.

25. The positive electrode slurry according to claim 20, wherein The content of the fluorine-containing binder is 1.0 wt % to 4.0 wt % based on the total weight of the solid matter in the positive electrode slurry.

26. The positive electrode slurry according to claim 20, wherein Based on the total weight of the solid matter in the positive electrode slurry, the content of the lithium iron phosphate is 92.7 wt % to 98.4 wt %, and the content of the first hydrogenated nitrile rubber is 0.1 wt % to 0.6 wt %.

27. The positive electrode slurry according to claim 20, wherein The second hydrogenated nitrile rubber is 33 wt % or less based on the total weight of the fluorine-containing adhesive and the second hydrogenated nitrile rubber.

28. The positive electrode slurry according to claim 20, wherein The rubber-based binder may be contained in an amount of 0.5 wt % to 1.5 wt % based on the total weight of solid matter in the positive electrode slurry.

29. The positive electrode slurry according to claim 20, wherein The lithium iron phosphate is a compound represented by the following chemical formula 1: [Chemical formula 1] Li 1+a Fe 1-x M x (PO 4-b )X b (In Chemical Formula 1, M comprises one or more elements selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn and Y, X contains one or more elements selected from F, S and N, and a, b and x are -0.5≤a≤0.5, 0≤b≤0.1 and 0≤x≤0.5 respectively).

30. The positive electrode slurry according to claim 20, wherein The conductive material is carbon nanotube.

31. The positive electrode slurry according to claim 30, wherein The content of the conductive material is 0.3 wt % to 2.0 wt % based on the total weight of the solid matter in the positive electrode slurry.

32. The positive electrode slurry according to claim 20, wherein The total weight of the fluorine-containing binder and the rubber-based binder is 2.0 wt % to 4.5 wt % based on the total weight of the solid matter in the positive electrode slurry.