Hyaluronic acid grafted nano titanium dioxide sun-screening agent and application thereof
By forming a hyaluronic acid graft structure on nanotitanium dioxide, the problem of agglomeration in sunscreen is solved, the sun protection effect is significantly improved, and better sun protection performance is provided for cosmetics.
Patent Information
- Application Number
- CN202411111061.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-19
AI Technical Summary
Nanotitanium dioxide is prone to agglomeration in sunscreen, resulting in poor sunscreen effects.
The reaction of KH550 with nanotitanium dioxide forms a titanium oxide chemical bond and condenses with hyaluronic acid through amide chemical bond to form hyaluronic acid graft-modified nanotitanium dioxide to prevent agglomeration.
It significantly improves the sunscreen effect and provides better application prospects in the cosmetics field.
Smart Images

Figure CN118975951A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sunscreen creams, and in particular to a hyaluronic acid-grafted nano titanium dioxide sunscreen and applications thereof. Background Art
[0002] Ultraviolet light is an electromagnetic ray with a shorter wavelength than visible light. Ultraviolet radiation is one of the main adverse effects of sunlight on human health. Excessive or long-term exposure can cause sunburn, skin aging, and various skin diseases. According to the principle of sun protection, sunscreens are generally divided into physical sunscreens and chemical sunscreens. Chemical sunscreens have a better skin feel, but they are harmful to sensitive skin or use. Physical sunscreens reflect ultraviolet light through nanoparticles, such as titanium dioxide, zinc oxide, etc. For this reason, scientific researchers have been committed to developing safe, stable, and high-sun protection factor sunscreens.
[0003] Nano titanium dioxide is in the form of fine particles with a particle size of less than 100nm and a white loose powder appearance. Titanium dioxide has a high refractive index and semiconductor properties, and has excellent ultraviolet scattering and absorption properties. It is widely used in the fields of cosmetics, polymers and building materials protection. Although nano titanium dioxide has many advantages and can be used as a sunscreen additive in cosmetics, nanoparticles have high polarity, small particle size, and are easy to agglomerate. Therefore, when nano titanium dioxide is directly used as a sunscreen in sunscreen, the sunscreen obtained is not effective.
[0004] Organic polymer surface modification is the most commonly used method to improve the dispersibility of nanopowders. The principle is to form a layer of organic polymer on the surface of the particles through chemical adsorption or chemical reaction, and to prevent the aggregation of nanoparticles by utilizing the steric hindrance of organic matter and the extension of organic long molecular chains. For example, Chinese invention patent CN103110535A discloses a TiO 2 -HA core-shell structure sunscreen particles, preparation method and application thereof, wherein the prepared sunscreen particles have an inner core inorganic TiO2 particle and an outer layer natural HA polymer connected by electrostatic action, and the outer layer polymer HA undergoes a cross-linking reaction in the presence of a cross-linking agent, and the formed network gel stable structure is wrapped around the outside of the TiO2 particle. The structure of the sunscreen can effectively prevent the aggregation of nano titanium dioxide particles, but if it is simply adsorbed and coated on the surface of the hydrophilic inorganic particle, the chemical interaction between the inorganic phase and the polymer phase is very weak, and when the pH value and ionic strength of the system change, the polymer shell will be desorbed from the surface of the inorganic particle, resulting in the separation of the polymer and the inorganic particle. Summary of the invention
[0005] The problem in the prior art is that nano titanium dioxide is directly used as a sunscreen in sunscreen, and the nano titanium dioxide is easy to agglomerate, and the sunscreen obtained has poor sunscreen effect. In view of the above problems, the present invention provides a hyaluronic acid grafted nano titanium dioxide sunscreen, and the preparation method thereof comprises the following steps:
[0006] (1) KH550 reacts with nano-titanium dioxide in anhydrous ethanol, and the silicon-oxygen chemical bonds in KH550 condense with the hydroxyl chemical bonds on the surface of nano-silicon dioxide to form titanium-oxygen-silicon chemical bonds. After the reaction is completed, KH550-modified nano-titanium dioxide is obtained;
[0007] (2) Using N, N-diisopropylethylamine as a catalyst and HATU as a condensation agent, the terminal amino chemical bonds in KH550-modified nano-titanium dioxide and the carboxyl chemical bonds in hyaluronic acid undergo a condensation chemical reaction to form amide chemical bonds, thereby obtaining hyaluronic acid-grafted modified nano-titanium dioxide.
[0008] Preferably, step (1) comprises the following steps:
[0009] (1) Dispersing 5-15 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1-2 h to obtain a nano-titanium dioxide dispersion;
[0010] (2) Add 1-5 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6-10 hours, then cool to room temperature. Centrifuge, wash, and freeze-dry the reaction solution to obtain KH550-modified nano-titanium dioxide.
[0011] Preferably, step (2) comprises the following steps:
[0012] (1) Dissolve 0.2 g-0.8 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 1-5 g of N,N-diisopropylethylamine and 2-10 g of HATU, stir and react at room temperature for 12-20 hours to obtain a hyaluronic acid solution;
[0013] (2) 5-15 g of KH550 modified nano-titanium dioxide is re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (1) is added and stirred to mix evenly, and the pH of the solution is adjusted to 5.8. The reaction is stirred at room temperature for 12-20 hours, and then the reaction solution is centrifuged, washed, and freeze-dried to obtain hyaluronic acid grafted modified nano-titanium dioxide, which is recorded as TiO2-g-HA.
[0014] Preferably, the nano titanium dioxide is rutile nano titanium dioxide with a purity of ≥99.0% and an average particle size of 20 nm.
[0015] A sunscreen cream adopts the hyaluronic acid grafted nano titanium dioxide sunscreen agent obtained by the invention as a sunscreen additive.
[0016] Preferably, the sunscreen comprises the following ingredients by weight:
[0017] C12-C15 Alkyl Benzoate 15%
[0018] Cetearyl Alcohol 2%
[0019] Sodium Stearoyl Glutamate 1%
[0020] Polyglyceryl-4 Isostearate 0.5%
[0021] Propyl Octyl Heptyl 12%
[0022] Disodium EDTA 0.05%
[0023] Deionized water 46%
[0024] Xanthan gum 0.5%
[0025] TiO2-g-HA5-15%
[0026] Fragrance 0.05%.
[0027] The present invention has the following beneficial effects:
[0028] Compared with nano-titanium dioxide modified with hyaluronic acid by other means, the TiO2-g-HA obtained by the present invention has a better sun protection effect and has a better application prospect in the field of cosmetics. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 : is the TEM image of TiO2-g-HA obtained in Example 1.
[0030] Figure 2 : is the SEM image of TiO2-g-HA obtained in Example 1. DETAILED DESCRIPTION
[0031] The present invention is described in detail below with reference to the examples. However, it should be understood that the following examples are only illustrative of the embodiments of the present invention, and are not intended to limit the scope of the present invention.
[0032] The nano titanium dioxide used in the following examples of the present invention is rutile nano titanium dioxide, with a purity of ≥99.0% and an average particle size of 20 nm. The flavor used in the following examples of the present invention is phenylethanol, purchased from Shanghai Exceptin Flavor Co., Ltd. The pH regulator used in the following examples of the present invention is dilute hydrochloric acid, with a concentration of 0.2 mol / L.
[0033] Example 1
[0034] A hyaluronic acid-grafted nano-titanium dioxide sunscreen, the preparation method of which is as follows:
[0035] (1) Dispersing 10 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1 h to obtain a nano-titanium dioxide dispersion;
[0036] (2) adding 1 mL of KH550 to the above nano-titanium dioxide dispersion, stirring and reacting at 80° C. for 6 h, then cooling to room temperature, centrifuging, washing, and freeze-drying the reaction solution to obtain KH550-modified nano-titanium dioxide;
[0037] (3) Dissolve 0.6 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 1 g of N,N-diisopropylethylamine and 2 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0038] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0039] A sunscreen cream, comprising the following ingredients by weight:
[0040] C12-C15 Alkyl Benzoate 15%
[0041] Cetearyl Alcohol 2%
[0042] Sodium Stearoyl Glutamate 1%
[0043] Polyglyceryl-4 Isostearate 0.5%
[0044] Propyl Octyl Heptyl 12%
[0045] Disodium EDTA 0.05%
[0046] Deionized water 46%
[0047] Xanthan gum 0.5%
[0048] TiO2-g-HA 5%
[0049] Fragrance 0.05%.
[0050] According to the above formula, the raw materials are mixed and stirred evenly to obtain the sunscreen.
[0051] Example 2 is the same as Example 1, except that in Example 2, the addition amount of TiO2-g-HA is 10%.
[0052] Example 3 is the same as Example 1, except that in Example 3, the addition amount of TiO2-g-HA is 15%.
[0053] Example 4 is the same as Example 2, except that in Example 4, the preparation method of TiO2-g-HA is as follows:
[0054] (1) Dispersing 10 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1 h to obtain a nano-titanium dioxide dispersion;
[0055] (2) Add 2 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6 h, then cool to room temperature. The reaction solution is centrifuged, washed, and freeze-dried to obtain KH550-modified nano-titanium dioxide;
[0056] (3) Dissolve 0.6 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 2 g of N,N-diisopropylethylamine and 4 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0057] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0058] Example 5 is the same as Example 2, except that in Example 5, the preparation method of TiO2-g-HA is as follows:
[0059] (1) Dispersing 10 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1 h to obtain a nano-titanium dioxide dispersion;
[0060] (2) Add 5 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6 h, then cool to room temperature. Centrifuge, wash, and freeze-dry the reaction solution to obtain KH550-modified nano-titanium dioxide;
[0061] (3) Dissolve 0.6 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 5 g of N,N-diisopropylethylamine and 10 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0062] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0063] Example 6 is the same as Example 2, except that in Example 6, the preparation method of TiO2-g-HA is as follows:
[0064] (1) Dispersing 10 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1 h to obtain a nano-titanium dioxide dispersion;
[0065] (2) Add 2 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6 h, then cool to room temperature. The reaction solution is centrifuged, washed, and freeze-dried to obtain KH550-modified nano-titanium dioxide;
[0066] (3) Dissolve 0.2 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 2 g of N,N-diisopropylethylamine and 4 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0067] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0068] Example 7 is the same as Example 2, except that in Example 7, the preparation method of TiO2-g-HA is as follows:
[0069] (1) Dispersing 10 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1 h to obtain a nano-titanium dioxide dispersion;
[0070] (2) Add 2 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6 h, then cool to room temperature. The reaction solution is centrifuged, washed, and freeze-dried to obtain KH550-modified nano-titanium dioxide;
[0071] (3) Dissolve 0.8 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 2 g of N,N-diisopropylethylamine and 4 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0072] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0073] Example 8 is the same as Example 2, except that in Example 8, the preparation method of TiO2-g-HA is as follows:
[0074] (1) Disperse 5 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicate for 1 h to obtain a nano-titanium dioxide dispersion;
[0075] (2) Add 2 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6 h, then cool to room temperature. The reaction solution is centrifuged, washed, and freeze-dried to obtain KH550-modified nano-titanium dioxide;
[0076] (3) Dissolve 0.6 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 2 g of N,N-diisopropylethylamine and 4 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0077] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0078] Example 9 is the same as Example 2, except that in Example 9, the preparation method of TiO2-g-HA is as follows:
[0079] (1) Dispersing 15 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1 h to obtain a nano-titanium dioxide dispersion;
[0080] (2) Add 2 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6 h, then cool to room temperature. The reaction solution is centrifuged, washed, and freeze-dried to obtain KH550-modified nano-titanium dioxide;
[0081] (3) Dissolve 0.6 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 2 g of N,N-diisopropylethylamine and 4 g of HATU, stir and react at room temperature for 12 h to obtain a hyaluronic acid solution;
[0082] (4) 10 g of KH550 modified nano-titanium dioxide was re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (3) was added and stirred to mix evenly, and the pH of the solution was adjusted to 5.8. The reaction was stirred at room temperature for 12 h, and then the reaction solution was centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
[0083] Comparative Example 1
[0084] A sunscreen cream, comprising the following ingredients by weight:
[0085] C12-C15 Alkyl Benzoate 15%
[0086] Cetearyl Alcohol 2%
[0087] Sodium Stearoyl Glutamate 1%
[0088] Polyglyceryl-4 Isostearate 0.5%
[0089] Propyl Octyl Heptyl 12%
[0090] Disodium EDTA 0.05%
[0091] Deionized water 46%
[0092] Xanthan gum 0.5%
[0093] Hyaluronic acid 10%
[0094] Fragrance 0.05%.
[0095] Comparative Example 2
[0096] A sunscreen cream, comprising the following ingredients by weight:
[0097] C12-C15 Alkyl Benzoate 15%
[0098] Cetearyl Alcohol 2%
[0099] Sodium Stearoyl Glutamate 1%
[0100] Polyglyceryl-4 Isostearate 0.5%
[0101] Propyl Octyl Heptyl 12%
[0102] Disodium EDTA 0.05%
[0103] Deionized water 46%
[0104] Xanthan gum 0.5%
[0105] Additives 10%
[0106] Fragrance 0.05%.
[0107] The additive is a mixture of nano titanium dioxide and hyaluronic acid in a mass ratio of 10:0.6.
[0108] Comparative Example 3
[0109] A sunscreen cream, comprising the following ingredients by weight:
[0110] C12-C15 Alkyl Benzoate 15%
[0111] Cetearyl Alcohol 2%
[0112] Sodium Stearoyl Glutamate 1%
[0113] Polyglyceryl-4 Isostearate 0.5%
[0114] Propyl Octyl Heptyl 12%
[0115] Disodium EDTA 0.05%
[0116] Deionized water 46%
[0117] Xanthan gum 0.5%
[0118] KH550 modified nano titanium dioxide 10%
[0119] Fragrance 0.05%.
[0120] The KH550 modified nano titanium dioxide is the same as that in Example 1.
[0121] Comparative Example 4 is the same as Example 2, except that the pH of the solution in step (4) in Comparative Example 4 is 4.
[0122] Comparative Example 5 is the same as Example 2, except that the pH of the solution in step (4) in Comparative Example 5 is 8.
[0123] Comparative Example 6 is the same as Example 2, except that Comparative Example 6 uses the TiO2-HA gel core-shell structure particles prepared by the method of Example 1 in Chinese invention patent CN103110535A to replace the TiO2-g-HA in Example 2, the amount of TiO2-HA gel core-shell structure particles is the same as that of TiO2-g-HA, and the amount of cross-linking agent added in the preparation process of TiO2-HA gel core-shell structure particles is 2 mL.
[0124] Performance Testing
[0125] The sunscreens obtained in Examples 1-9 of the present invention and Comparative Examples 1-6 were respectively subjected to UV-visible light transmittance tests, and the transmittance test results are shown in Table 1.
[0126] UV-visible light transmittance test: Use an analytical balance to accurately weigh the mass of the object to be tested and accurately prepare a test solution with a concentration of 50ppm. Use a quartz cuvette to test the liquid UV curve of the complex with a scanning range of 290-450nm and a scanning interval of 0.1nm.
[0127] Table 1
[0128]
[0129] The sunscreen effects of the sunscreens obtained in Examples 1-9 of the present invention and Comparative Examples 1-6 were tested, and the test results are shown in Table 2.
[0130] SPF value: Accurately weigh 32.5 mg of sunscreen and apply it on a clean PMMA plate. Use pre-impregnated latex finger cots to quickly and evenly apply the sample to the entire sample sheet. Immediately place it in a dark room temperature environment. After standing for 15 minutes, test its sun protection performance.
[0131] Table 2
[0132] Test items SPF value Example 1 20.7 Example 2 25.4 Example 3 28.6 Example 4 20.3 Example 5 20.5 Example 6 18.7 Example 7 18.5 Example 8 23 Example 9 24 Comparative Example 1 4 Comparative Example 2 10 Comparative Example 3 15 Comparative Example 4 14 Comparative Example 5 18 Comparative Example 6 8
[0133] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.
Claims
1. A hyaluronic acid-grafted nano-titanium dioxide sunscreen, characterized in that: The preparation method comprises the following steps: (1) KH550 reacts with nano-titanium dioxide in anhydrous ethanol, and the silicon-oxygen chemical bonds in KH550 condense with the hydroxyl chemical bonds on the surface of nano-titanium dioxide to form Ti-O-Si chemical bonds. After the reaction is completed, KH550-modified nano-titanium dioxide is obtained; (2) Using N, N-diisopropylethylamine as a catalyst and HATU as a condensation agent, the terminal amino chemical bonds in KH550-modified nano-titanium dioxide and the carboxyl chemical bonds in hyaluronic acid undergo a condensation chemical reaction to form an amide bond, thereby obtaining TiO2-g-HA.
2. The hyaluronic acid-grafted nano-titanium dioxide sunscreen according to claim 1, characterized in that: Step (1) comprises the following steps: (1) Dispersing 5-15 g of nano-titanium dioxide in 500 mL of anhydrous ethanol and ultrasonicating for 1-2 h to obtain a nano-titanium dioxide dispersion; (2) Add 1-5 mL of KH550 to the above nano-titanium dioxide dispersion, stir and react at 80° C. for 6-10 hours, then cool to room temperature. Centrifuge, wash, and freeze-dry the reaction solution to obtain KH550-modified nano-titanium dioxide.
3. The hyaluronic acid-grafted nano-titanium dioxide sunscreen according to claim 1, characterized in that: Step (2) comprises the following steps: (1) Dissolve 0.2 g-0.8 g of hyaluronic acid in 100 mL of deionized water, stir to dissolve, add 1-5 g of N,N-diisopropylethylamine and 2-10 g of HATU, stir and react at room temperature for 12-20 hours to obtain a hyaluronic acid solution; (2) 5-15 g of KH550 modified nano-titanium dioxide is re-dispersed uniformly in 500 mL of deionized water, and then the hyaluronic acid solution obtained in step (1) is added and stirred to mix evenly, the pH of the solution is adjusted to 5.8, and the reaction is stirred at room temperature for 12-20 hours. The reaction solution is then centrifuged, washed, and freeze-dried to obtain TiO2-g-HA.
4. The hyaluronic acid-grafted nano-titanium dioxide sunscreen according to claim 1, characterized in that: The nano titanium dioxide is rutile nano titanium dioxide with a purity of ≥99.0% and an average particle size of 20nm.
5. A sunscreen, characterized in that: The hyaluronic acid grafted nano titanium dioxide sunscreen obtained according to any one of claims 1 to 4 is used as a sunscreen additive.
6. A sunscreen according to claim 5, characterized in that: The sunscreen comprises the following ingredients by weight: C12-C15 Alkyl Benzoate 15% Cetearyl Alcohol 2% Sodium Stearoyl Glutamate 1% Polyglyceryl-4 Isostearate 0.5% Propyl Octyl Heptyl 12% Disodium EDTA 0.05% Deionized water 46% Xanthan gum 0.5% TiO2-g-HA 5-15%Fragrance 0.05%.
Citation Information
Patent Citations
Sunscreening granule with TiO2-HA core-shell structure as well as preparation method and application thereof