Porous bimetallic catalyst as well as preparation method and application thereof
By loading porous PdZn alloy on carbon materials, the surface adsorption of atomic hydrogen is generated by electrochemical reduction reaction, which solves the problems of low efficiency and poor stability of existing Pd-based electrocatalysts in dechlorination and hydrogenation reaction, and realizes organic chlorine in water Efficient and stable removal of pollutants.
Patent Information
- Application Number
- CN202411088337.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-19
AI Technical Summary
The existing Pd-based electrocatalysts have low efficiency and poor stability in the dechlorination hydrogenation reaction, and are prone to chlorine poisoning, resulting in material inactivation, and it is difficult to efficiently and stably remove organic chlorine pollutants in water.
The porous PdZn alloy is loaded on the carbon material, and the surface adsorbed atomic hydrogen is generated through electrochemical reduction reaction, so as to achieve dechlorination and hydrogenation reaction at a lower voltage, improving the removal efficiency and stability of the catalyst.
The efficient and stable removal of organic chlorine aromatic pollutants in water is achieved, the electrocatalytic degradation performance of the catalyst is improved, and the porous structure is obtained through etching and heating is improved, which is the stability of the material and the catalytic performance of the dehalogenation hydrogenation.
Smart Images

Figure CN118976487A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of catalyst materials, and particularly relates to a porous bimetallic catalyst and a preparation method and application thereof. Background Art
[0002] Chlorinated organic compounds (COCs) are widely used in agriculture, pharmaceuticals, and polymer industries, but the presence of chlorine atoms can cause acute toxicity, genotoxicity, and carcinogenicity, which is detrimental to human and ecosystem health. -1 ), which makes them resistant to traditional biochemical and physicochemical methods in water treatment, and chlorine atoms are not easily removed. Therefore, the development of effective dechlorination methods has received increasing attention.
[0003] Electrochemical reduction dechlorination has mild reaction conditions, does not require chemical addition, and is easy to operate. It is an effective and promising dechlorination method, but there is still a lack of electrocatalysts with high dechlorination efficiency. Among various materials, Pd electrocatalyst is the most effective cathode dechlorination catalyst because Pd can catalyze the Volmer reaction (i.e., H + +e - →H * ) to generate atomic hydrogen (H * ), which has strong reducing properties and can replace Cl atoms in chlorophenol compounds (CPs), but the Faraday efficiency (FE) of this catalyst in dechlorination hydrogenation is less than 2%. Many studies have been devoted to improving the dechlorination hydrogenation efficiency of Pd-based electrocatalysts, such as engineering nanostructures (Pd nanowires) and alloying with other elements (PdAg), but in practical water treatment applications, such Pd-based materials are easily poisoned by chlorine, resulting in material inactivation, and the Pd nanowire structure is prone to collapse after long-term operation. PdAg alloys are prone to electrochemical dissolution due to different metal reduction potentials, resulting in a rapid decrease in dechlorination hydrogenation performance, so their stability is poor.
[0004] Therefore, it is of great significance to provide a catalyst for efficiently and stably removing chlorinated organic compounds. Summary of the invention
[0005] The present invention aims to solve one or more technical problems existing in the above-mentioned prior art, and at least provide a beneficial choice or create conditions. Specifically, the present invention provides a porous bimetallic catalyst, which can efficiently and stably remove organic chlorinated pollutants in water.
[0006] The inventive concept of the present invention is as follows: the bimetallic catalyst of the present invention comprises a PdZn alloy and a carbon material; the PdZn alloy is loaded on the carbon material; the bimetallic catalyst has a porous structure. The present invention loads the PdZn alloy on the carbon material, and the synergistic effect of Pd and Zn can improve the electrocatalytic degradation performance of the catalyst for organic chlorinated aromatics. At the same time, the present invention uses the porous structure to readjust the activity of Pd in PdZn, so that it can generate surface adsorbed atomic hydrogen (H * ads ), and dechlorination and hydrogenation reactions occur under low voltage driving, achieving efficient and stable removal of organic chlorinated aromatic pollutants in water.
[0007] Accordingly, a first aspect of the present invention provides a porous bimetallic catalyst.
[0008] Specifically, the porous bimetallic catalyst comprises a PdZn alloy and a carbon material; the PdZn alloy is loaded on the carbon material; and the PdZn alloy has a porous structure.
[0009] Preferably, the carbon material includes at least one of carbon black, acetylene black and carbon nanotubes; further preferably, the carbon material is carbon black.
[0010] Preferably, the bimetallic catalyst is in the form of a sheet.
[0011] Preferably, the pore size of the porous structure is 0.9-11 nm; further preferably, the pore size of the porous structure is 1-10 nm.
[0012] The second aspect of the present invention provides a method for preparing the porous bimetallic catalyst described in the first aspect of the present invention.
[0013] Specifically, the method for preparing the porous bimetallic catalyst comprises the following steps:
[0014] (1) mixing a palladium precursor, a zinc precursor, and a solvent, and heating them to obtain a mixture;
[0015] (2) mixing a reducing agent and the mixture obtained in step (1), and heating the mixture to obtain a PdZn alloy;
[0016] (3) The PdZn alloy obtained in step (2) is etched and mixed with a carbon material, and heated to obtain the bimetallic catalyst.
[0017] Preferably, in step (1), the palladium precursor includes at least one of palladium diacetylacetonate (Pd(acac)2), PdCl2, and PdBr2; further preferably, the palladium precursor is Pd(acac)2.
[0018] Preferably, in step (1), the zinc precursor includes at least one of zinc diacetylacetonate (Zn(acac)2) and zinc acetate; further preferably, the zinc precursor is Zn(acac)2.
[0019] Preferably, in step (1), the solvent comprises at least one of oleylamine (OAm), 1-octadecene and oleic acid.
[0020] Preferably, in step (1), the mixing is carried out by ultrasonic treatment, and the ultrasonic treatment time is 0.4-1.2 h; more preferably, the ultrasonic treatment time is 0.5-1 h.
[0021] Preferably, in step (1), the heating is performed to a temperature of 55-110° C. and then kept warm for 9-65 min; further preferably, the heating is performed to a temperature of 60-100° C. and then kept warm for 10-60 min.
[0022] Preferably, in step (1), stirring is performed during the insulation process.
[0023] Preferably, in step (2), the reducing agent includes component A and component B; the component A includes at least one of W(CO)6, Mo(CO)6, and V(CO)6; and the component B includes at least one of ascorbic acid (AA), citric acid, and glucose.
[0024] Preferably, in step (2), the mixing is carried out by ultrasonic treatment, and the ultrasonic treatment time is 0.4-1.2 h; more preferably, the ultrasonic treatment time is 0.5-1 h.
[0025] Preferably, in step (2), the heating is performed to a temperature of 190-260° C. and then kept warm for 0.9-2.2 h; further preferably, the heating is performed to a temperature of 200-250° C. and then kept warm for 1-2 h.
[0026] Preferably, in step (2), stirring is performed during the heating process.
[0027] Preferably, in step (2), the heating and heat preservation are followed by washing and drying to obtain a PdZn alloy.
[0028] Preferably, washing is performed using a detergent; the detergent includes cyclohexane and ethanol.
[0029] Preferably, the molar ratio of the palladium precursor, the zinc precursor, the component A and the component B is 1:(0.4-1.8):(0.9-2.2):(2.5-6.5).
[0030] Further preferably, the molar ratio of the palladium precursor, the zinc precursor, the component A and the component B is 1:(0.5-1.5):(1-2):(3-6).
[0031] More preferably, the molar ratio of the palladium precursor, the zinc precursor, the component A and the component B is 1:1:1.87:4.25.
[0032] Preferably, the mass ratio of the PdZn alloy to the carbon material is 0.8-2:8; further preferably, the mass ratio of the PdZn alloy to the carbon material is 1-2:8; further preferably, the mass ratio of the PdZn alloy to the carbon material is 2:8.
[0033] Preferably, the etching is performed using an etchant, and the etchant includes at least one of acetic acid, oxalic acid, and propionic acid; further preferably, the etchant is acetic acid.
[0034] Preferably, after the etching is completed, the PdZn alloy is centrifuged and dried, and then mixed with the carbon material.
[0035] Specifically, a porous structure is obtained by etching. After acid etching, the active zinc (unstable Zn site) is etched into zinc acetate, while the Zn stably combined with Pd will not be etched. The active zinc part can be selectively removed by centrifugation. After the active zinc is removed, the material tends to be stable, Pd will reorganize, and then the Pd site will be readjusted to obtain a porous PdZn alloy, which can carry out catalytic dehalogenation hydrogenation reactions.
[0036] Preferably, in step (3), a porous PdZn alloy is obtained after etching and centrifugation.
[0037] Preferably, in step (3), the mixture is a mixture of the porous PdZn alloy, the carbon material and a solvent.
[0038] Preferably, in step (3), the mixing is carried out by ultrasonic treatment, and the ultrasonic treatment time is 0.4-1.2 h; more preferably, the ultrasonic treatment time is 0.5-1 h.
[0039] Preferably, in step (3), the mixing further includes a process of centrifugation and drying.
[0040] Preferably, in step (3), the heating is performed to a temperature of 270-450°C and then kept warm for 1.5-2.5 hours; further preferably, in step (3), the heating is performed to a temperature of 300-400°C and then kept warm for 1.8-2.2 hours.
[0041] Preferably, in step (3), the heating temperature rise rate is 1.5-2.5°C / min, further preferably, the heating temperature rise rate is 1.8-2.2°C / min; further preferably, the heating temperature rise rate is 2°C / min.
[0042] The third aspect of the present invention provides a use of the porous bimetallic catalyst described in the first aspect of the present invention in the electrocatalytic degradation of chlorinated organic compounds in water.
[0043] Preferably, the chlorinated organic compound includes at least one of 2,4,5-trichlorophenol, 2,4-dichlorophenol, 2-chlorophenol and chloramphenicol.
[0044] Preferably, a porous PdZn / C electrode needs to be prepared during the electrocatalytic degradation, and a platinum sheet and Ag / AgCl are used as a counter electrode and a reference electrode, respectively.
[0045] Preferably, the electrocatalytic degradation is carried out at a constant potential, and relative to the Ag / AgCl reference electrode, the constant potential is -0.75V to -1.25V; further preferably, the constant potential is -0.85V.
[0046] Preferably, the concentration of the chlorinated organic compound is 90-1100 μM; further preferably, the concentration of the chlorinated organic compound is 100-1000 μM; further preferably, the concentration of the chlorinated organic compound is 310 μM.
[0047] Preferably, the porous bimetallic catalyst in the porous PdZn / C electrode is 4.5-22 mg; further preferably, the porous bimetallic catalyst in the porous PdZn / C electrode is 5-20 mg; further preferably, the porous bimetallic catalyst in the porous PdZn / C electrode is 10 mg.
[0048] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:
[0049] (1) The bimetallic catalyst of the present invention comprises a PdZn alloy and a carbon material; the PdZn alloy is loaded on the carbon material; and the PdZn alloy has a porous structure. The present invention loads the PdZn alloy on the carbon material, and the synergistic effect of Pd and Zn can improve the electrocatalytic degradation performance of the catalyst for organic chlorinated aromatics. At the same time, the present invention uses the porous structure to readjust the activity of Pd in PdZn, so that it can generate surface adsorbed atomic hydrogen (H) through an electrochemical reduction reaction. * ads ), and dechlorination and hydrogenation reactions occur under low voltage driving, achieving efficient and stable removal of organic chlorinated aromatic pollutants in water.
[0050] (2) The preparation process of the present invention is simple. A porous structure is obtained by etching. After acid etching, the active zinc is etched into zinc acetate, while the Zn stably combined with Pd will not be etched. The active zinc part can be selectively removed by centrifugation. After the active zinc is removed, the material tends to be stable, Pd will be reorganized, and then the site of Pd will be readjusted to obtain a porous PdZn alloy. Then, a porous sheet structure is obtained by heating, which has good dehalogenation and hydrogenation catalytic performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0051] Figure 1 This is a transmission electron microscopy image of the porous PdZn / C bimetallic catalyst prepared in Example 1 of the present invention;
[0052] Figure 2 This is a transmission electron microscope image of the PdZn / C bimetallic catalyst prepared in Comparative Example 1 of the present invention;
[0053] Figure 3 This is a transmission electron microscope image of the porous Pd / C catalyst prepared in Comparative Example 2 of the present invention;
[0054] Figure 4 Cyclic voltammetry curves of the catalyst prepared in Example 1 of the present invention and Comparative Example 1 and a commercial Pd / C catalyst;
[0055] Figure 5 This is a graph showing the removal efficiency of 2,4-dichlorophenol by the catalysts prepared in Examples 1-2 of the present invention and Comparative Examples 1-2 and a commercial Pd / C catalyst;
[0056] Figure 6 This is a graph showing the stability results of the porous PdZn / C bimetallic catalyst prepared in Example 1 of the present invention;
[0057] Figure 7 This is a graph showing the stability results of the porous Pd / C catalyst prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION
[0058] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.
[0059] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.
[0060] Example 1
[0061] A method for preparing a porous bimetallic catalyst comprises the following steps:
[0062] (1) Pd(acac)2 (21.3 mg, 80 μmol) and Zn(acac)2 (21.6 mg, 80 μmol) were added to a four-necked flask containing 24 mL of Ammonium hydroxide and ultrasonicated for 0.5 h; the mixture was then heated to 80 °C in a vacuum and maintained under magnetic stirring for 1 h; then cooled to room temperature under a nitrogen atmosphere; W(CO)6 (53.3 mg, 150 μmol) and AA (60.0 mg, 340 μmol) were then added, ultrasonicated for 0.5 h, vacuumed again for 5 min, heated to 220 °C under a nitrogen atmosphere with magnetic stirring, and maintained for 2 h to obtain a mixture; the mixture was rapidly cooled to room temperature, centrifuged, the solid was collected, and washed two to three times with a mixture of cyclohexane / ethanol (v:v=1:3) to obtain a PdZn alloy;
[0063] (2) etching the PdZn alloy obtained in step (1) in an acetic acid solution at 80° C. for 12 h, centrifuging the obtained product with ethanol, washing it with ethanol three times, and drying it at 80° C. to obtain a porous PdZn alloy;
[0064] (3) The porous PdZn alloy obtained in step (2) was dispersed in 20 mL of cyclohexane, 40 mg of carbon (Vulcan XC-72) and 20 mL of ethanol, ultrasonically mixed for 1 h, and centrifuged to dry. In order to remove organic matter on the material, the product obtained by centrifugation was heated to 350° C. at 2° C. / min and maintained for 2 h in a mixed gas of H2 / Ar (the mass concentration of H2 in the mixed gas is 10%) to carbonize the organic matter on the alloy, thereby obtaining a porous bimetallic catalyst (porous PdZn / C bimetallic catalyst).
[0065] Example 2
[0066] A method for preparing a porous bimetallic catalyst comprises the following steps:
[0067] (1) PdBr2 (24.4 mg, 80 μmol) and Zn(CH3COO)2 (14.68 mg, 80 μmol) were added to a four-necked flask containing 24 mL of OAm, and ultrasonicated for 0.5 h. The mixture was heated to 80°C in a vacuum and maintained under magnetic stirring for 1 h. Then, it was cooled to room temperature under a nitrogen atmosphere, and then W(CO)6 (53.3 mg, 150 μmol) and AA (60.0 mg, 340 μmol) were added. The mixture was ultrasonicated for 0.5 h, vacuumed again for 5 min, and then heated to 220°C under nitrogen with magnetic stirring and maintained for 2 h to obtain a mixture. Finally, the mixture was rapidly cooled to room temperature, centrifuged, the solid was collected, and washed two to three times with a cyclohexane / ethanol (v:v=1:3) mixture to obtain a PdZn alloy.
[0068] (2) etching the PdZn alloy obtained in step (1) in an acetic acid solution at 80° C. for 12 h, centrifuging the obtained product with ethanol, washing it with ethanol three times, and drying it under ambient conditions to obtain a porous PdZn alloy;
[0069] (3) The porous PdZn alloy obtained in step (2) was dispersed in 20 mL of cyclohexane, 40 mg of carbon (Vulcan XC-72) and 20 mL of ethanol, ultrasonically mixed for 1 h, centrifuged and dried; in order to remove organic matter on the material, the product obtained by centrifugation was heated to 350° C. at 2° C. / min and maintained for 2 h in a mixed gas of H2 / Ar (the mass concentration of H2 in the mixed gas is 10%) to obtain a porous bimetallic catalyst (porous PdZn / C bimetallic catalyst).
[0070] Comparative Example 1
[0071] The only difference between Comparative Example 1 and Example 1 is that the bimetallic catalyst of Comparative Example 1 does not have a porous structure, and accordingly, step (2) is not performed in the preparation process of Comparative Example 1, but the PdZn alloy obtained in step (1) is directly subjected to step (3), and the rest is the same as Example 1.
[0072] Specifically, the preparation method of the PdZn / C catalyst in Comparative Example 1 comprises the following steps:
[0073] (1) Pd(acac)2 (21.3 mg, 80 μmol) and Zn(acac)2 (21.6 mg, 80 μmol) were added to a four-necked flask containing 24 mL of Ammonium hydroxide and ultrasonicated for 0.5 h; the mixture was then heated to 80 °C in a vacuum and maintained under magnetic stirring for 1 h; then cooled to room temperature under a nitrogen atmosphere; W(CO)6 (53.3 mg, 150 μmol) and AA (60.0 mg, 340 μmol) were then added, ultrasonicated for 0.5 h, vacuumed again for 5 min, heated to 220 °C under a nitrogen atmosphere with magnetic stirring, and maintained for 2 h to obtain a mixture; the mixture was rapidly cooled to room temperature, centrifuged, the solid was collected, and washed two to three times with a mixture of cyclohexane / ethanol (v:v=1:3) to obtain a PdZn alloy;
[0074] (2) The porous PdZn alloy obtained in step (1) was dispersed in 20 mL of cyclohexane, 40 mg of carbon (Vulcan XC-72) and 20 mL of ethanol, ultrasonically mixed for 1 h, centrifuged and dried, and in order to remove organic matter on the material, the product obtained by centrifugation was heated to 350° C. at 2° C. / min and maintained for 2 h in a mixed gas of H2 / Ar (the mass concentration of H2 in the mixed gas is 10%) to obtain a bimetallic catalyst (PdZn / C bimetallic catalyst).
[0075] Comparative Example 2
[0076] The catalyst of Comparative Example 2 has a porous structure, but does not contain Zn and is a single metal catalyst.
[0077] Specifically, the preparation method of the porous Pd / C catalyst comprises the following steps:
[0078] (1) Pd(acac)2 (24.4 mg, 80 μmol) and 80 mg of ammonium bromide were added to a four-necked flask containing 24 mL of OAm, and then placed in an oil bath at 70 °C for 2 h to obtain a light yellow uniform solution; after the solution was cooled to room temperature, W(CO)6 (53.3 mg, 150 μmol) and 3 mL of THF were added, the mixture was ultrasonicated for 30 min, and then heated at 50 °C for 1 h to obtain a black product; the black product was centrifuged at 2500 rpm, washed three times with cyclohexane, and then redispersed in 5 mL of cyclohexane and transferred to a 10 mL ordinary sample bottle; the sample bottle was then heated at 45 °C for 24 h to obtain porous Pd nanosheets;
[0079] (2) The porous Pd nanosheets prepared in step (1) were dispersed in 20 mL of cyclohexane, 40 mg of carbon (Vulcan XC-72) and 20 mL of ethanol, ultrasonically mixed for 1 h, centrifuged, dried, and in order to remove organic matter on the material, the product obtained by centrifugation was heated to 350 ° C at 2 ° C / min and maintained for 2 h in a mixed gas of H2 / Ar (the mass concentration of H2 in the mixed gas is 10%) to obtain a porous Pd / C catalyst.
[0080] Performance Testing
[0081] 1. Transmission electron microscopy test
[0082] The porous PdZn / C bimetallic catalyst prepared in Example 1, the PdZn / C bimetallic catalyst prepared in Comparative Example 1, and the porous Pd / C catalyst prepared in Comparative Example 2 were observed by transmission electron microscopy (TEM). The transmission electron microscopy images are shown as follows: Figure 1 , 2 , as shown in Figure 3.
[0083] Depend on Figure 1 It can be clearly seen from the TEM image that the dark flakes are PdZn alloys, and the smaller blank areas in the flakes are caused by the porous structure. That is, the catalyst prepared in Example 1 has a porous structure with a pore size of 0.5-2nm, which proves the successful synthesis of the porous PdZn bimetallic catalyst.
[0084] Depend on Figure 2 It can be seen from the TEM image that the PdZn bimetallic catalyst prepared in Comparative Example 1 has a strict sheet structure and does not have a porous structure.
[0085] Depend on Figure 3 It can be seen from the TEM image that the Pd / C catalyst prepared in Comparative Example 2 has a porous structure with a pore size of 2-5 nm.
[0086] 2. Cyclic voltammetry test
[0087] The performance of the catalyst prepared in Example 1 and Comparative Example 1 and the commercial Pd / C catalyst in generating H*ads was evaluated by cyclic voltammetry. The specific test method is as follows: 5 mg of the catalyst prepared in Example 1 and Comparative Example 1 and the commercial Pd / C catalyst were added with 0.8 mL of water, 0.2 mL of isopropanol and 0.01 mL of nafion solution, respectively, and then ultrasonicated for 0.5 h to obtain a uniformly dispersed solution, and then 20 μL of the solution was dripped on the glassy carbon electrode as the working electrode, and the Pt sheet and Ag / AgCl were used as the counter electrode and reference electrode respectively. The prepared electrode was tested in a 0.05 M sodium sulfate solution saturated with N2 at -1.15-0.6 V by cyclic voltammetry.
[0088] The cyclic voltammetry curves of the catalyst prepared in Example 1 and Comparative Example 1 and the commercial Pd / C catalyst are shown in FIG. Figure 4 As shown. Among them, the horizontal axis Potential (V vs. Ag / AgCl) represents the potential (relative to the Ag / AgCl reference electrode), and the vertical axis j (mAcm -2 ) represents the current density (milliamperes per square centimeter).
[0089] In the cyclic voltammetry curve, H2 molecules, H * abs (atomic hydrogen, H * The species is absorbed onto the Pd atom by forming a Pd-H bond as H * abs ) and H * ads The broad peaks related to oxidation appear at about -0.80 to -0.60 V, -0.20 to -0.10 V, and -0.10 to 0.00 V. Figure 4 It can be seen that the commercial Pd / C catalyst has obvious oxidation peaks in the potential range of these three substances, indicating that the Pd / C catalyst can effectively generate these three substances (H2 molecules, H * abs and H * ads In the porous PdZn / C bimetallic catalyst prepared in Example 1, not only the H2 oxidation peak was suppressed to a great extent, but also no obvious H * absThe oxidation peaks of the porous PdZn / C bimetallic catalyst are shown in Figure 2, except for a single broad oxidation peak at ∼0 V, which indicates that the porous PdZn / C bimetallic catalyst has good H * ads The PdZn / C bimetallic catalyst prepared in Comparative Example 1 mainly generates H2 molecules and H * abs . Due to H * ads It is the main reducing species in the electrochemical dehalogenation hydrogenation reaction. Accordingly, the porous PdZn / C bimetallic catalyst prepared in Example 1 will also have good dehalogenation hydrogenation catalytic performance and can effectively remove organic chlorinated aromatic pollutants in water.
[0090] 3. Dehalogenation and hydrogenation catalytic performance test
[0091] The dehalogenation hydrogenation catalytic performance of the catalysts prepared in Examples 1-2 and Comparative Examples 1-2 and the commercial Pd / C catalyst was tested, and the specific method is as follows:
[0092] The catalysts prepared in Example 1-2 and Comparative Example 1-2 and the commercial Pd / C catalyst were sprayed onto carbon paper to obtain corresponding electrodes. An electrolysis experiment was carried out using a double-chamber H-type electrolytic cell separated by a nafion 211 proton ion exchange membrane. A platinum sheet and Ag / AgCl (3.0 M potassium chloride) were used as the counter electrode and the reference electrode, respectively. The anolyte and the catholyte were both 50 mL of sodium sulfate (50 mM) solution. Before treatment, a certain amount of 2,4-dichlorophenol was added to the cathode chamber to make its concentration reach 0.31 mM. The cell was controlled at a constant potential of -0.85 V by an electrochemical station (CHI 760D). Samples were collected at 0 h, 0.5 h, 1 h, 1.5 h, 2 h, 2.5 h, and 3 h of electrocatalytic degradation, and filtered using a 0.21 μm polytetrafluoroethylene membrane. The concentrations of 2,4-dichlorophenol and its intermediates in the samples were tested by high performance liquid chromatography.
[0093] The calculation method for the removal efficiency of 2,4-dichlorophenol by the catalysts prepared in Example 1-2 and Comparative Example 1-2 and the commercial Pd / C catalyst is (final concentration of 1-2,4-dichlorophenol in sodium sulfate solution / initial concentration of 2,4-dichlorophenol)×100%.
[0094] The removal efficiency of 2,4-dichlorophenol by the catalysts prepared in Examples 1-2 and Comparative Examples 1-2 and the commercial Pd / C catalyst is as follows: Figure 5 As shown, the horizontal axis Time (h) represents time (hours), and the vertical axis C t / C0 represents the current concentration of 2,4-dichlorophenol in the solution / initial concentration, C trepresents the current concentration of 2,4-dichlorophenol in the solution; C0 represents the initial concentration of 2,4-dichlorophenol in the solution.
[0095] Depend on Figure 5 It can be seen that within 3 hours, the removal efficiency of the catalysts prepared in Examples 1 and 2 for 2,4-dichlorophenol can reach about 90%, while the removal efficiencies of the catalysts prepared in Comparative Examples 1-2 and the commercial Pd / C catalyst for 2,4-dichlorophenol are 18%, 48% and 53%, respectively. The removal efficiency of the catalysts in Examples 1-2 of the present invention for 2,4-dichlorophenol is significantly better than that of the catalysts prepared in Comparative Examples 1 and 2 and the commercial Pd / C catalyst, and has good dehalogenation and hydrogenation catalytic performance.
[0096] 4. Stability test
[0097] The porous PdZn / C bimetallic catalyst prepared in Example 1 and the porous Pd / C catalyst prepared in Comparative Example 2 were tested for stability. The test method was as follows:
[0098] The above dehalogenation hydrogenation catalytic performance test is a catalytic process. The porous PdZn / C bimetallic catalyst prepared in Example 1 and the porous Pd / C catalyst prepared in Comparative Example 2 were tested for 50 cycles respectively to observe the stability of the catalyst.
[0099] The stability test results of the porous PdZn / C bimetallic catalyst prepared in Example 1 are as follows: Figure 6 As shown, the stability test results of the porous Pd / C catalyst prepared in Comparative Example 2 are as follows Figure 7 As shown. Among them, the vertical axis C t / C0 represents the current concentration of 2,4-dichlorophenol in the solution / initial concentration, C t All represent the current concentration of 2,4-dichlorophenol in the solution; C0 all represent the initial concentration of 2,4-dichlorophenol in the solution.
[0100] Depend on Figure 6 and 7 It can be seen that after 50 cycles, the removal efficiency of the catalyst prepared in Example 1 for 2,4-dichlorophenol can still reach about 90% within 3 hours; while the removal efficiency of the catalyst prepared in Comparative Example 2 for 2,4-dichlorophenol after 50 cycles within 3 hours is only about 30%, and the removal efficiency is reduced by about 43%, indicating that the catalyst prepared in Example 1 has good stability for the dechlorination hydrogenation reaction.
[0101] In summary, the catalyst prepared by the present invention is a PdZn bimetallic catalyst with a porous structure. The synergistic effect of Pd and Zn can improve the electrocatalytic degradation performance of the catalyst for organic chlorinated aromatics. At the same time, the present invention uses the porous structure to readjust the activity of Pd in PdZn, so that it can generate surface adsorbed atomic hydrogen (H * ads ), and dechlorination and hydrogenation reactions occur under low voltage driving, achieving efficient and stable removal of organic chlorinated aromatic pollutants in water.
[0102] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A bimetallic catalyst, characterized in that: The invention comprises a PdZn alloy and a carbon material; the PdZn alloy is loaded on the carbon material; and the PdZn alloy has a porous structure.
2. The bimetallic catalyst according to claim 1, characterized in that The carbon material includes at least one of carbon black, acetylene black and carbon nanotubes.
3. The bimetallic catalyst according to claim 1, characterized in that The bimetallic catalyst is in the form of flakes.
4. The bimetallic catalyst according to claim 1, characterized in that The pore size of the porous structure is 0.9-11 nm.
5. The method for preparing the bimetallic catalyst according to any one of claims 1 to 4, characterized in that: The following steps are involved: (1) mixing a palladium precursor, a zinc precursor, and a solvent, and heating them to obtain a mixture; (2) mixing a reducing agent and the mixture obtained in step (1), and heating the mixture to obtain a PdZn alloy; (3) The PdZn alloy obtained in step (2) is etched and mixed with a carbon material, and heated to obtain the bimetallic catalyst.
6. The preparation method according to claim 5, characterized in that: In step (1), the palladium precursor includes at least one of palladium diacetylacetonate, PdCl2, and PdBr2; and / or the zinc precursor includes at least one of zinc diacetylacetonate and zinc acetate.
7. The preparation method according to claim 5, characterized in that: In step (2), the reducing agent includes component A and component B; the component A includes at least one of W(CO)6, Mo(CO)6, and V(CO)6; and the component B includes at least one of ascorbic acid, citric acid, and glucose.
8. The preparation method according to claim 7, characterized in that: The molar ratio of the palladium precursor, the zinc precursor, the component A and the component B is 1:(0.4-1.8):(0.9-2.2):(2.5-6.5).
9. The preparation method according to claim 5, characterized in that: In step (3), the etching is performed using an etchant, wherein the etchant includes at least one of acetic acid, oxalic acid, and propionic acid; and / or the mass ratio of the PdZn alloy to the carbon material is (0.8-2):
8.
10. Use of the bimetallic catalyst according to any one of claims 1 to 4 in the electrocatalytic degradation of chlorinated organic compounds in water.
Citation Information
Patent Citations
Palladium catalyst for processing chlorinated organics in water and method for preparing same
CN101711981A
Bimetal composite catalyst, preparation method and application thereof, working electrode and battery system
CN113813957A
High-efficiency composite Pd-Zn / ZnTiO3 catalyst with low Pd content as well as preparation method and application thereof
CN114984950A
Catalyst for liquid-phase selective hydrogenation of acetylene hydrocarbons and a method for production thereof
RU2738233C1
Nanoscale particles and the treatment of chlorinated contaminants
US20030039857A1
Cited By
Electrochemical double-hydrogenation three-pool system and application thereof
CN120700510A