Sulfur poisoning resistant catalyst as well as preparation method and application thereof
The anti-sulfur poisoning catalyst was prepared by impregnation method, and the oxalic acid-solution vanadium source supported by platinum and vanadium to aluminum oxide support was used to solve the problems of low activity and easy deactivation of existing catalysts, and achieve efficient reduction of carbon monoxide emissions and sulfur resistance. Improvement.
Patent Information
- Application Number
- CN202411268168.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The existing anti-sulfur poisoning catalysts have low activity, making it difficult to effectively reduce carbon monoxide emissions in the flue gas of the steel industry, and at the same time they are inactivated in the presence of sulfur dioxide, affecting the catalytic performance.
The anti-sulfur poisoning catalyst was prepared by impregnation method, and the oxalic acid-solution vanadium source was used to support platinum and vanadium on the surface of the aluminum oxide support. Vanadium was used as a sacrificial agent to adsorb platinum in sulfur oxide protective active site, achieving high activity and low activity through a one-step process. Cost production.
The prepared catalyst has excellent sulfur resistance and high catalytic activity, can effectively reduce carbon monoxide emissions, and remains stable in a high-temperature and high-sulfur environment, with a wide range of application prospects.
Smart Images

Figure CN118976488A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to a sulfur-poisoning resistant catalyst and a preparation method and application thereof. Background Art
[0002] Carbon monoxide is a common air pollutant. The steel industry is one of the main sources of carbon monoxide emissions. Carbon monoxide emitted from the sintering process accounts for 40% of the total carbon monoxide emitted by the entire steel industry, and it is urgent to focus on control. At present, the mainstream technology for carbon monoxide emission control is catalytic oxidation, which is to use catalysts to reduce the reaction energy barrier of carbon monoxide so that it can be converted into non-toxic carbon dioxide under relatively mild conditions. The core of this technology is to develop high-performance carbon monoxide oxidation catalysts. The components of fixed source flue gas are relatively complex. For example, sulfur dioxide is often included in the flue gas of the steel industry. The presence of sulfur dioxide will react with the active components on the catalyst surface to form inert sulfates, causing the catalyst to deactivate.
[0003] At present, the sulfur-poisoning-resistant catalysts prepared by existing technologies have low activity. Therefore, there is an urgent need to develop carbon monoxide oxidation catalysts that have both high activity and high sulfur resistance. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides a sulfur-resistant catalyst and a preparation method and application thereof. The sulfur-resistant catalyst prepared by the present invention has excellent sulfur resistance and high activity, and adsorbs sulfur oxides through the sacrificial agent effect of vanadium, thereby protecting the active site platinum. The present invention adopts an impregnation method and uses oxalic acid to dissolve the vanadium source. The production process is clean and the cost is low, which has application prospects.
[0005] To achieve this object, the present invention adopts the following technical solutions:
[0006] In a first aspect, the present invention provides a method for preparing a sulfur-poisoning resistant catalyst, the preparation method comprising:
[0007] Under stirring conditions, a platinum source, a vanadium source, oxalic acid, aluminum oxide and a solvent are mixed to obtain a suspension; after the suspension is dried and sintered, the sulfur-poisoning-resistant catalyst is obtained.
[0008] The present invention adopts an impregnation method and uses oxalic acid to dissolve the vanadium source. The capillary pressure is generated by surface tension, so that the mixed solvent penetrates into the interior of the solid aluminum oxide, eliminating the step of catalyst molding. At the same time, the present application directly loads the platinum source and the vanadium source onto the surface of the aluminum oxide carrier at the same time through a one-step impregnation method, the production process is clean, the cost is low, and the application prospect is broad.
[0009] Preferably, the platinum source comprises tetraammineplatinum nitrate.
[0010] Preferably, the mass of the platinum source accounts for 0.1-0.5% of the mass of the alumina, for example, it can be 0.1%, 0.15%, 0.2%, 0.25%, 0.3%, 0.35%, 0.4%, 0.45% or 0.5%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0011] Preferably, the vanadium source comprises ammonium metavanadate.
[0012] Preferably, the mass of the vanadium source accounts for 1-25% of the mass of the alumina, for example, it can be 1%, 3%, 5%, 7%, 9%, 11%, 15%, 17%, 20% or 25%, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0013] The present invention can further improve the catalytic activity of carbon monoxide by controlling the dosage of the vanadium source, and at the same time exhibits excellent resistance to sulfur poisoning.
[0014] Preferably, the solvent comprises deionized water.
[0015] Preferably, the mixing temperature is 30-40°C, for example, 30°C, 32°C, 34°C, 36°C, 37°C, 39°C or 40°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0016] Preferably, the mixing order is: first mix the solvent and the platinum source, then mix the vanadium source and oxalic acid, and finally mix the aluminum oxide.
[0017] Preferably, the stirring speed is 200-400 rpm, for example, 200 rpm, 250 rpm, 300 rpm, 350 rpm or 400 rpm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0018] Preferably, the stirring time is 2-4 h, for example, 2 h, 2.5 h, 3 h, 3.5 h or 4 h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0019] Preferably, the drying step includes drying after removing moisture.
[0020] Preferably, the drying temperature is 100-120°C, for example, it can be 100°C, 102°C, 104°C, 106°C, 108°C, 110°C, 112°C, 114°C, 116°C, 118°C or 120°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0021] Preferably, the drying time is 8-16 hours, for example, it can be 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours or 16 hours, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0022] Preferably, the sintering temperature is 400-600°C, for example, it can be 400°C, 420°C, 440°C, 460°C, 480°C, 500°C, 520°C, 540°C, 560°C, 580°C or 600°C, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0023] Preferably, the sintering time is 2-4 hours, for example, 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0024] As a preferred technical solution of the present invention, the preparation method comprises the following steps:
[0025] Dissolve the platinum source in deionized water at 30-40°C, then add the vanadium source and oxalic acid, and after all are dissolved, add aluminum oxide and stir to obtain a suspension;
[0026] The suspension is dehydrated and dried at 100-120° C. for 8-16 hours to obtain a dried material;
[0027] The dried material is sintered at 400-600° C. for 2-4 hours to obtain the sulfur-poisoning resistant catalyst.
[0028] In a second aspect, the present invention provides a sulfur-poisoning resistant catalyst prepared by the preparation method described in the first aspect, wherein the sulfur-poisoning resistant catalyst uses aluminum oxide as a carrier and is loaded with platinum and vanadium.
[0029] In the sulfur-poisoning resistant catalyst prepared by the present invention, platinum is the main active component of the catalyst, and vanadium is used as a sacrificial agent to adsorb sulfur oxides, thereby protecting the active site platinum, thereby ensuring the high activity of the catalyst. Therefore, the catalyst prepared by the present invention has excellent sulfur resistance and high activity.
[0030] Preferably, the molar ratio of platinum to vanadium is 1:(0.25-40), for example, it can be 1:0.5, 1:1, 1:2, 1:3, 1:3.5, 1:4, 1:5, 1:6, 1:7, 1:8, 1:9, 1:10, 1:12, 1:13, 1:14, 1:15, 1:20, 1:30 or 1:40, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, preferably 1:(0.25-15).
[0031] Preferably, the molar ratio of vanadium to aluminum oxide is (1-10):1, for example, 1:1, 1:3, 1:5, 1:7, 1:9, 1:10, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable, and more preferably (1-9):1.
[0032] In a third aspect, the present invention provides an application of the sulfur-poisoning resistant catalyst as described in the second aspect, wherein the sulfur-poisoning resistant catalyst is applied to catalytic oxidation of carbon monoxide.
[0033] Compared with the prior art, the present invention has at least the following beneficial effects:
[0034] (1) The present invention adopts an impregnation method to generate capillary pressure through surface tension, so that the mixed solvent penetrates into the interior of solid alumina, eliminating the step of catalyst molding. At the same time, the present application uses a one-step impregnation method, using oxalic acid to dissolve the vanadium source, and directly loads the platinum source and the vanadium source onto the surface of the alumina carrier at the same time. The production process is clean, the cost is low, and the application prospects are broad;
[0035] (2) In the sulfur-poisoning resistant catalyst prepared by the present invention, vanadium is a sacrificial agent and platinum is an active component of the catalyst. The vanadium adsorbs sulfur oxides to protect the active site platinum, thereby ensuring the high activity of the catalyst. Therefore, the catalyst prepared by the present invention has excellent sulfur resistance and high activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a catalytic activity diagram of oxidizing carbon monoxide before presulfurization of the sulfur-poisoning-resistant catalysts prepared in Example 1, Examples 4-7 and Comparative Example 1;
[0037] Figure 2 It is a catalytic activity diagram of the oxidation of carbon monoxide by the sulfur-poisoning resistant catalysts prepared in Example 1, Examples 4-7 and Comparative Example 1 after presulfurization. DETAILED DESCRIPTION
[0038] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.
[0039] Example 1
[0040] This embodiment provides a method for preparing a sulfur-poisoning resistant catalyst, and the preparation method is as follows:
[0041] (1) 0.03 g of tetraammine platinum nitrate was dissolved in 150 mL of deionized water at 37° C., and then 0.41 g of ammonium metavanadate and 6.2 g of oxalic acid were added. After the tetraammine platinum nitrate, ammonium metavanadate and oxalic acid were completely dissolved, 6 g of Al2O3 was added, and the mixture was stirred at 37° C. and 300 rpm for 3 h to obtain a suspension;
[0042] (2) placing the suspension in step (1) into a rotary evaporator to remove moisture, and then drying in an oven at 110° C. for 10 h to obtain a dried material;
[0043] (3) placing the dried material in step (2) in a muffle furnace and sintering at 500° C. for 3 h to obtain the catalyst resistant to sulfur poisoning.
[0044] The catalyst prepared in this example is named F-Pt 0.25 V3Al2O3.
[0045] Example 2
[0046] This embodiment provides a method for preparing a sulfur-poisoning resistant catalyst, and the preparation method is as follows:
[0047] (1) 0.006 g of tetraammine platinum nitrate was dissolved in 100 mL of deionized water at 40° C., and then 0.06 g of ammonium metavanadate and 6 g of oxalic acid were added. After the tetraammine platinum nitrate, ammonium metavanadate and oxalic acid were completely dissolved, 6 g of Al2O3 was added, and the mixture was stirred at 40° C. and 400 rpm for 2 h to obtain a suspension;
[0048] (2) placing the suspension in step (1) into a rotary evaporator to remove moisture, and then drying in an oven at 120° C. for 8 h to obtain a dried material;
[0049] (3) placing the dried material in step (2) in a muffle furnace and sintering at 400° C. for 4 h to obtain the catalyst resistant to sulfur poisoning.
[0050] The catalyst prepared in this example is named F2-Pt 0.05 V 0.4 Al2O3.
[0051] Example 3
[0052] This embodiment provides a method for preparing a sulfur-poisoning resistant catalyst, and the preparation method is as follows:
[0053] (1) 0.03 g of tetraammine platinum nitrate was dissolved in 100 mL of deionized water at 30° C., and then 1.38 g of ammonium metavanadate and 6 g of oxalic acid were added. After the tetraammine platinum nitrate, ammonium metavanadate and oxalic acid were completely dissolved, 6 g of Al2O3 was added, and the mixture was stirred at 30° C. and 200 rpm for 4 h to obtain a suspension;
[0054] (2) placing the suspension in step (1) into a rotary evaporator to remove moisture, and then drying in an oven at 100° C. for 16 h to obtain a dried material;
[0055] (3) placing the dried material in step (2) in a muffle furnace and sintering at 600° C. for 2 h to obtain the catalyst resistant to sulfur poisoning.
[0056] The catalyst prepared in this example is named F3-Pt 0.25 V 10 Al2O3.
[0057] Example 4
[0058] The difference between this embodiment and embodiment 1 is that, except for adding 0.14 g of ammonium metavanadate in step (1), the rest is the same as embodiment 1.
[0059] The catalyst prepared in this example is named F-Pt 0.25 V1Al2O3.
[0060] Example 5
[0061] The difference between this embodiment and embodiment 1 is that, except for adding 0.69 g of ammonium metavanadate in step (1), the rest is the same as embodiment 1.
[0062] The catalyst prepared in this example is named F-Pt 0.25 V5Al2O3.
[0063] Example 6
[0064] The difference between this embodiment and embodiment 1 is that, except for adding 0.96 g of ammonium metavanadate in step (1), the rest is the same as embodiment 1.
[0065] The catalyst prepared in this example is named F-Pt 0.25 V7Al2O3.
[0066] Example 7
[0067] The difference between this embodiment and embodiment 1 is that, except for adding 1.38 g of ammonium metavanadate in step (1), the rest is the same as embodiment 1.
[0068] The catalyst prepared in this example is named F-Pt 0.25 V 10 Al2O3.
[0069] Example 8
[0070] The only difference between this embodiment and embodiment 1 is that, except for the sintering temperature of step (3) being 700° C., the rest is the same as embodiment 1.
[0071] The catalyst prepared in this example is named F4-Pt 0.25 V3Al2O3.
[0072] Example 9
[0073] The only difference between this embodiment and embodiment 1 is that, except for the sintering temperature of step (3) being 300° C., the rest is the same as embodiment 1.
[0074] The catalyst prepared in this example is named F5-Pt 0.25 V3Al2O3.
[0075] Comparative Example 1
[0076] The difference between this comparative example and Example 1 is that, except that ammonium metavanadate is not added in step (1), the rest is the same as Example 1.
[0077] The catalyst prepared in this comparative example is named F-Pt 0.25 Al2O3.
[0078] Figure 1 The catalytic activity diagram of the anti-sulfur poisoning catalysts prepared in Examples 1, 4-7 and Comparative Example 1 before presulfurization for oxidizing carbon monoxide is shown in the figure. It can be seen from the figure that the introduction of vanadium almost increases the activity of the catalyst for oxidizing carbon monoxide. This may be because the appropriate interaction between vanadium and platinum improves the ability of Pt to oxidize carbon monoxide;
[0079] Figure 2 The catalytic activity diagram of the oxidized carbon monoxide by the presulfurized anti-sulfurized catalysts prepared in Examples 1, 4-7 and Comparative Example 1 is shown in FIG. 1 . 0.25 V3Al2O3 catalyst has the best catalytic carbon monoxide oxidation activity. The introduction of a lower content of vanadium cannot fully play the role of the sacrificial agent, while the introduction of too high a content will cause more sulfate to accumulate on the carrier, thereby blocking the active sites.
[0080] Comparative Example 2
[0081] The difference between this comparative example and Example 1 is that, except that oxalic acid is not added in step (1), the rest is the same as Example 1.
[0082] The catalyst prepared in this comparative example is named F6-Pt 0.25 V3Al2O3.
[0083] Comparative Example 3
[0084] The difference between this comparative example and Example 1 is that, except for replacing oxalic acid with ethanol in step (1), the rest is the same as Example 1.
[0085] The catalyst prepared in this comparative example is named F7-Pt 0.25 V3Al2O3.
[0086] Test Method
[0087] The sulfur-resistant catalysts prepared in Examples 1-9 and Comparative Examples 1-3 were placed in a 100 ppm SO2 / Air atmosphere for presulfurization for 12 h. The obtained catalysts were named S-Pt 0.25 / Al2O3、S-Pt 0.25 V1 / Al2O3, S-Pt 0.25 V3 / Al2O3, S-Pt 0.25 V5 / Al2O3, S-Pt 0.25 V7 / Al2O3, S-Pt 0.25 V 10 / Al2O3、S2-Pt 0.05 V 0.4 / Al2O3, S3-Pt 0.25 V 10 / Al2O3、S4-Pt 0.25 V3 / Al2O3 and S5-Pt 0.25 V3 / Al2O3.
[0088] Take a certain amount of the above catalyst, the size is 40-60 mesh, put it into the catalyst activity evaluation device, and the activity evaluation is carried out in a fixed bed reactor. The test conditions are: N2 = 400mL / min, CO = 4000ppm, O2 = 50mL / min; the total flow rate is 500mL / min, and the reaction space velocity is 100000mL / gh -1 The test results of the catalyst and presulfurized catalyst are as follows Figure 1 and Figure 2 As shown, the T of the catalyst before and after presulfurization is 10 , T 50 , T 90 The temperatures are recorded in Tables 1 and 2, respectively.
[0089] Table 1
[0090] Catalyst naming <![CDATA[T 10 (℃)]]> <![CDATA[T 50 (℃)]]> <![CDATA[T 90 (℃)]]> Example 1 <![CDATA[F-Pt 0.25 V3 / Al2O3]]> 178 208 216 Example 2 <![CDATA[F2-Pt 0.25 V3 / Al2O3]]> 218 237 246 Example 3 <![CDATA[F3-Pt 0.25 V3 / Al2O3]]> 175 203 215 Example 4 <h2 style=";text-align:left;direction:ltr"><![CDATA[F-Pt <h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> V1 / Al2O3<h2 style=";text-align:left;direction:ltr"> 191 223 228 Example 5 <h2 style=";text-align:left;direction:ltr"><![CDATA[F-Pt <h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> V5 / Al2O3<h2 style=";text-align:left;direction:ltr"> 158 199 206 Example 6 <h2 style=";text-align:left;direction:ltr"><![CDATA[F-Pt <h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> V7 / Al2O3<h2 style=";text-align:left;direction:ltr"> 173 205 210 Example 7 <![CDATA[F-Pt 0.25 V 10 / Al2O3]]> 178 207 215 Example 8 <![CDATA[F4-Pt 0.25 V3 / Al2O3]]> 167 206 220 Example 9 <![CDATA[F5-Pt 0.25 V3 / Al2O3]]> 162 206 215 Comparative Example 1 <h2 style=";text-align:left;direction:ltr"><![CDATA[F-Pt <h2 style=";text-align:left;direction:ltr"> 0.25 <h2 style=";text-align:left;direction:ltr"> / Al2O3]]><h2 style=";text-align:left;direction:ltr"> 192 212 216 Comparative Example 2 <![CDATA[F6-Pt 0.25 V3 / Al2O3]]> 195 226 235 Comparative Example 3 <![CDATA[F7-Pt 0.25 V3 / Al2O3]]> 189 220 227
[0091] Table 2
[0092]
[0093]
[0094] The test results show that:
[0095] (1) It can be seen from Examples 1-9 and Comparative Examples 1-3 that the present invention uses a one-step impregnation method and uses oxalic acid to dissolve the vanadium source to directly load the platinum source and the vanadium source onto the surface of the alumina carrier at the same time, and controls the interaction between the carrier and the active component by adjusting the vanadium content, thereby finally obtaining a catalyst with excellent CO oxidation ability.
[0096] (2) Through Example 1, Examples 4-7 and Comparative Example 1, the present invention controls the molar ratio of platinum to vanadium to prepare a sulfur-resistant catalyst having more excellent sulfur resistance and higher activity. The present invention controls the amount of vanadium to further improve the ability of the catalyst to resist sulfur poisoning and further optimize the catalytic effect of the catalyst. The introduction of a lower content of vanadium cannot fully exert the role of the sacrificial agent, while the introduction of an excessively high content will lead to the accumulation of more sulfate on the carrier, thereby blocking the active sites.
[0097] (3) It can be seen from Example 1 and Examples 8-9 that the sulfur-resistant catalyst prepared by controlling the sintering temperature of the present invention has excellent sulfur resistance and high activity. When the sintering temperature is high, the Pt and V impregnated on Al2O3 agglomerate, resulting in a reduction in active sites, thereby reducing the sulfur resistance and catalytic activity; when the sintering temperature is low, it is not enough to remove the impurities contained in the platinum source and the vanadium source, which may reduce the sulfur resistance and inhibit the catalytic activity.
[0098] In summary, the present invention adopts an impregnation method and utilizes oxalic acid to dissolve the vanadium source. Capillary pressure is generated by surface tension, so that the mixed solvent penetrates into the interior of the solid alumina, eliminating the step of catalyst molding. At the same time, the present application directly loads the platinum source and the vanadium source onto the surface of the alumina carrier at the same time through a one-step impregnation method. The production process is clean, the cost is low, and the application prospects are broad. The prepared sulfur-poisoning-resistant catalyst, platinum is the main active component of the catalyst, and vanadium acts as a sacrificial agent to adsorb sulfur oxides, thereby protecting the active site platinum, thereby ensuring the high activity of the catalyst. Therefore, the catalyst prepared by the present invention has excellent sulfur resistance and high activity.
[0099] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention are within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a sulfur-poisoning resistant catalyst, characterized in that: The preparation method comprises: Under stirring conditions, a platinum source, a vanadium source, oxalic acid, aluminum oxide and a solvent are mixed to obtain a suspension; after the suspension is dried and sintered, the sulfur-poisoning-resistant catalyst is obtained.
2. The preparation method according to claim 1, characterized in that: The platinum source includes tetraammine platinum nitrate; Preferably, the mass of the platinum source accounts for 0.1-0.5% of the mass of the aluminum oxide.
3. The preparation method according to claim 1 or 2, characterized in that: The vanadium source includes ammonium metavanadate; Preferably, the mass of the vanadium source accounts for 1-25% of the mass of the aluminum oxide; Preferably, the solvent comprises deionized water.
4. The preparation method according to any one of claims 1 to 3, characterized in that The mixing temperature is 30-40°C; Preferably, the mixing order is: first mix the solvent and the platinum source, then mix the vanadium source and oxalic acid, and finally mix the aluminum oxide.
5. The preparation method according to any one of claims 1 to 4, characterized in that: The stirring speed is 200-400 rpm; Preferably, the stirring time is 2-4 hours.
6. The preparation method according to any one of claims 1 to 5, characterized in that: The drying step includes drying after removing moisture; Preferably, the drying temperature is 100-120°C; Preferably, the drying time is 8-16 hours.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The sintering temperature is 400-600°C; Preferably, the sintering time is 2-4 hours.
8. The preparation method according to claim 1, characterized in that: The preparation method comprises the following steps: Dissolve the platinum source in deionized water at 30-40°C, then add the vanadium source and oxalic acid, and after all are dissolved, add aluminum oxide and stir to obtain a suspension; The suspension is dehydrated and dried at 100-120° C. for 8-16 hours to obtain a dried material; The dried material is sintered at 400-600° C. for 2-4 hours to obtain the sulfur-poisoning resistant catalyst.
9. A sulfur-poisoning resistant catalyst prepared by the preparation method according to any one of claims 1 to 8, characterized in that: The sulfur-poisoning resistant catalyst uses aluminum oxide as a carrier and carries platinum and vanadium.
10. An application of the sulfur-poisoning resistant catalyst as claimed in claim 9, characterized in that: The sulfur-poisoning resistant catalyst is applied to the catalytic oxidation of carbon monoxide.
Citation Information
Patent Citations
Process for purification of exhaust gas of diesel engines
CN1052262A
Titanium modified cerium vanadate catalyst as well as preparation method and application thereof
CN114682246A
Sulfur poisoning-resistant VOCs catalyst as well as preparation method and application thereof
CN116099542A
Synergistic purification titanium-based catalyst as well as preparation method and application thereof
CN118022717A
Preparation method of denitration catalyst for effectively inhibiting oxidation of sulfur dioxide
WO2015158139A1