CO catalyst and production method and application thereof
By using titanium dioxide, lanthanum oxide and cerium oxide as support and supporting tungsten and platinum CO catalysts, the problem of poor catalytic effect of CO catalysts in the prior art under high water and high sulfur environments has been solved, and efficient CO conversion and Good water and sulfur resistance.
Patent Information
- Application Number
- CN202411072106.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
The existing CO catalysts have poor catalytic effects under sulfur-containing and water-containing conditions, especially poor water-resistant and sulfur-resistant properties, resulting in low CO conversion.
The CO catalyst with the support being titanium dioxide, lanthanum oxide and cerium oxide is loaded with tungsten and platinum, and is prepared by ball milling, calcining and drying, so as to optimize the mass ratio and particle size of the support and metal loads, and improve the sulfur and water resistance of the catalyst.
Under the conditions of 200-300°C, the CO catalyst exhibits high conversion and excellent sulfur and water resistance, and is suitable for CO oxidation reactions in high water and high sulfur environments.
Smart Images

Figure BDA0004981153150000111
Abstract
Description
Technical Field
[0001] The invention relates to a CO catalyst and a production method and application thereof. Background Art
[0002] Catalytic oxidation refers to the oxidation of CO to CO2 under the action of a catalyst, thereby eliminating CO in the environment. Currently, catalytic oxidation is considered to be one of the effective methods for eliminating CO.
[0003] CN109569678A discloses a carbon monoxide catalyst, comprising an active component, a carrier, an active aid and a molding aid. The active component is selected from any one of Pt, Pd and Ru. The carrier is pseudo-boehmite or γ-Al2O3. The active aid is selected from any one of FePO4, LaPO4 or PrPO4. The molding aid is selected from one or both of calcium oxide and magnesium oxide. The catalyst has poor water resistance and sulfur resistance.
[0004] CN101530796A discloses a low-temperature CO catalytic oxidation catalyst, comprising an active component and a carrier, wherein the active component is gold, and the carrier is a mixture of any two of NaZSM-5, MCM-41, NaY, 13X, and 5A molecular sieves in any mass ratio. The catalyst has a relatively low operating temperature.
[0005] CN117819773A discloses an integral carbon monoxide catalyst, comprising a carrier and metal catalytic particles loaded on the surface of the carrier; the loading amount of the metal catalytic particles is 90-150 kg / m 3 The metal catalytic particles include at least one of titanium particles, cerium particles, cobalt particles, nickel particles, ruthenium particles, rhodium particles, palladium particles, iridium particles, platinum particles, and molybdenum particles; and the carrier includes at least one of cordierite, honeycomb, and hierarchical porous carbon. The catalytic effect of the carbon monoxide catalyst is poor. Summary of the invention
[0006] In view of this, an object of the present invention is to provide a CO catalyst, which has a high conversion rate for CO under sulfur-containing and water-containing conditions. Another object of the present invention is to provide a method for producing CO. Another object of the present invention is to provide a use of a CO catalyst.
[0007] On the one hand, the present invention provides a CO catalyst, including a carrier and tungsten and platinum loaded on the carrier; the carrier includes titanium dioxide, lanthanum oxide and cerium oxide, and the mass ratio of titanium dioxide, lanthanum oxide and cerium oxide is (6-10): (0.5-2.5):1.
[0008] According to the CO catalyst of the present invention, preferably, based on the weight of the CO catalyst, the loading amount of platinum is 0.05-0.5 wt%, and the loading amount of tungsten is 0.5-3 wt%.
[0009] According to the CO catalyst of the present invention, preferably, the particle size of the carrier is 1 to 15 μm.
[0010] In another aspect, the present invention provides a method for producing the above-mentioned CO catalyst, comprising the following steps:
[0011] (1) ball-milling titanium dioxide, lanthanum oxide and cerium oxide to obtain ball-milled oxides; calcining the ball-milled oxides at 400 to 600° C. to obtain calcined products; cooling the calcined products and grinding them to obtain a carrier;
[0012] (2) stirring the carrier, the water-soluble tungsten-containing inorganic salt and water at 50 to 75° C., and then drying to obtain a first intermediate product;
[0013] (3) stirring the first intermediate product, a water-soluble platinum-containing inorganic salt and water at 50 to 75° C., and then drying to obtain a second intermediate product;
[0014] (4) The second intermediate product is calcined at 400-600° C. to obtain a CO catalyst.
[0015] According to the production method of the present invention, preferably, in step (1), the calcination time is 1 to 5 hours, and the heating rate to the calcination temperature is 2 to 8°C / min;
[0016] In step (4), the calcination time is 1 to 5 hours, and the heating rate to the calcination temperature is 2 to 8°C / min.
[0017] In yet another aspect, the present invention provides use of the above CO catalyst in catalytic oxidation of carbon monoxide.
[0018] According to the use of the present invention, preferably, the CO catalyst is used at a temperature of 200 to 300°C.
[0019] According to the use of the present invention, preferably, the carbon monoxide exists in a gaseous substance, and the content of carbon monoxide in the gaseous substance is 6000-15000 mg / Nm 3 .
[0020] According to the use of the present invention, preferably, the gaseous substance also contains SO2 and / or water; the content of SO2 is 50-150 ppm, and the content of water is 10-40 vol%.
[0021] According to the use of the present invention, preferably, the gaseous substance further contains one or more of NO, NO2, CO2, and O2; the content of NO is 100 to 800 mg / Nm 3 , the content of NO2 is 2 to 100 mg / Nm 3 , the content of CO2 is 10 to 30 vol%, and the content of O2 is 1 to 20 vol%.
[0022] The catalyst of the present invention has excellent sulfur and water resistance performance and still has a high conversion rate for CO under sulfur- and water-containing conditions. The catalyst of the present invention has excellent performance at 200 to 300 °C. Specific Embodiments
[0023] The present invention will be further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0024] <CO Catalyst>
[0025] The CO catalyst of the present invention includes a carrier and tungsten and platinum supported on the carrier. Tungsten can be supported on the carrier in the form of an oxide or in the form of an element. Platinum can be supported on the carrier in the form of an oxide or in the form of an element.
[0026] The carrier includes titanium dioxide, lanthanum oxide, and cerium oxide. Preferably, the carrier is composed of titanium dioxide, lanthanum oxide, and cerium oxide. Titanium dioxide is preferably anatase titanium dioxide.
[0027] The mass ratio of titanium dioxide to cerium oxide is (6 to 10):1; preferably (7 to 9):1; more preferably (8 to 8.5):1.
[0028] The mass ratio of lanthanum oxide to cerium oxide is (0.5 to 2.5):1; preferably (0.8 to 2):1; more preferably (1 to 1.5):1.
[0029] The carrier composed of titanium dioxide, lanthanum oxide, and cerium oxide in an appropriate mass ratio can improve the water and sulfur resistance performance of the catalyst and improve the catalytic performance of the catalyst under medium-temperature conditions.
[0030] Based on the weight of the CO catalyst, the loading amount of platinum can be 0.05 to 0.5 wt%; preferably 0.08 to 0.3 wt%; more preferably 0.1 to 0.2 wt%. The loading amount of platinum is calculated based on the mass of platinum element. This can improve the catalytic performance of the catalyst and reduce the cost.
[0031] Based on the weight of the CO catalyst, the tungsten loading can be 0.5 to 3 wt%; preferably 0.8 to 2 wt%; more preferably 1 to 1.5 wt%. The tungsten loading is based on the mass of tungsten element. An appropriate amount of tungsten in combination with platinum can improve the catalytic performance and, in combination with the support, improve the water and sulfur resistance of the catalyst.
[0032] The particle size of the support can be 1 to 15 μm. This can increase the specific surface area of the catalyst and reduce agglomeration.
[0033] <Production method of the CO catalyst>
[0034] The production method of the catalyst of the present invention includes the following steps: (1) a step of preparing a support; (2) a step of loading tungsten; (3) a step of loading platinum; and (4) a step of calcination.
[0035] Steps for preparing the vector
[0036] Milling titanium dioxide, lanthanum oxide and cerium oxide to obtain milled oxides; calcining the milled oxides at 400 to 600 °C to obtain a calcined product; grinding the calcined product after cooling to obtain a support.
[0037] The ball-to-material ratio can be (0.5 to 2):1; preferably (0.8 to 1.5):1; more preferably (1 to 1.2):1. This helps to obtain a support with an appropriate particle size and form a solid solution.
[0038] The milling time can be 0.5 to 2 h; preferably 0.8 to 1.5 h; more preferably 1 to 1.2 h.
[0039] The particle size of the milled oxides can be 1 to 15 μm.
[0040] The calcination temperature can be 400 to 600 °C; preferably 450 to 550 °C; more preferably 480 to 500 °C.
[0041] The calcination time can be 1 to 5 h; preferably 2 to 4 h; more preferably 3 to 3.5 h.
[0042] The heating rate for raising the temperature to the calcination temperature can be 2 to 8 °C / min; preferably 3 to 7 °C / min; more preferably 4 to 5 °C / min.
[0043] Tungsten Loading Steps
[0044] Stir the support, water-soluble tungsten-containing inorganic salt and water at 50 to 75 °C, and then dry to obtain a first intermediate product.
[0045] Based on 20g of the carrier, the amount of the water-soluble tungsten-containing inorganic salt can be 0.05-1g, preferably 0.1-0.5g, and more preferably 0.2-0.3g. The water-soluble tungsten-containing inorganic salt can be ammonium metatungstate.
[0046] Based on 20 g of the carrier, the amount of water used can be 10 to 150 g, preferably 40 to 100 g, and more preferably 60 to 80 g.
[0047] Preferably, the carrier, the water-soluble tungsten-containing inorganic salt and water are stirred at 55-70° C. More preferably, the carrier, the water-soluble tungsten-containing inorganic salt and water are stirred at 60-65° C. The above temperature can be reached by heating in a water bath.
[0048] The drying temperature may be 90 to 130° C., preferably 100 to 120° C., and more preferably 110 to 115° C. The drying time may be 7 to 15 hours, preferably 10 to 14 hours, and more preferably 12 to 13 hours.
[0049] Platinum loading steps
[0050] The first intermediate product, a water-soluble platinum-containing inorganic salt and water are stirred at 50-75° C. and then dried to obtain a second intermediate product.
[0051] Based on 20g of the carrier, the amount of the water-soluble platinum-containing inorganic salt is 0.005-0.1g, preferably 0.01-0.05g, and more preferably 0.02-0.03g. The water-soluble platinum-containing inorganic salt is preferably chloroplatinic acid.
[0052] Based on 20 g of the carrier, the amount of water used can be 10 to 150 g, preferably 40 to 100 g, and more preferably 60 to 80 g.
[0053] Preferably, the first intermediate product, the water-soluble platinum-containing inorganic salt and water are stirred at 55-70° C. More preferably, the first intermediate product, the water-soluble platinum-containing inorganic salt and water are stirred at 60-65° C. The above temperature can be reached by heating in a water bath.
[0054] The drying temperature may be 90 to 130° C., preferably 100 to 120° C., and more preferably 110 to 115° C. The drying time may be 7 to 15 hours, preferably 10 to 14 hours, and more preferably 12 to 13 hours.
[0055] Roasting steps
[0056] The second intermediate product is calcined at 400-600° C. to obtain a CO catalyst.
[0057] The calcination temperature can be 400 - 600 °C; preferably 450 - 550 °C; more preferably 480 - 500 °C.
[0058] The calcination time can be 1 - 5 h; preferably 1.5 - 4 h; more preferably 2 - 3 h.
[0059] The heating rate for raising the temperature to the calcination temperature can be 2 - 8 °C / min; preferably 3 - 7 °C / min; more preferably 4 - 5 °C / min.
[0060] <Use of the CO catalyst>
[0061] The catalyst of the present invention has good catalytic oxidation effect on CO in an environment with high water and high sulfur. Therefore, the present invention provides the use of the above CO catalyst in the catalytic oxidation of carbon monoxide.
[0062] The use temperature of the CO catalyst can be 200 - 300 °C; preferably 220 - 280 °C; more preferably 240 - 260 °C. The catalyst of the present invention has good catalytic oxidation performance at the above temperatures.
[0063] Carbon monoxide can exist in gaseous substances. The gaseous substances are, for example, flue gas. The content of carbon monoxide in the gaseous substances can be 6000 - 15000 mg / Nm 3 ; preferably 8000 - 13000 mg / Nm 3 ; more preferably 10000 - 11000 mg / Nm 3 .
[0064] The gaseous substances may also contain SO2 and / or water. The content of SO2 can be 50 - 150 ppm; preferably 70 - 130 ppm; more preferably 100 - 110 ppm. The content of water can be 10 - 40 vol%; preferably 15 - 30 vol%; more preferably 20 - 25 vol%.
[0065] In some embodiments, the gaseous substances also contain NO. The content of NO can be 100 - 800 mg / Nm 3 ; preferably 200 - 600 mg / Nm 3 ; more preferably 300 - 400 mg / Nm 3 .
[0066] In some embodiments, the gaseous substances also contain NO2. The content of NO2 can be 2 - 100 mg / Nm 3 ; preferably 10 - 50 mg / Nm 3 ; more preferably 20 - 30 mg / Nm 3 .
[0067] In some embodiments, the gaseous substance further contains CO2. The content of CO2 may be 10-30 vol%, preferably 15-25 vol%, and more preferably 20-22 vol%.
[0068] In some embodiments, the gaseous substance further contains O2. The content of O2 may be 1 to 20 vol%, preferably 10 to 18 vol%, and more preferably 15 to 16 vol%.
[0069] The gaseous material containing carbon monoxide may be contacted with the CO catalyst in a fixed bed reactor.
[0070] The airspeed can be 10000~30000h -1 ; preferably 15000~25000h -1 ; More preferably 18000~22000h -1 .
[0071] Here is the test method:
[0072] The simulated gas and catalyst were placed in a fixed bed reactor at a temperature of 240 °C and a space velocity of 20000 h -1 The content of CO in the outlet gas was tested under the conditions of . The content of each component in the simulated gas distribution and outlet gas was tested using a flue gas analyzer. The conversion rate of CO was calculated using the following formula:
[0073] Conversion rate = (C CO入口 -C CO出口 ) / C CO入口 ×100%
[0074] Among them, C CO入口 Indicates the CO content in the simulated gas distribution; C CO出口 Indicates the CO content in the outlet gas.
[0075] The simulated gas composition is: NO 300mg / Nm 3 , NO2 20mg / Nm 3 ,CO 10000mg / Nm 3 , CO2 20vol%, O216vol%, H2O 20vol%, SO2 100ppm.
[0076] Example 1
[0077] (1) Anatase titanium dioxide, lanthanum oxide and cerium oxide in a mass ratio of 8:1:1 were mixed uniformly, and then ball-milled in a ball mill for 1 hour to obtain a ball-milled oxide. The ball-to-material ratio was 1:1. The particle size of the ball-milled oxide was 1 to 15 μm. The ball-milled oxide was calcined in a muffle furnace at 500°C for 3 hours to obtain a calcined product. The heating rate was 5°C / min. The calcined product was cooled and ground to obtain a carrier with a particle size of 1 to 15 μm.
[0078] (2) 20 g of the carrier, 0.27 g of ammonium metatungstate and 70 g of water were heated in a water bath at 65° C., stirred until the water was evaporated, and then dried at 110° C. for 12 h to obtain a first intermediate product.
[0079] (3) The first intermediate product, 0.02 g of chloroplatinic acid and 70 g of water were heated in a water bath at 65° C., stirred until the water was evaporated, and then dried at 110° C. for 12 h to obtain a second intermediate product.
[0080] (4) The second intermediate product was calcined in a muffle furnace at 500° C. for 2 h to obtain a CO catalyst. The heating rate was 5° C. / min.
[0081] Based on the weight of the CO catalyst, the loading amount of platinum is 0.1 wt %, and the loading amount of tungsten is 1 wt %. The loading amount of platinum is calculated based on the mass of the platinum element, and the loading amount of tungsten is calculated based on the mass of the tungsten element.
[0082] The conversion rates of CO by the catalysts are shown in Table 1.
[0083] Comparative Example 1
[0084] Except that step (3) is different from embodiment 1, the rest is the same as embodiment 1. Step (3) is as follows:
[0085] The first intermediate product, chloroplatinic acid, palladium chloride and water are heated in a water bath at 65° C., stirred until the water is evaporated, and then dried at 110° C. for 12 hours to obtain a second intermediate product.
[0086] Based on the weight of the CO catalyst, the loading amount of platinum is 0.75wt%, the loading amount of palladium is 0.25wt%, and the loading amount of tungsten is 1wt%. The loading amount of platinum is calculated based on the mass of the platinum element, the loading amount of palladium is calculated based on the mass of the palladium element, and the loading amount of tungsten is calculated based on the mass of the tungsten element.
[0087] The conversion rates of CO by the catalysts are shown in Table 1.
[0088] Comparative Example 2
[0089] The same procedures as in Example 1 are followed except that anatase titanium dioxide, lanthanum oxide and cerium oxide are replaced by anatase titanium dioxide, aluminum oxide and manganese dioxide in a mass ratio of 8:1:1.
[0090] The conversion rates of CO by the catalysts are shown in Table 1.
[0091] Comparative Example 3
[0092] Except that the calcination temperature in step (4) is 350° C., the rest is the same as in Example 1.
[0093] The conversion rates of CO by the catalysts are shown in Table 1.
[0094] Comparative Example 4
[0095] The same procedures as in Example 1 are followed except that anatase titanium dioxide, lanthanum oxide and cerium oxide are replaced by anatase titanium dioxide and cerium oxide in a mass ratio of 8:2.
[0096] The conversion rates of CO by the catalysts are shown in Table 1.
[0097] Comparative Example 5
[0098] Except that ammonium metatungstate is replaced by ammonium molybdate, and in the obtained CO catalyst, based on the weight of the CO catalyst, the platinum loading is 0.1wt%, the molybdenum loading is 1wt%, the platinum loading is based on the mass of the platinum element, and the molybdenum loading is based on the mass of the molybdenum element, the rest is the same as Example 1.
[0099] The conversion rates of CO by the catalysts are shown in Table 1.
[0100] Comparative Example 6
[0101] The same procedures as in Example 1 are the same except that the amount of ammonium metatungstate used is different from that in Example 1 and the loading amount of tungsten is 0.2 wt %.
[0102] The conversion rates of CO by the catalysts are shown in Table 1.
[0103] Comparative Example 7
[0104] Except that the amount of ammonium metatungstate used is different from that in Example 1 and the loading amount of tungsten is 5 wt %, the rest is the same as in Example 1.
[0105] The conversion rates of CO by the catalysts are shown in Table 1.
[0106] Comparative Example 8
[0107] Except that the particle size of the oxide after ball milling is 20-50 μm and the particle size of the carrier is 20-50 μm, the rest is the same as Example 1.
[0108] The conversion rates of CO by the catalysts are shown in Table 1.
[0109] Comparative Example 9
[0110] Except that the particle size of the oxide after ball milling is <0.3 μm and the particle size of the carrier is <0.8 μm, the rest is the same as Example 1.
[0111] The conversion rates of CO by the catalysts are shown in Table 1.
[0112] Table 1
[0113]
[0114] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A CO catalyst, It is characterized in that The CO catalyst comprises a carrier and tungsten and platinum loaded on the carrier; the carrier comprises titanium dioxide, lanthanum oxide and cerium oxide, and the mass ratio of titanium dioxide, lanthanum oxide and cerium oxide is (6-10): (0.5-2.5):
1.
2. The CO catalyst according to claim 1, It is characterized in that Based on the weight of the CO catalyst, the loading amount of platinum is 0.05-0.5wt%, and the loading amount of tungsten is 0.5-3wt%.
3. The CO catalyst according to claim 1, It is characterized in that The particle size of the carrier is 1 to 15 μm.
4. The method for producing a CO catalyst according to any one of claims 1 to 3, It is characterized in that The steps include: (1) ball-milling titanium dioxide, lanthanum oxide and cerium oxide to obtain ball-milled oxides; calcining the ball-milled oxides at 400 to 600° C. to obtain calcined products; cooling the calcined products and grinding them to obtain a carrier; (2) stirring the carrier, the water-soluble tungsten-containing inorganic salt and water at 50 to 75° C., and then drying to obtain a first intermediate product; (3) stirring the first intermediate product, a water-soluble platinum-containing inorganic salt and water at 50 to 75° C., and then drying to obtain a second intermediate product; (4) The second intermediate product is calcined at 400-600° C. to obtain a CO catalyst.
5. The production method according to claim 4, Features: In step (1), the calcination time is 1 to 5 hours, and the heating rate to the calcination temperature is 2 to 8°C / min; In step (4), the calcination time is 1 to 5 hours, and the heating rate to the calcination temperature is 2 to 8°C / min.
6. Use of the CO catalyst according to any one of claims 1 to 3 in catalytic oxidation of carbon monoxide.
7. The use according to claim 6, It is characterized in that The operating temperature of the CO catalyst is 200-300°C.
8. The use according to claim 6, It is characterized in that The carbon monoxide exists in the gaseous substance, and the content of carbon monoxide in the gaseous substance is 6000-15000 mg / Nm 3 .
9. The use according to claim 8, It is characterized in that The gaseous substance also contains SO 2 and / or water; SO 2 The content of is 50-150ppm, and the content of water is 10-40vol%.
10. The use according to claim 9, It is characterized in that The gaseous substance also contains NO, NO 2 , CO 2 and O 2 One or more of; NO content is 100~800mg / Nm 3 , NO 2 The content is 2~100mg / Nm 3 , CO 2 The content of O is 10~30vol% 2 The content is 1 to 20 vol%.
Citation Information
Patent Citations
CO removing catalyst as well as preparation method and use thereof
CN101371984A
Catalytic purification method of carbon monoxide-containing waste gas
CN107511065A
Pt-based catalyst for CO purification as well as preparation method and application of the Pt-based catalyst
CN111185167A
Carbon monoxide catalyst as well as preparation method and application thereof
CN114950469A
Catalyst, preparation method and application thereof, and flue gas treatment method
CN115155610A
Cited By
Preparation method and application of sulfur-resistant catalyst for low-temperature high-concentration CO treatment
CN123079356A