Copper slag ozone catalyst as well as preparation method and application thereof
By preparing an EDTA-CBC/HCS catalyst, the problems of low ozone utilization and difficulty in heavy metal recovery when using ozone catalysts to treat cyanide wastewater were solved, achieving efficient removal of cyanide and heavy metals from wastewater and reducing treatment costs.
Patent Information
- Application Number
- CN202411068297.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-06
AI Technical Summary
In existing technologies, ozone catalysts suffer from low ozone utilization, poor selectivity, and insufficient treatment depth when treating cyanide wastewater. Furthermore, copper ion catalysts are not easy to recover, resulting in high treatment costs and making it difficult to meet national emission standards.
EDTA-CBC was prepared by EDTA-Fe,Na-phosphoric acid activation and then loaded onto modified copper slag to prepare a copper slag ozone catalyst EDTA-CBC/HCS. Through the synergistic effect of modified copper slag and EDTA-CBC, the selectivity and catalytic efficiency of ozone were improved, achieving efficient removal of cyanide and heavy metal ions from wastewater.
It achieved a maximum removal rate of 98.71% for total cyanide in wastewater, while reducing the residual concentration of heavy metals copper and zinc, improving ozone utilization and catalyst recovery efficiency, and reducing water treatment costs.
Smart Images

Figure CN118976499A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preparation, and in particular to a copper slag ozone catalyst and a preparation method and application thereof. Background Art
[0002] Cyanide is a widely used complexing particle with super strong complexing ability. After CN- enters the human body, it reacts with gastric acid to form highly toxic hydrogen cyanide. Hydrogen cyanide reacts with Fe in oxidase in body fluids. 3+ Combined with iron, cyanide forms an extremely stable complex, which causes hypoxia in human organs. At the same time, cyanide can also generate thiocyanate compounds in the human body, causing chronic poisoning.
[0003] At present, the treatment method for cyanide wastewater includes homogeneous treatment method and heterogeneous treatment method, the homogeneous treatment method includes oxidation method and complex method, and the heterogeneous treatment method includes ozone oxidation method, activated carbon-oxygen heterogeneous catalytic oxidation method, liquid membrane oxidation method and ion exchange method. Among them, hydrogen peroxide oxidation method is suitable for treating low-concentration cyanide wastewater, and has the characteristics of fast reaction speed, but the hydrogen peroxide and metal ion catalyst used in this method are expensive, the treatment cost is high and the copper ion catalyst is not easy to recover. When the complex method treats cyanide wastewater, the generated iron blue precipitate cannot be completely filtered and removed, resulting in insufficient treatment depth, high residual cyanide content, and cannot meet national emission standards. Ozone oxidation method does not introduce secondary pollution during the treatment process, but the ozone utilization rate is low and the treatment depth is insufficient. In addition, the ozone catalytic reaction has a certain selectivity and poor decomposition ability for certain substances. Therefore, in order to enhance the treatment effect, a catalyst for catalytic ozonation is often used.
[0004] In the prior art, CN106396205A discloses a method for removing heavy metals from high-concentration cyanide wastewater by breaking cyanide, including electrolyzing high-concentration cyanide wastewater with direct current under alkaline conditions, adding hydrogen peroxide to promote its reaction speed, electrolyzing to obtain low-concentration cyanide wastewater, adjusting the pH of low-concentration cyanide wastewater to 10-11, adding EDTA and catalyst reaction, adding hydrogen peroxide for deep cyanide breaking treatment, and finally using ferrite method to remove heavy metals in solution. The above patent uses hydrogen peroxide and EDTA to improve electrolysis efficiency, but the EDTA used is difficult to degrade and extremely difficult to biochemically treat. At the same time, EDTA is also not easy to be directly fixed on the surface of activated carbon.
[0005] Therefore, an ozone catalyst is needed for ozone treatment of cyanide wastewater to improve the selectivity of ozone, thereby improving the degradation effect of cyanide and heavy metal ions in the wastewater. Summary of the invention
[0006] In view of the above-mentioned prior art, the purpose of the present invention is to provide a copper slag ozone catalyst. The present invention adopts EDTA-Fe, Na-phosphoric acid activation method to prepare EDTA-CBC, and loads it on modified copper slag to prepare copper slag ozone catalyst EDTA-CBC / HCS. Specifically, sodium iron ethylenediaminetetraacetate (EDTA-Fe, Na) is selected as a modifier for modifying CBC to obtain EDTA-CBC, and then EDTA-CBC is mixed with HCS, and then calcined after adding a binder to obtain a copper slag ozone catalyst. The copper slag ozone catalyst prepared by the present invention is used to treat total cyanide, copper and zinc in wastewater with ozone, and the removal rate of total cyanide in wastewater can reach up to 98.71%. At the same time, the concentrations of residual copper and zinc in the wastewater are 0.448 and 0.032 mg / L, respectively.
[0007] To achieve the above object, the present invention adopts the following technical solution:
[0008] The first aspect of the present invention provides a copper slag ozone catalyst, which is prepared from a carrier and an active component, wherein the carrier is modified copper slag (HCS) and the active component is EDTA-modified coconut shell ash (EDTA-CBC); the mass ratio of the carrier to the active component is (0.5-3):1.
[0009] Preferably, the modified copper slag (HCS) is prepared by the following method: washing and drying copper slag particles and then calcining to obtain modified copper slag; the calcination temperature is 700-750° C. and the calcination time is 4-4.5 h.
[0010] Preferably, the particle size of the copper slag particles is 150-200 mesh.
[0011] Preferably, the washing operation is: stirring and washing the copper slag particles with deionized water for 10-15 minutes, and repeating the operation 2-3 times.
[0012] Preferably, the drying temperature is 105-120° C. and the drying time is 10-12 h.
[0013] Preferably, the calcination temperature is 700-750°C, the calcination time is 4-4.5h, and the heating rate during the calcination process is 10°C / min. More preferably, the calcination temperature is 722°C, and the calcination time is 4.32h.
[0014] Preferably, the EDTA-modified coconut shell ash is prepared by the following method: coconut shell ash (CBC) and sodium ferric ethylenediaminetetraacetate (EDTA-Fe, Na) are mixed, and then immersed in a phosphoric acid solution to obtain a sample, and the sample is placed in an inert gas for activation, and cooled to room temperature to obtain EDTA-modified coconut shell ash (EDTA-CBC).
[0015] Preferably, the material-liquid ratio of coconut shell ash to sodium ferric ethylenediaminetetraacetate is 1 g: (1-5) mmol.
[0016] Further preferably, the solid-liquid ratio of coconut shell ash to sodium ferric ethylenediaminetetraacetate is 1 g:3 mmol.
[0017] Preferably, the concentration of the phosphoric acid solution is 85 wt %.
[0018] Preferably, the mass ratio of coconut shell ash to phosphoric acid solution is 1:3.
[0019] Preferably, the immersion time is 8-12 hours, and more preferably, the immersion time is 10 hours.
[0020] Preferably, N2 is selected as the inert gas.
[0021] Preferably, the activation temperature is 300-800°C, the activation time is 1-6h, and the heating rate is controlled at 10°C / min during the activation process; further preferably, the activation temperature is 600°C, and the activation time is 2h.
[0022] The second aspect of the present invention provides a method for preparing a copper slag ozone catalyst, comprising the following steps:
[0023] The modified copper slag, EDTA-CBC and the binder are mixed, put into water and mixed evenly to obtain a binder, the binder is calcined, ground and sieved to obtain the copper slag ozone catalyst (EDTA-CBC / HCS).
[0024] Preferably, the mass ratio of EDTA-CBC to modified copper slag is 1:(0.5-3).
[0025] Preferably, the mass ratio of the total mass of the modified copper slag and EDTA-CBC to the binder is 100:1.
[0026] Preferably, the mass ratio of the total mass of the modified copper slag, EDTA-CBC and the binder to the mass ratio of water is 1:1.
[0027] Preferably, the binder is hydroxypropyl methylcellulose (HPMC).
[0028] Preferably, the operation of calcining the binder is: placing the binder in a N2 atmosphere and calcining at 500-600°C for 1.5-2.5h.
[0029] Preferably, the powder is ground through a 100 mesh screen.
[0030] A third aspect of the present invention provides an application of a copper slag ozone catalyst in catalytic ozone treatment of cyanide and heavy metal ions in wastewater.
[0031] Preferably, the heavy metal ions are copper ions and / or zinc ions.
[0032] Beneficial effects of the present invention:
[0033] The present invention adopts EDTA-Fe, Na-phosphoric acid activation method to prepare EDTA-CBC, and loads it on HCS to prepare EDTA-CBC / HCS catalyst. Specifically, ethylenediaminetetraacetic acid sodium iron (EDTA-Fe, Na) is selected as a modifier to modify CBC to prepare EDTA-CBC, and then EDTA-CBC is mixed with HCS, and then calcined after adding a binder to obtain a copper slag ozone catalyst. The copper slag ozone catalyst prepared by the present invention is mainly used for ozone treatment of total cyanide, copper and zinc in wastewater by chemical adsorption, and the removal rate of total cyanide in wastewater can reach up to 98.71%. At the same time, the concentrations of residual copper and zinc in the wastewater are 0.448 mg / L and 0.032 mg / L respectively.
[0034] The present invention obtains EDTA-CBC by mixing EDTA and CBC and placing them in a phosphoric acid solution for immersion activation. During the preparation process, the optimal activation temperature is guaranteed to be 600° C. and the optimal activation time is 2 hours. Under this activation temperature and time, EDTA-Fe, Na is guaranteed to be completely decomposed. The functional groups generated by EDTA-Fe, Na during the decomposition process that are conducive to heavy metal capture are utilized, and the active sites are guaranteed to be fully exposed to improve the catalytic effect. The present invention prepares EDTA-CBC by using the EDTA-Fe, Na-phosphoric acid activation method, effectively avoiding the problem of EDTA being difficult to degrade, and also improving the catalytic effect of the finally obtained copper slag ozone catalyst.
[0035] In addition, the present invention modifies the copper slag so that the modified copper slag is magnetic, easy to recycle and has a high reuse efficiency. The modified copper slag combines with ozone through hydroxylation in an aqueous solution and realizes electron transfer through oxygen vacancies, thereby generating active oxygen species with higher oxidizing properties and improving catalytic efficiency. At the same time, it can also reduce the cost of ozone catalysts, improve ozone utilization, and ultimately reduce water treatment costs and large-scale solid waste resource utilization. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 :(a) The effect of the addition amount of EDTA-Fe, Na on the total cyanide removal rate; (b) The effect of the addition amount of EDTA-Fe, Na on the removal rates of copper and zinc;
[0037] Figure 2 :(a) Effect of activation temperature on total cyanide removal rate;(b) Effect of activation temperature on copper and iron removal rates;
[0038] Figure 3 :(a) Effect of activation time on total cyanide removal rate;(b) Effect of activation time on copper and zinc removal rates;
[0039] Figure 4 :(a) The effect of EDTA-CBC loading on total cyanide removal efficiency;(b) The effect of EDTA-CBC loading on copper and zinc removal efficiency;
[0040] Figure 5 :SEM images of EDTA-CBC and EDTA-CBC / HCS;
[0041] Figure 6 : (a) N2 adsorption-desorption isotherm of the copper slag ozone catalyst EDTA-CBC / HCS prepared in Example 2; (b) pore size distribution diagram;
[0042] Figure 7 : XRD patterns of CBC, HCS, EDTA-CBC and EDTA-CBC / HCS obtained in Example 2;
[0043] Figure 8 : FT-IR spectra of CBC, phosphoric acid-activated CBC and EDTA-CBC prepared in Example 2;
[0044] Fig. 9 :(a) Effect of ozone dosage concentration on total cyanide removal efficiency; (b) Effect of ozone dosage concentration on copper and zinc removal efficiency.
[0045] Fig.10 :(a) Effect of the addition concentration of copper slag ozone catalyst on the total cyanide removal rate in wastewater;(b) Effect of the addition concentration of copper slag ozone catalyst on the removal rate of copper and zinc in wastewater;
[0046] Fig.11 ; (a) Effect of initial solution pH on total cyanide removal efficiency; (b) Effect of initial solution pH on removal efficiency of copper and zinc; Relationship between pH change (c) and O3 concentration in solution (d);
[0047] Fig.12 :(a) Effect of reaction temperature on total cyanide removal rate in wastewater;(b) Effect of reaction temperature on copper and zinc removal rate in wastewater; Relationship between pH change (c) and O3 concentration in solution;(d) Kinetic fitting curves of catalytic ozonation at different temperatures;
[0048] Fig.13 :(a) Effect of cycle number on total cyanide removal efficiency in wastewater; (b) Effect of cycle number on copper and zinc removal efficiency in wastewater. DETAILED DESCRIPTION
[0049] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.
[0050] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in conjunction with specific embodiments.
[0051] Compared with homogeneous catalysts, heterogeneous catalysts have the advantages of simple manufacturing process, low cost, high catalytic activity, good mass transfer effect, and easy reuse. Ozone oxidation as a heterogeneous catalytic oxidation technology has been popularized, but there is a problem of low ozone utilization rate, and catalysts are needed to improve ozone utilization rate. At present, low-content metal active phase supported catalysts are widely used in industry, with a price of 8,000 to 15,000 yuan / ton, but the amount of active raw material components is not high.
[0052] Copper slag is a by-product of the pyrometallurgical smelting process of copper. The production of copper slag in my country has exceeded 16 million tons, and the amount of copper slag stored has exceeded 50 million tons. The low utilization rate of copper slag has caused resource waste and environmental safety hazards. The main components of copper slag are magnetite and iron vanadium, with an iron content of about 30-40%. Its high iron content makes copper slag a high value-added secondary resource.
[0053] Based on this, the present invention provides a copper slag ozone catalyst, which is prepared from a carrier and an active component, wherein the carrier is modified copper slag (HCS), and the active component is EDTA-modified coconut shell ash (EDTA-CBC). HCS has more metal active sites for catalyzing ozonation, while EDTA-CBC has a large specific surface area and abundant functional groups for capturing pollutants, and the final removal of pollutants such as cyanide is the result of the synergistic effect of the two. The present invention controls the mass ratio of EDTA-CBC and HCS, so that the prepared copper slag ozone catalyst can not only catalyze ozonation to degrade cyanide, but also adsorb and remove heavy metal ions well.
[0054] Among them, the present invention modifies the copper slag so that the modified copper slag is magnetic, easy to recycle and has a high reuse efficiency. The modified copper slag combines with ozone through hydroxylation in aqueous solution and realizes electron transfer through oxygen vacancies, thereby generating active oxygen species with higher oxidizing properties, improving the catalytic efficiency. At the same time, it can also reduce the cost of ozone catalysts, improve ozone utilization, and ultimately reduce water treatment costs and bulk solid waste resource utilization. The mechanism of ozone decomposition and oxidation catalyzed by modified copper slag mainly includes two aspects: when the solution pH is less than the zero isoelectric point of the copper slag catalyst, the metal ions on the surface of the copper slag combine with water to form a hydroxylation interface. Ozone and the hydroxyl groups on the surface of the copper slag transfer electrons through coordination bonds and hydrogen bonds to form a five-membered ring structure. The electron transfer destroys its stable conjugated structure, thereby decomposing the ozone molecules to generate a series of active oxygen species, including ·OH and superoxide radicals (·O -2 );Second, small molecular organic matter passes through the Fe 3+ Complexation reduces Fe 3+ / Fe 2+ The redox potential of ·OH and ·O -2 of production, thereby increasing the reaction rate.
[0055] The adsorption of cyanide, copper and zinc by the EDTA-CBC / HCS prepared in the present invention is mainly chemical adsorption. The EDTA-CBC / HCS catalytic O3 oxidation system follows the free radical law, and the active species involved in the reaction are ·OH, ·O -2 and 1 O2, and the process is accompanied by an increase in Fe valence, a decrease in adsorbed oxygen and bound oxygen, and a transformation of unsaturated functional groups to saturated forms. The removal of cyanide is the common result of direct and indirect oxidation by O3.
[0056] The main components of the copper slag used in the present invention are shown in the following table:
[0057]
[0058] The experimental materials used in the embodiments of the present invention are all conventional experimental materials in the art and can be purchased through commercial channels.
[0059] The wastewater was obtained by diluting the wastewater after the roasting process of a gold leaching plant in Yantai 20 times. The total cyanide concentration in the diluted water sample was about 72 mg / L, and the ion concentrations of Cu and Zn were 244 and 168 mg / L respectively. The coconut shell charcoal was purchased from Guangdong Xuanyu Carbon Industry Co., Ltd.
[0060] Example 1: Optimization of Preparation Conditions of Copper Slag Ozone Catalyst EDTA-CBC / HCS
[0061] By adjusting the preparation parameters in the copper slag ozone catalyst preparation process, the optimal test parameters are selected according to the effect of the prepared copper slag ozone catalyst on the removal rate of total cyanide, copper and zinc. The specific test steps for the copper slag ozone catalyst to catalyze ozone treatment of total cyanide, copper and zinc in wastewater are as follows:
[0062] The copper slag ozone catalyst and wastewater were placed in a reaction tower, and after the ozone was introduced, the reaction was carried out, and 30 mL of samples were taken every 5 minutes. The samples were passed through N2 to expel the residual O3, and then filtered through a 0.45 μm filter membrane to detect the concentrations of cyanide, copper and zinc in the water. The experiment was repeated three times, and the results were averaged and the removal rate was calculated.
[0063] Among them, the calculation formula of removal rate RE is:
[0064]
[0065] In the formula, C t and C0 are the concentrations (mg / L) of the target substance (cyanide, copper or zinc) in the solution at time t and the initial time, respectively.
[0066] 1. Addition amount of EDTA-Fe, Na
[0067] This experiment set up 5 treatment groups, in each treatment group, the addition amount of EDTA-Fe,Na was 10mmol / g, 20mmol / g, 30mmol / g, 40mmol / g and 50mmol / g. In the process of preparing copper slag ozone catalyst in each treatment group, the mass ratio of EDTA-CBC and HCS was 2:1, the activation temperature was 600℃, and the activation time was 2h.
[0068] A control group was also set up. EDTA-Fe, Na was not added in the preparation of copper slag ozone catalyst in the control group. The removal rates of total cyanide, copper and zinc in wastewater by copper slag ozone catalysts prepared in each treatment group and the control group were investigated. The results are as follows: Figure 1 shown.
[0069] During the test, C O3 =30mg / L, the O3 air flow rate is 0.2L / min, the addition concentration of copper slag ozone catalyst is 0.4g / L, the reaction temperature is 20℃, and the reaction time is 30min.
[0070] Depend on Figure 1 As shown in (a), the total cyanide removal rate of the component without EDTA-Fe,Na addition is 87.24%. When the addition amount is 2mmol / g and 3mmol / g, it shows a better catalytic effect and a faster degradation rate. At this time, the total cyanide removal rate is 91.51% and 93.88% respectively. As the addition amount continues to increase, the degradation efficiency of the total cyanide remains almost unchanged, or even slightly decreases. Figure 1 (b) It can be seen that with the increase of EDTA-Fe,Na addition, the removal rates of Zn and Cu are improved, especially Zn is almost completely removed. Compared with the catalytic oxidation of cyanide, the EDTA-Fe,Na modification effect improves the heavy metal removal effect more significantly.
[0071] 2. Activation temperature
[0072] This experiment set up 6 treatment groups, and the activation temperatures in each treatment group were 300℃, 400℃, 500℃, 600℃, 700℃ and 800℃. In the process of preparing copper slag ozone catalyst in each treatment group, the mass ratio of EDTA-CBC and HCS was 2:1, the added concentration of EDTA-Fe,Na was 3mmol / g, and the activation time was 2h.
[0073] The removal rates of total cyanide, copper and zinc in wastewater by copper slag ozone catalysts prepared in each treatment group were investigated. Figure 2 As shown. During the test, C O3 =30mg / L, the O3 air flow rate is 0.2L / min, the addition concentration of copper slag ozone catalyst is 0.4g / L, the reaction temperature is 20℃, and the reaction time is 30min.
[0074] Depend on Figure 2 (a) It can be seen that when the activation temperature increases from 300℃ to 800℃, the cyanide removal rate increases from 85.53% to 97.37%. When the activation temperature is higher than 600℃, the degradation effect increases slowly. Figure 2 (b) It can be seen that the removal effect of Cu and Zn gradually increases when the activation temperature increases from 300°C to 600°C. Considering the removal rate of total cyanide and metal ions, 600°C is determined to be the optimal activation temperature.
[0075] 3. Activation time
[0076] This experiment set up 6 treatment groups, and the activation time in each treatment group was 1h, 2h, 3h, 4h, 5h and 6h respectively. In the process of preparing copper slag ozone catalyst in each treatment group, the mass ratio of EDTA-CBC and HCS was 2:1, the added concentration of EDTA-Fe,Na was 3mmol / g, and the activation temperature was 600℃.
[0077] The removal rates of total cyanide, copper and zinc in wastewater by copper slag ozone catalysts prepared in each treatment group were investigated. Figure 3 As shown. During the test, C O3 =30mg / L, the O3 air flow rate is 0.2L / min, the addition concentration of copper slag ozone catalyst is 0.4g / L, the reaction temperature is 20℃, and the reaction time is 30min.
[0078] Depend on Figure 3 (a) It can be seen that after 30 minutes of reaction, the activation time has little effect on the removal of total cyanide. Figure 3 (b) It can be seen that when the activation time exceeds 1 h and EDTA-Fe,Na is fully activated, the activation time has little effect on the final removal effect of Cu and Zn. Therefore, the most suitable activation time is determined to be 2 h.
[0079] 4. Loading capacity of EDTA-CBC
[0080] Five treatment groups were set up in this experiment, and the mass ratios of EDTA-CBC and HCS in each treatment group were 3:1, 2:1, 1:1, 1:2 and 1:3 respectively. In the process of preparing copper slag ozone catalyst in each treatment group, the activation temperature was 600℃ and the activation time was 2h.
[0081] The removal rates of total cyanide, copper and zinc in wastewater by copper slag ozone catalysts prepared in each treatment group were investigated. Figure 4 As shown. During the test, C O3 =30mg / L, the O3 air flow rate is 0.2L / min, the addition concentration of copper slag ozone catalyst is 0.4g / L, the reaction temperature is 20℃, and the reaction time is 30min.
[0082] Depend on Figure 4 (a) It can be seen that when the mass ratio of EDTA-CBC and HCS is 1:2, the system can exert the maximum catalytic efficiency, at which time the degradation rate of cyanide is 97.37%, and the residual concentrations of Cu and Zn are 0.034 mg / L and 0.524 mg / L. The preparation conditions of the catalyst should be determined by comprehensive consideration of various dimensions. Therefore, the mass ratio of EDTA-CBC and HCS in subsequent experiments is determined to be 1:2.
[0083] In summary, based on the removal rate of total cyanide, copper and zinc, production cost and energy issues, the preparation conditions of copper slag ozone catalyst were finally determined as follows: EDTA-Fe,Na dosage 2 mmol / g, activation temperature and time 600 °C and 2 h respectively, the mass ratio of EDTA-CBC and HCS was 1:2, and the prepared copper slag ozone catalyst was marked as EDTACBC / HCS.
[0084] Example 2: Preparation method of copper slag ozone catalyst
[0085] (1) Coconut shell ash CBC and sodium ethylenediaminetetraacetate iron were mixed at a ratio of 1 g: 2 mmol, and then immersed in a 85 wt% phosphoric acid solution for 10 h to obtain a sample, wherein the mass ratio of coconut shell ash to phosphoric acid solution was 1:3. The sample was placed in a N2 atmosphere, heated to 600°C at a rate of 10°C / min, and activated at this temperature for 2 h. After cooling to room temperature, EDTA-CBC was obtained;
[0086] (2) screening out 150 mesh copper slag particles, stirring and washing them with deionized water for 15 min, repeating the washing for 3 times, drying them at 120 °C for 12 h, and then placing the copper slag particles in an air atmosphere, heating them to 722 °C at a rate of 10 °C / min, and calcining them at this temperature for 4.32 h to obtain modified copper slag (HCS);
[0087] (3) The modified copper slag and EDTA-CBC were mixed in a mass ratio of 2:1, and then hydroxypropyl methylcellulose (HPMC) was added as a binder to mix well, and then put into water to obtain an adhesive, wherein the mass ratio of the total mass of the modified copper slag, EDTA-CBC and the binder to the mass ratio of water was 1:1. The adhesive was placed in a N2 atmosphere, calcined at 550°C for 2h, and ground through a 100-mesh sieve to obtain a copper slag ozone catalyst (EDTA-CBC / HCS).
[0088] The copper slag ozone catalyst (EDTA-CBC / HCS) prepared in this example was subjected to morphological analysis. Figure 5-Figure 8 shown.
[0089] Depend on Figure 5 It can be seen that many agglomerates grow on the surface of activated EDTA-CBC, while the composite material EDTA-CBC / HCS shows the characteristics of EDTA-CBC surface roughness and full of agglomerates, and also shows the characteristics of HCS mineral structure slender crystals, proving that the composite catalyst was successfully prepared. According to surface element analysis, CBC activated by EDTA-Fe, Na and phosphoric acid impregnation is evenly covered with elements such as P, Fe, and Na, indicating that the activation process successfully improved the surface structure of CBC, but the Fe content is relatively small. After loading EDTA-CBC on HCS, the C and P elements mainly contributed by EDTA-CBC on the catalyst surface are evenly distributed, the Fe content is significantly increased, and Si representing the characteristics of HCS appears, further proving that the composite of EDTA-CBC and HCS is effective.
[0090] Depend on Figure 6It can be seen that according to the isotherm type classified by IUPAC, the N2 adsorption-desorption curve of the copper slag ozone catalyst is type I. It can be seen that the surface structure of the copper slag ozone catalyst mainly shows the characteristics of EDTA-CBC, and the appearance of the H3 type hysteresis loop indicates that the material is mainly a non-rigid aggregate of layered particles, mostly composed of slit-type channels. The pore size distribution of the copper slag ozone catalyst is mainly concentrated below 50nm, and it is a mesoporous material.
[0091] Depend on Figure 7 It can be seen that by comparing with the standard card, the components and crystal characteristics of the active substances generated during the reaction are analyzed. The crystal characteristics of EDTA-CBC are similar to those of C and Fe2P4O 12 Therefore, under the action of phosphoric acid, EDTA-Fe,Na converts Fe into Fe2P4O 12 , and in situ grows on the CBC surface. EDTA-CBC / HCS has both Fe3O4 and Fe2P4O 12 The crystal characteristics of the composite material EDTA-CBC / HCS were successfully prepared.
[0092] Depend on Figure 8 It can be seen that at a wavelength of 3420cm -1 The absorption peak at wavelength 1570 cm -1 The absorption peak at 1260 cm is mainly attributed to the stretching vibration of aromatic C=C. -1 、1050cm -1 and 710cm -1 The absorption peaks at 510cm correspond to the CN bending vibration, C=O bond and CH bond in the amide III band. -1 The OPO structure is responsible, indicating that phosphoric acid interacted strongly with the biochar surface during the activation process. Comparing CBC and EDTA-CBC activated with phosphoric acid, the peaks of OH, C=C, C=O, CN, and CH were significantly enhanced, indicating that the in-situ activation of CBC not only changed the physical properties such as pore structure, but also changed the microscopic chemical morphology. EDTA-Fe,Na decomposes at high temperature, and amino and carboxyl groups grow on the surface of CBC, increasing the unsaturation of biochar and increasing the number of functional groups containing N and O, which is conducive to the adsorption reaction.
[0093] Test Example 1:
[0094] The copper slag ozone catalyst prepared in Example 2 was subjected to ozone treatment to remove total cyanide, copper and zinc in the wastewater, and the experimental conditions were optimized. The specific experimental steps were the same as in Example 1.
[0095] 1. Ozone concentration
[0096] This experiment set up 5 treatment groups, in each treatment group, the O3 addition concentration was 15mg / L, 20mg / L, 25mg / L, 30mg / L and 35mg / L, where O3 addition concentration = ozone addition amount (mg) / wastewater volume (L). The removal rate of total cyanide, copper and zinc in each treatment group was investigated. The results are as follows Fig. 9 During the test, the O3 gas flow rate was 0.2 L / min, the mass ratio of copper slag ozone catalyst EDTA-CBC / HCS to wastewater was 0.4 g:1 L, the reaction temperature was 20°C, and the reaction time was 30 min.
[0097] like Fig. 9 As shown in (a), with the increase of O3 addition concentration, the total cyanide removal rate gradually increases. When the O3 addition concentration exceeds 25 mg / L, the total cyanide removal rate does not increase significantly, but the removal rate is significantly accelerated. At this time, the content of oxidant in the system is not the decisive factor limiting the reaction. When the O3 addition concentration is 25 mg / L, the total cyanide removal rate is 97.07%. Fig. 9 (b) It can be seen that the O3 dosage has a significant effect on the removal of Cu, and the O3 concentration at a lower level can achieve a better effect on the removal of Zn. Based on the comprehensive experimental results and economic factors, when the O3 dosage concentration is 25 mg / L, the removal effect of Cu and Zn is relatively good, and the residual concentrations of the two are 0.539 and 0.041 mg / L respectively. Therefore, the optimal ozone dosage concentration is 25 mg / L.
[0098] 2. Dosage concentration of copper slag ozone catalyst
[0099] This experiment set up 7 treatment groups. In each treatment group, the addition concentration of copper slag ozone catalyst was 0g / L, 0.1g / L, 0.2g / L, 0.3g / L, 0.4g / L, 0.5g / L and 0.6g / L, respectively. The addition concentration of copper slag ozone catalyst = the addition amount of copper slag ozone catalyst (g) / the volume of wastewater (L). The removal rates of total cyanide, copper and zinc in each treatment group were investigated. The results are as follows Fig.10 During the test, the concentration of O3 added was 25 mg / L, the O3 gas flow rate was 0.2 L / min, the reaction temperature was 20°C, and the reaction time was 30 min.
[0100] Depend on Fig.10 (a) It can be seen that after 30 minutes of reaction, the total cyanide removal rate in the components without catalyst was 75.19%, and the removal rate gradually increased after adding catalyst. When the EDTA-CBC / HCS dosage was 0.3g / L, the total cyanide removal rate reached the critical value of 94.96%. Fig.10(b) It can be seen that the copper slag ozone catalyst has a significant effect on the removal of Cu and Zn. The residual concentrations of Cu and Zn in the components without catalyst addition are 1.121 and 0.096 mg / L, respectively. With the increase of the dosage of copper slag ozone catalyst EDTA-CBC / HCS, the residual concentrations of Cu and Zn in the components gradually decrease.
[0101] 3. Initial pH of the solution
[0102] This experiment set up 6 treatment groups, and the initial pH of the solution in each treatment group was 8.0, 8.5, 9.0, 9.5, 10.0 and 10.5 respectively. The removal rates of total cyanide, copper and zinc in each treatment group were investigated. The results are as follows Fig.11 During the test, the concentration of O3 added was 25 mg / L, the O3 gas flow rate was 0.2 L / min, the mass ratio of copper slag ozone catalyst EDTA-CBC / HCS to wastewater was 0.4 g:1 L, the reaction temperature was 20 °C, and the reaction time was 30 min.
[0103] Depend on Fig.11 (a) It can be seen that in a single ozonation system, as the pH increases, the total cyanide removal rate shows a trend of first increasing and then decreasing. When the pH is 9.5, the total cyanide removal rate is the best, which is 86.81%. Fig.11 (b) It can be seen that by comparing the ozonation system and the catalytic ozonation system, the addition of the catalyst significantly enhanced the removal of metal ions, especially the removal of Cu. The effect of increasing pH on the precipitation of ions was not significant. The optimal pH for the synergistic removal of Cu and Zn was 9.5, at which the residual concentrations of the two were 0.44 and 0.03 mg / L, respectively. Fig.11 (c) and Fig.11 (d) It can be seen that when the pH is between 8 and 8.5, the O3 and OH - The consumption of cyanide in the catalytic oxidation system is not much different, but the removal effect of cyanide in the catalytic oxidation system is better than that of the single ozonation system, which shows that the indirect oxidation performance of the free radicals generated by the catalytic reaction is higher than that of the direct oxidation. - The consumption of ozonation system is significantly higher than that of the single ozonation system. At this time, the catalytic effect of the catalyst is significantly enhanced, and indirect oxidation is dominant. When the pH is higher than 10, both direct and indirect oxidation are inhibited. Considering the removal of total cyanide, Cu and Zn, and the utilization of O3, the catalytic effect is best and most economical when the pH is 9.5.
[0104] 4. Reaction temperature
[0105] This experiment set up 3 treatment groups, and the reaction temperatures in each treatment group were 20℃, 30℃ and 40℃ respectively. The removal rates of total cyanide, copper and zinc in each treatment group were investigated. The results are as follows: Fig.12 During the test, the O3 concentration was 25 mg / L, the O3 gas flow rate was 0.2 L / min, the mass ratio of copper slag ozone catalyst EDTA-CBC / HCS to wastewater was 0.3 g:1 L, the initial pH of the solution was 9.5, and the reaction time was 30 min.
[0106] Depend on Fig.12 (a) and (c) show that as the temperature increases, the total cyanide removal rate decreases slightly and the reaction rate constant also decreases, which indicates that the negative impact of the decrease in O3 solubility is greater than the promoting effect of the temperature increase on the reaction. Fig.12 (b) It can be seen that the removal of C is concentrated in 15-20 minutes, and the removal of Zn is mainly concentrated in the first 5 minutes of the reaction. Fig.12 (c) It can be seen that the amount of O3 dissolved in the system decreases with increasing temperature, indicating that O3 dissolution is greatly affected by temperature, and the consumption of OH- is greater at low temperatures. Comprehensive analysis shows that the optimal reaction temperature is 20℃.
[0107] In summary, the copper slag ozone catalyst EDTA-CBC / HCS prepared in Example 2 was used to ozone treat total cyanide, copper and zinc in wastewater, the solid-liquid ratio of ozone to wastewater was 25 mg:1L, the solid-liquid ratio of copper slag ozone catalyst to wastewater was 0.3 g:1L, the initial pH of the solution was 9.5, and the reaction temperature was 20°C.
[0108] Test Example 2:
[0109] The copper slag ozone catalyst prepared in Example 2 was used to treat total cyanide, copper and zinc in wastewater and was recycled 5 times. The removal effects of total cyanide, copper and zinc were used as evaluation indicators. The results are as follows: Fig.13 shown.
[0110] Depend on Fig.13 It can be seen that the removal rate of total cyanide by catalytic ozonation of the catalyst used for the first time was 98.71%, and after 5 cycles, the removal rate decreased by 6.45%. The residual concentrations of Cu and Zn in the catalyst system used for the first time were 0.448 and 0.032 mg / L, respectively. After 5 cycles, the residual concentrations of Cu and Zn in the system were 0.568 and 0.062 mg / L, respectively.
[0111] The above description is only the preferred embodiment of the present application and is not intended to limit the present application. For those skilled in the art, the present application may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present application shall be included in the protection scope of the present application.
Claims
1. A copper slag ozone catalyst, characterized in that: The copper slag ozone catalyst is prepared from a carrier and an active component, wherein the carrier is modified copper slag and the active component is EDTA-modified coconut shell ash; the mass ratio of the carrier to the active component is (0.5-3):
1.
2. The copper slag ozone catalyst according to claim 1, characterized in that The modified copper slag is prepared by the following method: washing and drying copper slag particles and then calcining to obtain modified copper slag; the calcination temperature is 700-750° C. and the calcination time is 4-4.5 hours.
3. The copper slag ozone catalyst according to claim 2, characterized in that The particle size of the copper slag particles is 150-200 mesh, the drying temperature is 105-120° C., and the drying time is 10-12 hours.
4. The copper slag ozone catalyst according to claim 1, characterized in that The EDTA-modified coconut shell ash is prepared by the following method: coconut shell ash and sodium ferric ethylenediaminetetraacetate are mixed, and then immersed in a phosphoric acid solution to obtain a sample, and the sample is placed in an inert gas for activation, and cooled to room temperature to obtain EDTA-modified coconut shell ash.
5. The copper slag ozone catalyst as claimed in claim 4, characterized in that: The solid-liquid ratio of coconut shell ash and sodium ferric ethylenediaminetetraacetate is 1g:(1-5)mmol, the impregnation time is 8-12h, the activation temperature is 300-800℃, the activation time is 1-6h, the inert gas is N2, and the mass ratio of coconut shell ash and phosphoric acid solution is 1:
3.
6. The method for preparing the copper slag ozone catalyst according to any one of claims 1 to 5, characterized in that: The steps include: The modified copper slag, EDTA-modified coconut shell ash and adhesive are mixed, and then put into water for uniform mixing to obtain an adhesive, and the adhesive is calcined, ground and sieved to obtain a copper slag ozone catalyst.
7. The preparation method according to claim 6, characterized in that: The binder is hydroxypropyl methylcellulose, the mass ratio of the total mass of modified copper slag, EDTA-modified coconut shell ash and the binder to water is 1:1; the mass ratio of the total mass of modified copper slag, EDTA-modified coconut shell ash and the binder is 100:
1.
8. The preparation method according to claim 6, characterized in that: The operation of calcining the bond is as follows: placing the bond in a N2 atmosphere and calcining at 500-600°C for 1.5-2.5 hours.
9. Use of the copper slag ozone catalyst according to any one of claims 1 to 5 in catalytic ozone treatment of cyanide and heavy metal ions in wastewater.
10. The use according to claim 9, characterized in that The heavy metal ions are copper ions and / or zinc ions.
Citation Information
Patent Citations
Method for preparing ozone catalytic oxidation catalyst for treating cyanide waste water
CN102008965A
Transition metal catalyst applied to ozone catalytic advanced oxidation sewage treatment and preparation method thereof, and ozone catalytic advanced oxidation sewage treatment method
CN106964353A
Catalyst for oil field wastewater treatment and preparation process thereof
CN110180595A
Solid-catalysed oxidn. of organic esp. hardly biodegradable cpds. in water
DE4446375C1