Lanthanide-doped bismuth oxybromide photocatalyst, preparation method and application

By doping the BiOBr photocatalyst with lanthanides, the solar energy utilization and dye degradation efficiency in the printing and dyeing wastewater is improved, the problem of low efficiency of a single BiOBr material is solved, and efficient printing and dyeing wastewater treatment is achieved.

CN118976517APending Publication Date: 2024-11-19CHINA AGRI UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411014065.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The single BiOBr photocatalytic material has problems such as low solar energy utilization efficiency and limited dye degradation efficiency in printing and dyeing wastewater treatment.

Method used

Through lanthanide doping, the visible light response capability and photogenerated carrier separation capability of BiOBr were improved, and a lanthanide doped bismuth oxide photocatalyst was prepared. A photocatalyst with spherical honeycomb structure was prepared by solvothermal reaction method. Rapidly degrade methyl orange in printing and dyeing wastewater.

Benefits of technology

It significantly improves the treatment efficiency of printing and dyeing wastewater, has excellent material performance, and can achieve rapid degradation of methyl orange in a short time, with a degradation rate of more than 94%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976517A_ABST
    Figure CN118976517A_ABST
Patent Text Reader

Abstract

The invention provides a lanthanide doped bismuth oxybromide photocatalyst as well as a preparation method and application thereof. The lanthanide doped bismuth oxybromide photocatalyst comprises bismuth nitrate pentahydrate, polyvinylpyrrolidone and potassium bromide in a ratio of (0.5-1.5) mmol: (0.2-1.0) g: (0.5-1.5) mmol. The ratio of lanthanide to Bi is 1.0%-60%; the lanthanide doped bismuth oxybromide photocatalyst is of a spherical honeycomb structure. According to the lanthanide doped bismuth oxybromide photocatalyst, the preparation method and the application, the lanthanide doped bismuth oxybromide photocatalyst has excellent methyl orange catalytic degradation performance under visible light.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of inorganic nanometer photocatalytic materials, and in particular to a lanthanide element-doped bismuth oxybromide photocatalyst, a preparation method and an application thereof. Background Art

[0002] Printing and dyeing wastewater is one of the key pollution sources in my country's industrial system. It has a large amount of wastewater, high content of organic pollutants, deep chromaticity, large changes in alkalinity and pH value, and is one of the organic wastewaters with high treatment difficulty. At present, the commonly used treatment methods for printing and dyeing wastewater include adsorption, biological method, electrochemical oxidation method, photocatalysis, etc. Among them, the photocatalysis method has the advantages of utilizing solar energy and completely degrading pollutants, showing great potential in the treatment of printing and dyeing wastewater.

[0003] Photocatalytic technology, as a type of advanced oxidation process, is considered to be one of the cleanest and most effective treatment methods and has been proven to be an effective method for degrading printing and dyeing wastewater. Bismuth oxybromide (BiOBr) is a photocatalyst with visible light response, suitable bandgap width and unique layered structure, showing good potential in photocatalytic water purification. However, a single BiOBr material can only absorb high-energy sunlight, and the charge transfer and separation efficiency is limited.

[0004] In order to improve the solar energy utilization and dye degradation efficiency of single BiOBr photocatalytic materials, lanthanide elements are used for doping. Lanthanide elements have a specific and unique upconversion effect and are similar in size to the ionic radius of bismuth. Lanthanide element doping helps to improve BiOBr's visible light response ability and photogenerated carrier separation ability. Summary of the invention

[0005] The purpose of the present invention is to provide a lanthanide element-doped bismuth oxybromide photocatalyst, a preparation method and an application thereof. The material has excellent performance and strong visible light response capability, can achieve rapid degradation of methyl orange in a short time, and significantly improve the treatment efficiency of printing and dyeing wastewater.

[0006] To achieve the above object, the present invention provides a lanthanide element doped bismuth oxybromide photocatalyst, comprising

[0007] Bismuth nitrate pentahydrate, polyvinyl pyrrolidone, potassium bromide = 0.5-1.5 mmol: 0.2-1.0 g: 0.5-1.5 mmol;

[0008] Lanthanide / Bi (molar ratio) = 1.0% to 60%;

[0009] Lanthanide-doped bismuth oxybromide photocatalyst has a spherical honeycomb structure.

[0010] Preferably, the types of lanthanide elements include La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium).

[0011] Preferably, bismuth nitrate pentahydrate, potassium bromide = 0.6-1.4 mmol: 0.6-1.4 mmol;

[0012] Lanthanide elements / Bi (molar ratio) = 2.0% to 50%.

[0013] Preferably, bismuth nitrate pentahydrate, polyvinyl pyrrolidone = 0.7-1.3 mmol: 0.3-0.9 g;

[0014] Lanthanide elements / Bi (molar ratio) = 5.0% to 45%.

[0015] A method for preparing a lanthanide element-doped bismuth oxybromide photocatalyst comprises the following steps:

[0016] Step 1: dissolving bismuth nitrate pentahydrate and polyvinyl pyrrolidone in an ethylene glycol solution, stirring rapidly for the first time to obtain a mixed solution, adding potassium bromide, stirring for a second time to fully react; then adding lanthanide elements to the mixed solution, stirring for a third time to fully react;

[0017] Step 2: The mixed solution is transferred to a polytetrafluoroethylene-lined reactor for a solvent thermal reaction, and the obtained product is centrifuged, filtered, washed and dried to obtain a photocatalytic material.

[0018] Preferably, step 1 is carried out at room temperature;

[0019] In step 1, the first stirring time is 30 to 120 min, the second stirring time is 120 to 240 min, and the third stirring time is 30 to 120 min.

[0020] Preferably, in step 2, the solvent thermal reaction temperature is 120-200° C., and the heating time is 2-6 hours.

[0021] Preferably, in step 2, the drying temperature is 50 to 80° C. and the drying time is 1 to 6 hours.

[0022] The invention discloses an application of a lanthanide element-doped bismuth oxybromide photocatalyst for degrading methyl orange in water.

[0023] Preferably, the method comprises dispersing the photocatalytic material in an aqueous solution containing methyl orange, stirring in a dark environment until adsorption-desorption equilibrium is reached, performing photocatalytic degradation under visible light, sampling at intervals, filtering the taken samples through a membrane, and determining the concentration of the filtrate.

[0024] Therefore, the present invention adopts the above-mentioned lanthanide element-doped bismuth oxybromide photocatalyst, preparation method and application, and the technical effects are as follows:

[0025] (1) The lanthanide-doped BiOBr-based photocatalyst material prepared by the present invention has excellent performance and strong visible light response ability, and can achieve rapid degradation of methyl orange in a short time, thereby significantly improving the treatment efficiency of printing and dyeing wastewater.

[0026] (2) The BiOBr-based photocatalyst material prepared by the present invention has a simple preparation method, low raw material cost, and simple operation. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a comparison chart of the photocatalytic activity of the photocatalytic materials of Examples 1 to 7 of the present invention to methyl orange.

[0028] Figure 2 This is a comparison chart of the photocatalytic activity of methyl orange in Examples 6, 9 and 21 of the present invention.

[0029] Figure 3 This is the XRD diagram of the photocatalytic material of Example 6 of the present invention.

[0030] Figure 4 This is the XPS graph of the photocatalytic material of Example 6 of the present invention.

[0031] Figure 5 This is the SEM image of the photocatalytic material of Example 6 of the present invention.

[0032] Figure 6 This is the ultraviolet-visible diffuse reflectance spectrum of the photocatalytic material of Example 6 of the present invention. DETAILED DESCRIPTION

[0033] The technical solution of the present invention is further described below through the accompanying drawings and embodiments.

[0034] Unless otherwise defined, technical or scientific terms used in the present invention shall have the common meanings understood by one having ordinary skills in the field to which the present invention belongs.

[0035] Experimental reagents

[0036] All reagents were of analytical grade and used without further purification. Deionized water was used throughout the study.

[0037] Bismuth nitrate pentahydrate (Bi(NO3)3·5H2O, 99.0%), neodymium nitrate hexahydrate (Nd(NO3)3·6H2O, 99.0%), lanthanum nitrate hexahydrate (La(NO3)3·6H2O, 99.0%), cerium nitrate hexahydrate (Ce(NO3)3·6H2O, 99.0%), praseodymium nitrate hexahydrate (Pr(NO3)3·6H2O, 99.0%), samarium nitrate hexahydrate (Sm(NO3)3·6H2O, 99.0%), europium nitrate hexahydrate (Eu(NO3)3·6H2O, 99.0%), gadolinium nitrate hexahydrate (Gd(NO3)3·6H2O, 99.0%) 6H2O, 99.0%), terbium nitrate hexahydrate (Tb(NO3)3·6H2O, 99.0%), dysprosium nitrate hexahydrate (Dy(NO3)3·6H2O, 99.0%), holmium nitrate pentahydrate (Ho(NO3)3·5H2O, 99.0%), erbium nitrate hexahydrate (Er(NO3)3·6H2O, 99.0%), thulium nitrate pentahydrate (Tm(NO3)3·5H2O, 99.0%), ytterbium nitrate pentahydrate (Yb(NO3)3·5H2O, 99.0%) and lutetium nitrate hexahydrate (Lu(NO3)3·6H2O, 99.0%) are selected from Aladdin;

[0038] Potassium bromide (KBr, 99.0%) was purchased from Sinopharm Chemical Reagent Co., Ltd. (Shanghai test);

[0039] Ethylene glycol (C2H6O) was purchased from Beijing Tongguang Fine Chemical Co., Ltd.

[0040] Polyvinylpyrrolidone (PVP(K30)) and methyl orange were supplied by Maclean (Shanghai, China).

[0041] Experimental equipment

[0042] Xenon lamp: Made in China Yuyu

[0043] UV-Vis Spectrophotometer: T6 New Century - Beijing Puxi General Instrument Co., Ltd.

[0044] XRD: Rigaku Ultima IV

[0045] XPS: Thermo Scientific ESCALAB 250Xi

[0046] SEM: ZEISS GeminiSEM 300

[0047] UV-Vis diffuse reflectance spectroscopy: Shimadzu UV-3600i Plus.

[0048] Example 1

[0049] The present invention provides a method for preparing a lanthanide element-doped bismuth oxybromide photocatalyst, comprising the following steps:

[0050] Weigh 0.4851g (1mmol) of bismuth nitrate pentahydrate and 0.2g of polyvinyl pyrrolidone into a beaker, add 60ml of ethylene glycol solution, stir at room temperature for 30min, add 0.119g (1mmol) of potassium bromide to the mixed solution, stir at room temperature for 60min, then add 0.01mmol of neodymium nitrate hexahydrate to the mixed solution, and stir at room temperature for 30min. Transfer the mixed solution to a polytetrafluoroethylene-lined reactor and heat at 160°C for 3h. The resulting suspension is centrifuged at 8000r / min for 10min. After solid-liquid separation, the sample is washed 3 times with ethanol and deionized water in a suction filtration device, and the obtained material is dried in an oven at 60°C for use.

[0051] The present invention provides an application of a lanthanide element-doped bismuth oxybromide photocatalyst, comprising the following steps:

[0052] The prepared lanthanide-doped BiOBr-based photocatalyst material was subjected to a methyl orange degradation experiment. A xenon lamp (300W) was used as a light source to simulate sunlight. 50 mg of the photocatalytic material was dispersed in 50 mL of a 20 mg / L methyl orange solution, stirred for 30 min in the dark to achieve adsorption-desorption equilibrium, and then reacted for 120 min under a λ>420 nm filter and illumination conditions. During the whole process, samples were taken every 10 min, and after passing through a 0.45 μm filter membrane, the methyl orange concentration in the liquid was determined using a UV-visible spectrophotometer.

[0053] Example 2

[0054] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.03 mmol.

[0055] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.03 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0056] Example 3

[0057] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.05 mmol.

[0058] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.5 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0059] Example 4

[0060] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.10 mmol.

[0061] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.10 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0062] Example 5

[0063] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.20 mmol.

[0064] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.20 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0065] Example 6

[0066] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.30 mmol.

[0067] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0068] Example 7

[0069] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.40 mmol.

[0070] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.40 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0071] Example 8

[0072] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that the amount of neodymium nitrate hexahydrate added is set to 0.50 mmol.

[0073] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.50 mmol of neodymium nitrate hexahydrate is used to degrade methyl orange.

[0074] Example 9

[0075] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by lanthanum nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0076] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of lanthanum nitrate hexahydrate is used to degrade methyl orange.

[0077] Example 10

[0078] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by cerium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0079] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of cerium nitrate hexahydrate is used to degrade methyl orange.

[0080] Example 11

[0081] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by praseodymium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0082] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of praseodymium nitrate hexahydrate is used to degrade methyl orange.

[0083] Example 12

[0084] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by samarium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0085] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of samarium nitrate hexahydrate is used to degrade methyl orange.

[0086] Example 13

[0087] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by europium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0088] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of europium nitrate hexahydrate is used to degrade methyl orange.

[0089] Example 14

[0090] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by gadolinium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0091] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of gadolinium nitrate hexahydrate is used to degrade methyl orange.

[0092] Example 15

[0093] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by terbium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0094] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of terbium nitrate hexahydrate is used to degrade methyl orange.

[0095] Example 16

[0096] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by dysprosium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0097] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of dysprosium nitrate hexahydrate is used to degrade methyl orange.

[0098] Example 17

[0099] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by holmium nitrate pentahydrate, and the added amount is set to 0.30 mmol.

[0100] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of holmium nitrate pentahydrate is used to degrade methyl orange.

[0101] Example 18

[0102] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by erbium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0103] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of erbium nitrate hexahydrate is used to degrade methyl orange.

[0104] Example 19

[0105] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by thulium nitrate pentahydrate, and the added amount is set to 0.30 mmol.

[0106] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of thulium nitrate pentahydrate is used to degrade methyl orange.

[0107] Example 20

[0108] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by ytterbium nitrate pentahydrate, and the added amount is set to 0.30 mmol.

[0109] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of ytterbium nitrate pentahydrate is used to degrade methyl orange.

[0110] Example 21

[0111] A method for preparing a lanthanide-doped BiOBr-based photocatalyst material, which is different from Example 1 in that neodymium nitrate hexahydrate is replaced by lutetium nitrate hexahydrate, and the added amount is set to 0.30 mmol.

[0112] An application of a lanthanide element doped BiOBr-based photocatalyst material is different from Example 1 in that the lanthanide element doped BiOBr-based photocatalyst material prepared by adding 0.30 mmol of lutetium nitrate hexahydrate is used to degrade methyl orange.

[0113] The properties of the BiOBr-based photocatalyst materials prepared using Examples 1 to 21 are as follows:

[0114] like Figure 1 As shown, the comparison of the photocatalytic adsorption (0-30 min) and photocatalytic degradation of methyl orange in Examples 1 to 7 proves that Example 6 has the best catalytic effect, followed by Example 5. Under the simulated visible light of a 300W xenon lamp, the degradation rate of methyl orange in Example 6 can reach more than 94% in 2 hours.

[0115] like Figure 2 As shown, the comparison of the photocatalytic adsorption (0-30 min) and photocatalytic degradation of methyl orange of Example 6 and Examples 9 to 21 proves that the catalytic effect of Example 6 is the best, followed by Examples 11, 12 and Example 14.

[0116] like Figure 3 As shown, the sample of Example 6 corresponds to the standard card, which proves the successful synthesis of the lanthanide-doped BiOBr-based photocatalytic material, and the lanthanide-doping has no significant effect on the crystal structure of the BiOBr-based photocatalytic material.

[0117] like Figure 4 As shown, the elements contained in the sample of Example 6 include Bi, O, Br and Nd, indicating that the lanthanide elements are successfully introduced into the BiOBr lattice.

[0118] like Figure 5As shown, the sample of Example 6 formed a regular honeycomb spherical structure, which further confirmed that the elements contained in the sample included Bi, O, Br and Nd, the lanthanide elements were successfully introduced, and no other impurities were contained.

[0119] like Figure 6 As shown, the sample of Example 6 has the ability to absorb visible light, and due to the introduction of lanthanide elements, it exhibits an obvious up-conversion effect.

[0120] Comparative Example

[0121] Under the conditions of reference document 2 (CN104971711B), the catalytic degradation test of methyl orange in Example 9 of the present invention was carried out, except that the concentration of methyl orange in reference document 2 was 15 mg / L, while that in this test was 20 mg / L. After 60 minutes of dark reaction and 60 minutes of illumination, the degradation efficiency of methyl orange was 84.12%, while the degradation efficiency published in reference document 2 was in the range of 68.12% to 85.31%.

[0122] Therefore, the present invention adopts the above-mentioned lanthanide element-doped bismuth oxybromide photocatalyst and its preparation method and application, which has excellent material performance and strong visible light response ability, can achieve rapid degradation of methyl orange in a short time, and significantly improve the treatment efficiency of printing and dyeing wastewater.

[0123] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that they can still modify or replace the technical solution of the present invention with equivalents, and these modifications or equivalent replacements cannot cause the modified technical solution to deviate from the spirit and scope of the technical solution of the present invention.

Claims

1. A lanthanide-doped bismuth oxybromide photocatalyst, characterized in that: include Bismuth nitrate pentahydrate, polyvinyl pyrrolidone, potassium bromide = 0.5-1.5 mmol: 0.2-1.0 g: 0.5-1.5 mmol; Lanthanide / Bi (molar ratio) = 1.0% to 60%; Lanthanide-doped bismuth oxybromide photocatalyst has a spherical honeycomb structure.

2. The lanthanide-doped bismuth oxybromide photocatalyst according to claim 1, characterized in that: The types of lanthanide elements include La (lanthanum), Ce (cerium), Pr (praseodymium), Nd (neodymium), Sm (samarium), Eu (europium), Gd (gadolinium), Tb (terbium), Dy (dysprosium), Ho (holmium), Er (erbium), Tm (thulium), Yb (ytterbium), and Lu (lutetium).

3. The lanthanide-doped bismuth oxybromide photocatalyst according to claim 1, characterized in that: Bismuth nitrate pentahydrate, potassium bromide = 0.6-1.4 mmol: 0.6-1.4 mmol; Lanthanide elements / Bi (molar ratio) = 2.0% to 50%.

4. The lanthanide-doped bismuth oxybromide photocatalyst according to claim 1, characterized in that: Bismuth nitrate pentahydrate, polyvinyl pyrrolidone = 0.7-1.3 mmol: 0.3-0.9 g; Lanthanide elements / Bi (molar ratio) = 5.0% to 45%.

5. A method for preparing a lanthanide-doped bismuth oxybromide photocatalyst, characterized in that: The following steps are involved: Step 1: dissolving bismuth nitrate pentahydrate and polyvinyl pyrrolidone in an ethylene glycol solution, stirring rapidly for the first time to obtain a mixed solution, adding potassium bromide, stirring for a second time to fully react; then adding lanthanide elements to the mixed solution, stirring for a third time to fully react; Step 2: The mixed solution is transferred to a polytetrafluoroethylene-lined reactor for a solvothermal reaction, and the obtained product is centrifuged, filtered, washed and dried to obtain a photocatalytic material.

6. The method for preparing a lanthanide-doped bismuth oxybromide photocatalyst according to claim 5, characterized in that: Step 1 is carried out at room temperature; In step 1, the first stirring time is 30 to 120 min, the second stirring time is 120 to 240 min, and the third stirring time is 30 to 120 min.

7. The method for preparing a lanthanide-doped bismuth oxybromide photocatalyst according to claim 5, characterized in that: In step 2, the solvent thermal reaction temperature is 120 to 200° C., and the heating time is 2 to 6 hours.

8. The method for preparing a lanthanide-doped bismuth oxybromide photocatalyst according to claim 5, characterized in that: In step 2, the drying temperature is 50 to 80° C. and the drying time is 1 to 6 hours.

9. An application of a lanthanide element-doped bismuth oxybromide photocatalyst, characterized in that: Used to degrade methyl orange in water.

10. The use of a lanthanide element-doped bismuth oxybromide photocatalyst according to claim 9, characterized in that: The method comprises dispersing the photocatalytic material in a water solution containing methyl orange, stirring in a dark environment until adsorption and desorption equilibrium is reached, performing photocatalytic degradation under visible light, sampling at intervals, filtering the taken samples through a membrane, and determining the concentration of the filtrate.

Citation Information

Patent Citations

  • Bismuth oxyhalide light-emitting material with doped rare earth ions and preparation method thereof

    CN103421511A

  • Preparation method of rare-earth element doped modified hollow microsphere bismuth oxyiodide photocatalyst

    CN107597150A

  • Application of composite photocatalyst in dye wastewater treatment

    CN111825156A

  • Ce-doped BiOBr nano photocatalyst as well as preparation method and application thereof

    CN113828334A