Preparation method and application of aeration-free durable and stable advanced oxidation catalyst

By designing a carbon nitride-based S-type heterojunction Fenton photocatalyst at double defect sites, VO-M-Co3O4@CNx is assisted in the preparation of VO-M-Co3O4@CNx with a porous zeolite imidazole salt framework and an oxygen-rich polymer, the high energy consumption of traditional systems is solved. and the problem of structural instability, efficient and low-energy consumption pollutant removal is achieved, which is suitable for wastewater treatment.

CN118976521AActive Publication Date: 2024-11-19JIANGSU JIANGKE NEW COMPOSITE MATERIAL CO LTD +2
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410812898.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-22
Publication Date
2024-11-19
Estimated Expiration
2044-06-22

AI Technical Summary

Technical Problem

The traditional Fenton-like photocatalytic degradation system relies on oxygen transport and forced convection, resulting in high energy consumption; the Co-based catalyst structure is unstable, resulting in cobalt ions escape and secondary pollution; the Fenton-like catalyst has low absorption and utilization of solar light, and PMS The activation rate is slow and the degradation efficiency is low.

Method used

Design a carbon nitride-based S-type heterojunction Fenton photocatalyst at double defect sites, and assisted in the preparation of VO-M-Co3O4@CNx catalyst through porous zeolite imidazole salt framework ZIF-67 and oxygen-rich polymer PEG to improve its Stability and PMS activation performance enable advanced oxidation treatment without aeration.

Benefits of technology

It significantly improves pollutant removal efficiency, increases degradation rate by 10 times, reduces energy consumption, enhances catalyst stability and anti-interference ability, and is suitable for large-scale applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976521A_ABST
    Figure CN118976521A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a persistent and stable advanced oxidation catalyst without aeration. Nitrogen-defect-containing carbon nitride (CNx) of a 2D lamellar structure is used as a carrier, an oxygen-rich group-containing polymer is introduced as a structure-directing agent to soften CNX, and then MOF-derived oxygen vacancy-containing cobaltosic oxide (VO-M-Co3O4) is coated with CNX, so that VO-M-Co3O4 has high dispersity and a large number of catalytic active sites, and the catalytic activity of the catalyst is improved. Therefore, the environmental problems caused by easy agglomeration of VO-M-Co3O4 and leaching of Co ions are solved; the catalyst shows good reaction stability, has enough visible light absorption capability and relatively strong peroxymonosulfate (PMS) activation capability, and realizes efficient degradation of an organic pollutant atrazine (ATZ) which is difficult to remove. In the aspect of application, the system is different from a traditional degradation system depending on O2, the ATZ degradation efficiency of the VO-M-Co3O4 (at) CNx under the anaerobic condition is far higher than the ATZ degradation efficiency under the aerobic condition through multiple synergistic degradation paths, it is indicated that the VO-M-Co3O4 (at) CNx can achieve ATZ catalytic degradation without aeration, the water treatment cost is greatly reduced, and the application prospect is wide. The method has potential practical application value in the field of advanced oxidation treatment of wastewater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the fields of advanced oxidation wastewater treatment and photocatalytic nanocomposite material technology, and in particular to a preparation method and application of a durable and stable advanced oxidation catalyst that does not require aeration. Background Art

[0002] Pesticides have the function of preventing and controlling crop diseases and ensuring the normal growth of crops. They are widely used in agricultural and food industry production to meet the growing food demand brought about by the world's population explosion. However, the large-scale use of various pesticides has brought about various environmental problems. Taking the widely used atrazine (ATZ) as an example, due to its stable s-triazine structure, long half-life, low biodegradability, it will still remain toxic and residual in the ecological environment in trace amounts, posing a high risk to human health and the ecosystem, and restricting the sustainable development of agriculture. Therefore, it is crucial to seek an effective and sustainable treatment technology to eliminate the ecological and environmental risks of ATZ in the water environment. The Fenton-like process based on peroxymonosulfate (PMS) has been proven to be a clean and effective technology for the treatment of persistent organic pollutants by catalytically activating PMS to produce reactive oxygen species (ROS). Among them, the asymmetric structure (HO-OSO3 - ) and PMS with longer OO bonds can be catalyzed by external field energy (heat, light, ultrasound, microwaves, etc.), transition metal ions / compounds (Co 2+ , Fe 2+ , Co3O4, etc.) and metal-free materials (carbon-based, boron-based and sulfur-based). Among the above activation methods, photocatalysts can continuously generate abundant photogenerated electrons under light irradiation, which is considered to be a more effective and cost-effective strategy for activating PMS. It has been reported that there is no significant difference in the removal efficiency of pollutants under aerobic and anaerobic conditions in Fenton-like degradation systems, which may be due to the fact that the O in the active oxygen is not derived from dissolved oxygen, but from PMS. It is well known that in traditional photocatalytic degradation systems, the O in the active oxygen is usually overly dependent on the forced convection of oxygen (O2) atmosphere and air, which greatly limits its large-scale application in industry. Traditional photo-Fenton-like degradation systems rely heavily on the energy consumption of O2 transportation and forced convection, which will greatly increase the treatment cost. According to statistics, aeration accounts for 35-51% of the total energy consumption in wastewater treatment, with an annual energy consumption of 500-750 million kWh. Therefore, it becomes crucial to design and develop aeration-free photocatalyst photo-Fenton-like systems to effectively promote the activation of PMS and remove persistent organic pollutants and have good application prospects.

[0003] Graphitic carbon nitride (CN) is composed of abundant elements on the earth and has attracted widespread attention from researchers in the field of environmental remediation due to its suitable band gap (2.7 eV), visible light response, and PMS activation ability. It is reported that CNs with different degrees of defects were prepared by thermal polymerization of several precursors (melamine, thiourea, and their mixtures). These structural defects are formed due to the inevitable loss of nitrogen atoms in the CN framework during the thermal polymerization process. N vacancies, as a special internal defect of CN, have been confirmed to be beneficial to light-assisted PMS activation. After the loss of N atoms, lone pairs of electrons are presented, making it easy to accept electrons or interact with electron-rich substances, and easily attract negatively charged PMS or interact with PMS (Science of The Total Environment, (2021, 756:144139). In addition, CN is 1 It shows high activity in the non-radical degradation of pollutants mainly based on O2, and shows good anti-interference ability to coexisting substances. The donor-acceptor engineered g-C3N4 designed by Weng et al. (Journal of Hazardous Materials, 2023, 448: 130869) selectively removes ATZ through PMS photocatalytic activation, and the removal performance of ATZ under aerobic and anaerobic conditions remains almost unchanged. This shows that it is feasible and promising to construct a CN-based photocatalyst activated PMS-like Fenton system to remove organic pollutants. However, for single-component photocatalysts, the PMS activation kinetics are slow, the light adsorption performance is poor, and the photoinduced electron-hole pair recombination is fast, resulting in pollutant degradation activity that is far from satisfactory. In recent years, the S-type heterojunction developed has a unique charge migration pathway and strong photoredox ability because the electrons and holes generated by the photoexcited heterojunction accumulate in the more negative conduction band (CB) and the more positive valence band (VB) positions, respectively. At present, the excellent performance of CN-based S-type heterojunction photocatalytic system in photocatalytic degradation of environmental pollutants has been demonstrated (Science China Materials 2024, 67(2): 444-472). The cobalt-based Fenton process has been proven to be an effective means of activating PMS, which can rely on PMS to act as both an electron donor and an acceptor to generate ROS to attack organic pollutants. Among the candidate materials for constructing heterojunctions, Co3O4 has a narrow band gap of 1.7-2.0 eV, which can be activated by Co III / Co IIReduction induces PMS activation at the active site and is considered to be a promising PMS activator. However, cobalt ions in Co3O4 can easily escape from Co3O4, resulting in secondary pollution and reduced catalytic activity. After four cycles, the pollutant degradation performance of Co3O4@C-500 prepared by Sheng et al. (Chemical Engineering Journal, 2023, 471: 143945) dropped from 100% to 64%.

[0004] In summary, the prior art has the following problems:

[0005] (1) The traditional Fenton-like photocatalytic degradation system relies heavily on the energy consumption of O2 transport and forced convection, which will greatly increase the treatment cost. The harsh reaction conditions and high energy consumption are not conducive to the practical application of advanced oxidation treatment technology in the wastewater field;

[0006] (2) Although Co-based catalysts have shown a certain ability to activate PMS, due to structural instability and the complexity of the use environment, a large amount of cobalt leaching is inevitable. Co ions easily accumulate in the environment, which has a significant impact on the ecological environment and human health;

[0007] (3) Fenton-like photocatalysts have low utilization rates of visible light absorption in sunlight, high recombination rates of photogenerated electron-hole pairs, few active sites for catalytic reactions, and slow activation rates of PMS, resulting in low catalytic degradation efficiency. Summary of the invention

[0008] The technical problems to be solved by the present invention are as follows:

[0009] (1) The present invention designs and constructs a new type of carbon nitride-based S-type heterojunction Fenton-like photocatalyst with double defect sites, which does not require aeration of the reaction system, has low energy consumption, and a simple and easy preparation process, which is conducive to the large-scale application of advanced oxidation treatment technology in the field of wastewater. This solves the problem of high energy consumption of the current traditional photo-Fenton-like technology for treating difficult-to-degrade organic pollutants.

[0010] (2) Cobalt ions in Co3O4 can easily escape, causing secondary environmental pollution, reducing catalytic activity and showing poor PMS activation ability. On the one hand, the present invention selects a porous zeolite imidazolate framework (ZIF-67) as a precursor, and pyrolyzes V in an inert atmosphere and air respectively. O -M-Co3O4 photocatalyst improves its stability and conductivity, where the obtained V O-The presence of oxygen vacancies (Vo) in M-Co3O4 provides abundant active sites, increases the speed of electron generation, accelerates PMS activation and thus enhances the generation of ROS; on the other hand, the present invention introduces an oxygen-rich polymer PEG as a structure-directing agent to soften the nitrogen-defective carbon nitride CN x Carrier, realize CN x V O -M-Co3O4 coating makes V O -M-Co3O4 is highly dispersed and has a large number of PMS activation sites to solve the problem of V O -M-Co3O4 is easy to agglomerate and has environmental problems caused by Co ion leaching.

[0011] (3) Currently, the photo-Fenton-like catalysts have fewer active sites, which leads to reduced PMS activation performance and low Fenton-like photocatalytic degradation efficiency. The carbon nitride-based S-type heterojunction Fenton-like photocatalyst material with double defect sites prepared by the present invention can coordinate the directional migration path of photogenerated carriers under the action of built-in electric field and Coulomb attraction to transfer to the surface, thereby improving the PMS activation performance and accelerating the reaction rate, thereby greatly enhancing its catalytic degradation efficiency.

[0012] In order to solve the problems of the prior art, the technical solution adopted by the present invention is:

[0013] A method for preparing a durable and stable advanced oxidation catalyst without aeration and its application, by introducing an oxygen-rich polymer-assisted hydrothermal method to prepare V O -M-Co3O4@CN x The advanced oxidation catalyst specifically comprises the following steps:

[0014] Step 1, weigh 8-12g of urea and put it into a 50-150mL covered ceramic crucible, calcine at a certain temperature and a certain heating rate, the ambient temperature is 25-35°C, and the relative humidity is about 65-85%. The obtained catalyst is named CN x ;

[0015] Step 2, weigh 750-900 mg Co(NO3)2·6H2O and 1200-2000 mg 2-methylimidazole and dissolve them in methanol solution. Then stir the mixed solution rapidly and age at room temperature. The obtained precipitate is washed with ethanol and then dried at 50-80°C overnight to obtain the precursor ZIF-67;

[0016] Step 3, the dried ZIF-67 precursor is kept at a certain temperature for a certain time under the protection of high-purity N2, cooled to room temperature with the furnace, and then calcined in air at a certain temperature for a certain time. The obtained catalyst is named V O -M-Co3O4;

[0017] Step 4: Set a certain proportion of V O -M-Co3O4 was prepared into a water dispersion and sealed with plastic wrap, ultrasonicated, and then stirred at a certain temperature for a period of time using a magnetic stirrer. At the same time, a certain amount of CN x Mix with oxygen-containing polymer, dilute with a certain volume of deionized water, stir for 5-20 minutes, and then add different volumes of V O -M-Co3O4 solution to a certain volume. Subsequently, the composite solution was stirred for 0.5-2h, moved to a reactor, and after hydrothermal treatment. After cooling to room temperature, it was washed with deionized water and anhydrous ethanol, and dried at 50-80°C overnight to obtain a composite material named Y%V O -M-Co3O4@CN x ,Y represents V O -Theoretical addition amount of M-Co3O4.

[0018] As an improvement, the calcination conditions in step 1 are calcined at 450-600°C for 2°C min -1 ,4h.

[0019] As an improvement, the aging time in step 2 is 20-40 hours.

[0020] As an improvement, the heating rate in step 3 is 1-5℃min -1 The first calcination temperature is 450-550℃, the insulation time is 10-50min, the second calcination temperature is 300-400℃, the insulation time is 1-5h.

[0021] As an improvement, in step 4, the oxygen-containing polymer is polyethylene glycol PEG, the hydrothermal reaction conditions are 100-200° C., the reaction time is 8-20 h, and the value of Y is 1-10 wt %.

[0022] The catalyst obtained by the above preparation method is applied in the field of advanced oxidation synergistic photocatalysis to treat organic pollutants in wastewater without aeration, thereby achieving efficient removal thereof.

[0023] Beneficial effects:

[0024] Compared with the prior art, the preparation method of a durable and stable advanced oxidation catalyst without aeration and its application in the present invention have the following advantages:

[0025] (1) The present invention uses carbon nitride CN containing nitrogen defects x As a carrier, the oxygen-rich polymer PEG was introduced to assist in the preparation of an S-type heterojunction V with double defects. O -M-Co3O4@CN x Catalysts increase their reactive sites and greatly improve pollutant removal efficiency, especially 5% VO -M-Co3O4@CN x , the degradation efficiency under air conditions reaches 0.12min -1 , is a pure CN catalyst (0.011min -1 ) is 10.9 times that of V O -M-Co3O4 removes 5 times more organic pollutants. This shows that the technology provided by the present invention can greatly enhance the catalytic removal efficiency of pollutants;

[0026] (2) To solve the problems of cobalt ions in Co3O4 escaping easily, causing secondary environmental pollution, reducing catalytic activity and showing poor PMS activation ability. On the one hand, the present invention selects a porous zeolite imidazolate framework (ZIF-67) as a precursor, and pyrolyzes it under atmosphere to obtain a Vo-M-Co3O4 photocatalyst to improve its stability and conductivity, wherein the oxygen vacancies (V O ) provides abundant active sites, increases the speed of photogenerated electron generation, accelerates PMS activation and thus enhances the generation of ROS; on the other hand, the present invention introduces an oxygen-rich polymer PEG as a structure-directing agent to soften the nitrogen-defective carbon nitride CN X Carrier, realize CN x V O -M-Co3O4 coating makes Vo-M-Co3O4 highly dispersible, which is conducive to the efficient activation of PMS;

[0027] (3) The present invention constructs a novel catalytic system for activating PMS to degrade organic pollutants using a carbon nitride-based S-type heterojunction advanced oxidation catalyst with dual defect sites that does not require aeration. The preparation process is simple and easy, and there is no need to aerate the reaction system, the energy consumption is low, and it is suitable for large-scale application. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 Monomer CN prepared for different examples x and V O -M-Co3O4 and different proportions of V O -M-Co3O4 added amount of composite sample V O -M-Co3O4@CN x XRD spectra of the catalysts, wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, (d) is Example 4, and (e) is Example 5;

[0029] Figure 2 The monomer CN prepared by different methods x and V O -M-Co3O4 and V O -M-Co3O4@CN xTransmission electron microscope (TEM) images of the catalyst, wherein (a) is Example 1, (b) is Example 2, and (c) is Example 4;

[0030] Figure 3 (A) Figure 3 (B) are respectively V prepared in Example 1 and Example 4 of the present invention O -M-Co3O4@CN x In-situ and ex-situ XPS spectra of high-resolution C1s and N 1s, where (a) is Example 1 and (b) is Example 4;

[0031] Figure 3 (C) Figure 3 (D) is V prepared in Examples 2 and 4 of the present invention O -M-Co3O4@CN x High-resolution XPS spectra of Co 2p and O 1s in-situ and ex-situ XPS spectra, where (a) is Example 2 and (b) is Example 4;

[0032] Figure 4 (A) is the monomer CN prepared by different methods of the present invention x and V O -M-Co3O4 and different proportions of V O -M-Co3O4 added amount of composite sample V O -M-Co3O4@CN x A linear graph showing the change in the rate of degradation of organic pollutants by photocatalysis in coordination with PMS activation, wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, (d) is Example 4, and (e) is Example 5;

[0033] Figure 4 (B) is the monomer CN prepared by different methods of the present invention x and V O -M-Co3O4 and different proportions of V O -M-Co3O4 added amount of composite sample V O -M-Co3O4@CN x A bar graph showing the rate of photocatalytic synergistic PMS activation degradation of organic pollutants by the catalyst, wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, (d) is Example 4, and (e) is Example 5;

[0034] Figure 5 CN prepared in Examples 1 and 4 of the present invention x and V O -M-Co3O4@CN xLinear graph for the change in the rate of degradation of organic pollutants by photocatalytic synergistic PMS activation under air (aerobic) and argon (anaerobic) conditions, wherein (a) is Example 1 and (b) is Example 4;

[0035] Figure 6 V prepared in Example 4 of the present invention O -M-Co3O4@CN x The bar graph of the degradation rate of organic pollutants by photocatalysis and PMS activation after 6 cycles of the catalyst and the Co ion concentration leaching diagram during the cycle reaction;

[0036] Figure 7 The monomer CN prepared by different methods of the present invention x and V O -M-Co3O4 and different proportions of V O -M-Co3O4 added amount of composite sample V O -M-Co3O4@CN x Catalyst UV-visible absorption spectrum (DRS) diagram, wherein (a) is Example 1, (b) is Example 2, (c) is Example 3, (d) is Example 4, and (e) is Example 5;

[0037] Figure 8 V under different methods of the present invention O -M-Co3O4@CN x Photocurrent response diagram of the catalyst, where (a) is Example 1, (b) is Example 2, and (c) is Example 4. DETAILED DESCRIPTION

[0038] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art in the art described herein. Although the present invention only describes preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials related to the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0039] Example 1CN x Catalyst preparation

[0040] Weigh 10g of urea into a 100mL ceramic crucible with a lid and heat at 550℃ at 2℃min. -1 The catalyst was synthesized under the conditions of calcination for 4 hours, ambient temperature of 25-35°C, and relative humidity of about 65-85%. x .

[0041] Example 2VO - Preparation of M-Co3O4 catalyst

[0042] 875 mg Co(NO3)2·6H2O and 1600 mg 2-methylimidazole were weighed and dissolved in 20 mL methanol solution. The mixed solution was then stirred rapidly and aged at room temperature. The obtained precipitate was washed with ethanol and then dried at 50-80°C overnight to obtain the precursor ZIF-67. The dried ZIF-67 precursor was kept at 550°C for 30 min under high-purity N2 protection, cooled to room temperature with the furnace, and then calcined at 350°C in air for 2 h.

[0043] Example 3 1% V O -M-Co3O4@CN x Catalyst preparation

[0044] 2mgV O -M-Co3O4 was prepared into an aqueous solution and sealed with plastic wrap, ultrasonicated, and then stirred at a certain temperature for a period of time with a magnetic stirrer. At the same time, 200 mg of CN x Mix with 2 mL PEG, dilute with a certain volume of deionized water, stir for 10 minutes, and then add different volumes of V O -M-Co3O4 solution to a certain volume. Subsequently, the composite solution was stirred for 1 hour, transferred to a reactor, and subjected to hydrothermal treatment at 140°C for 12 hours. After cooling to room temperature, it was washed with deionized water and anhydrous ethanol three times, and dried at 50-80°C overnight to obtain a composite material named 1% V O -M-Co3O4@CN x , where V O -The added amount of M-Co3O4 was 1wt%.

[0045] Example 4 5% V O -M-Co3O4@CN x Preparation of photocatalyst

[0046] 10mgV O -M-Co3O4 was prepared into an aqueous solution and sealed with plastic wrap, ultrasonicated, and then stirred at a certain temperature for a period of time with a magnetic stirrer. At the same time, 200 mg of CN x Mix with 2 mL PEG, dilute with a certain volume of deionized water, stir for 10 minutes, and then add different volumes of V O -M-Co3O4 solution to a certain volume. Subsequently, the composite solution was stirred for 1 hour, transferred to a reactor, and subjected to hydrothermal treatment at 140°C for 12 hours. After cooling to room temperature, it was washed with deionized water and anhydrous ethanol three times, and dried at 50-80°C overnight to obtain a composite material named 5% V O -M-Co3O4@CNx , where V O -The added amount of M-Co3O4 is 5wt%.

[0047] Example 5 10% V O -M-Co3O4@CN x Preparation of photocatalyst

[0048] 20mgV O -M-Co3O4 was prepared into an aqueous solution and sealed with plastic wrap, ultrasonicated, and then stirred at a certain temperature for a period of time with a magnetic stirrer. At the same time, 200 mg of CN x Mix with 2 mL PEG, dilute with a certain volume of deionized water, stir for 10 minutes, and then add different volumes of V O -M-Co3O4 solution to a certain volume. Subsequently, the composite solution was stirred for 1 hour, transferred to a reactor, and subjected to hydrothermal treatment at 140°C for 12 hours. After cooling to room temperature, it was washed with deionized water and anhydrous ethanol three times, and dried at 50-80°C overnight to obtain a composite material named 10% V O -M-Co3O4@CN x , where V O -The added amount of M-Co3O4 is 10wt%.

[0049] Morphology and characterization tests

[0050] 1. Material Characterization

[0051] 1.XRD analysis

[0052] Figure 1 XRD patterns of different catalysts prepared in Examples 1-8, Figure 2 a is different initial mass composition V O -M-Co3O4@CN x X-ray diffraction (XRD) pattern of the sample. O -M-Co3O4@CN x The crystal structure of the (100) and (002) planes corresponds to two CN x Diffraction peaks. Among them, the weaker and broader peak appearing on the (100) plane is attributed to CN x There are nitrogen vacancies (V N ), this is due to CN x The long-range order of the in-plane structure filling is low. By comparing with the Co3O4 standard card (JCPDS.42-1467) as a reference, it is found that V O -M-Co3O4 peaks are in good agreement with the standard mode spectrum, indicating that V O-M-Co3O4 formation. Among them, the characteristic peaks of the XRD spectrum of the material at 2θ=19.0°, 31.2°, 36.8°, 44.8°, 59.4° and 65.3° correspond to the (111), (220), (311), (400), (511) and (440) crystal planes respectively. It can be found that V O -M-Co3O4@CN x The XRD patterns of the samples contain CN x and V O -M-Co3O4 diffraction peaks, indicating that CN x and V O -M-Co3O4 coexists. Figure 1 It can be seen that V O -M-Co3O4@CN x The (002) peak of V O -M-Co3O4 shows a small displacement to a higher angle, indicating that the introduction of PEG causes the CN interlayer to shrink.

[0053] 2. Morphology Analysis

[0054] Further analysis of the morphological characteristics of the catalyst materials prepared by the research. Figure 2 (a) is the TEM image of the sample prepared in Example 1, showing that the synthesized photocatalyst has a lamellar morphology. Figure 2 (b) TEM image of the composite sample prepared in Example 3 shows that with the help of the oxygen-containing polymer PEG, V O -M-Co3O4 species through softening of CN x The morphological structure makes it well covered, and V O -M-Co3O4 in CN x Highly dispersed in.

[0055] 3.XPS analysis

[0056] Ex situ XPS can characterize the material composition, valence state and defects of photocatalytic materials. Figure 3 (A) is the XPS C 1s graph of the samples prepared in Example 1 and Example 4. x The high-resolution C1s XPS spectrum (a) shows that CN x The NC=N in the aromatic ring CC(sp 2 ), CO / C-NH2 and sp 2 Hybridized carbon has three obvious peaks at 288.10, 286.19 and 284.79 eV, respectively. O -M-Co3O4@CN x(b) shifts 0.10 eV in the negative direction. Figure 3 (B) Original CN x The N1s XPS spectrum of the nanostructured carbon nanotubes can be well decomposed into four peaks at 404.30, 400.98, 399.30 and 398.48 eV (a), which are respectively attributed to CN x π excitation, CNH, N-(C3) and C=NC peaks. O -M-Co3O4@CN x The π excitation peak corresponding to sample (b) showed a positive shift of 0.1 eV, while CNH, N-(C3) and C=NC showed negative shifts of 0.2 eV, 0.2 eV and 0.1 eV respectively. x of 0.98 increases to V O -M-Co3O4@CN x 1.07, higher than CN x The theoretical value is 0.75. x Nitrogen vacancies (V N ) is formed due to the thermal polymerization process of CN x The loss of nitrogen atoms in the framework and the V O -M-Co3O4@CN x Medium V N The increase is due to the V O -Coupling of M-Co3O4.

[0057] Figure 3 (C) is the XPS of the samples prepared in Example 2 and Example 4. Through high-resolution Co 2p XPS spectra, V O The Co 2p spectrum of -M-Co3O4(a) consists of two asymmetric peaks, namely: Co 2+ (2p 1 / 2 :795.91eV; 2p 3 / 2 :780.80eV) and Co 3+ (2p 1 / 2 :794.30eV); 2p 3 / 2 :779.26eV), while the peaks at 803.51eV and 787.29eV may be V O -M-Co3O4 satellite peaks. In addition, the peak area ratio was calculated to obtain Co 2+ / Co 3+ The atomic ratio of V is 1.86, which is significantly deviated from the theoretical value of 0.5. O -M-Co3O4@CN x (b) The atomic ratio in the sample increases to 1.87. According to the law of electrical neutrality, it can be inferred that the excess Co 2+ In VO -M-Co3O4 and V O -M-Co3O4@CN x There is V O This conclusion is further confirmed by its O1s spectrum. Figure 3 (D) is the O1s XPS spectra of the samples prepared in Example 2 and Example 4; the three characteristic peaks at 532.61, 531.7 and 529.50 eV are caused by the adsorption of oxygen (O ads ), 531.1eV surface chemically adsorbed oxygen (O S ) and metal-oxygen bond lattice oxygen (O L ). Consider O S / O L The ratio of surface oxygen vacancies (V O ) relative amount, the higher the ratio, the higher the surface V O The calculation results show that V O The relative amount of oxygen vacancies on the surface of M-Co3O4 is 44%, indicating that V O -M-Co3O4 is rich in V O . V O -M-Co3O4@CN x The higher O S / O L The value is as high as 0.66%, indicating that there are more V O , which may be due to the higher Co 2+ / Co 3+ Increased V O concentration. In addition, with V O -M-Co3O4(a) compared with V O -M-Co3O4@CN x (b) The Co 2p spectrum and O1s spectrum of the sample also shifted toward the direction of lower binding energy, indicating that V O -M-Co3O4 and CN x There is a strong interfacial interaction between them, which is beneficial to electron transfer and the construction of S-type heterostructures.

[0058] Figure 3 The in-situ XPS (b+ light) spectrum of the sample prepared in Example 4 can be seen due to V O -M-Co3O4@CN x The strong interaction at the interface was shown, and the migration of photoexcited electrons was monitored by in situ XPS under xenon lamp illumination, demonstrating an S-type charge transfer route. Figure 3 As shown in (AB), V O -M-Co3O4@CNx The peak positions of C1s and N1s of the heterojunction are positively shifted relative to those in the ex situ spectrum, while V O -M-Co3O4@CN x The O1s of the heterojunction undergoes a negative shift toward the direction of greater binding energy ( Figure 3 (D)). The shift in binding energy indicates that CN x The electron density of V O -The electron density of M-Co3O4 increases, indicating that CN x The photoexcited electrons in the CB migrate to V under light. O -M-Co3O4 in the VB follows the proposed S-type charge transfer route.

[0059] Performance Testing

[0060] 1. Test method for Fenton-type photocatalytic performance in aerobic system

[0061] A 250mL double-layer jacketed beaker was used as the reactor for the pollutant degradation performance test. Circulating cooling water was introduced into the jacket of the double-layer jacketed beaker to eliminate the heat generated by the light source during the catalytic reaction, thereby ensuring that the photocatalytic water decomposition hydrogen production performance test was carried out at room temperature and pressure. O -M-Co3O4@CN x The photocatalytic performance of the S-type heterojunction was tested by adding 10 mg of photocatalyst to 50 mL of ATZ solution (10 mg L -1 ). First, balance in the dark for 30 minutes to reach adsorption-desorption equilibrium. After adsorption equilibrium, add 0.6mM PMS, turn on the light source, take out 0.8mL of degradation solution every 6 minutes, filter with 0.22μm nylon membrane, and then immediately stop the reaction with 200μL methanol. During the reaction, the degradation products are analyzed by liquid chromatography-mass spectrometry (LC-MS) system.

[0062] 2. Test method for Fenton photocatalytic performance of anaerobic system catalysis

[0063] Anaerobic system: Except changing the continuous air pump to continuous Ar into the catalytic system to remove dissolved oxygen or generate oxygen during the reaction, other test methods remain unchanged.

[0064] Figure 4 The catalysts prepared in Examples 1-5 were used to study the photocatalytic activity of V in a Fenton-like system under forced convection atmospheric conditions. O -M-Co3O4@CN xThe ability of detecting pollutant ATZ (10 mg / L) by activating PMS under visible light irradiation. Figure 4 (A) reflects the efficiency of different catalysts in degrading organic pollutants with the illumination time. It can be seen that V O -M-Co3O4@CN x Exhibits excellent photoactivation capability of PMS, with V O -M-Co3O4 and CN x Compared with ATZ, the removal efficiency is significantly improved. O -M-Co3O4@CN x The removal rate of ATZ was the highest, reaching 97.80% degradation rate within 30 minutes. Figure 4 Based on the data of (A), the reaction rate (k) of catalyst degradation of ATZ was calculated according to the pseudo-first-order kinetic model, as shown in Figure 4 (B) As shown. Pure CN prepared by Example 1 x V prepared in Example 2 O -M-Co3O4 reaction rate is only 0.011 and 0.024min -1 , V prepared by Example 3-5 O -M-Co3O4@CN x At 1wt%, 5wt% and 10wt% V O -M-Co3O4 added, the reaction rates were 0.063, 0.12, and 0.11 min, respectively -1 , combined with Figure 4 (A) It can be found that the catalytic activity of the catalyst in Example 4 is the highest, reaching 0.12 min -1 .

[0065] Figure 5 The catalysts prepared in Example 1 and Example 4 were evaluated for V under an oxygen-free atmosphere (Ar). O -M-Co3O4@CN x The Fenton-like photocatalytic performance of the NH4Cl2O3 was used to support the construction of the aeration-free system. x With V O -M-Co3O4@CN x The degradation of ATZ was not only not inhibited, but was significantly improved, proving that the system can efficiently degrade pollutants without the presence of oxygen, and successfully constructed a new aeration-free carbon nitride-based catalyst catalytic system for activating PMS to degrade organic pollutants.

[0066] Figure 6 The activity diagram of the visible light synergistic PMS catalytic degradation of pollutants and the Co ion leaching experiment during the reaction process of the sample prepared in Example 4 after 6 cycles of experiments are shown in FIG. Figure 6As shown, it is found that V O -M-Co3O4@CN x After 6 cycles of testing, it showed excellent photocatalytic durability and repeatability, and the leaching amount of Co ions was less than 0.4 mg / L, indicating that V O -M-Co3O4@CN x The catalyst has high stability and low Co ion leaching and is environmentally friendly.

[0067] Photoelectrochemical characterization

[0068] Figure 7 The DRS diagrams of the catalysts prepared in Examples 1, 2, 3, 4 and 5 show that V O -The introduction of M-Co3O4 can enhance the CN x Visible light absorption intensity, thereby improving the absorption and utilization rate of visible light in sunlight.

[0069] Figure 8 The photocurrent response comparison diagram of the photocatalysts in Example 1, Example 2, and Example 4 shows that V O -M-Co3O4@CN x The photocatalyst has a higher separation and migration rate of photogenerated carriers, which indicates that V O -The introduction of M-Co3O4 inhibits the x The recombination of photogenerated electron-hole pairs indicates that the construction of S-type heterojunction greatly improves the CN x Catalytic degradation efficiency.

[0070] In summary, the present invention discloses a method for preparing a carbon nitride-based S-type heterojunction Fenton-like photocatalyst with double defect sites. Characterization results show that the carbon nitride with nitrogen defects in the lamellar structure CN X As a carrier, an oxygen-rich polymer was introduced as a structure-directing agent to soften CN X , then implement CN X MOF-derived V O -M-Co3O4 coating, showing extremely high stability and reusability during the reaction process, and the degradation efficiency under air conditions reached 0.12min -1 , is a pure CN catalyst (0.011min -1 ) is 10.9 times that of V O -M-Co3O4(0.024min -1 ) can remove 5 times more organic pollutants. The increase in the rate of hydrogen production from water can be attributed to the effective separation and migration of photogenerated charges and the enhanced activation ability of PMS. In addition, from an application perspective, unlike traditional degradation systems that rely on O2, V O-M-Co3O4@CN x The efficiency of ATZ degradation through multiple synergistic pathways under anaerobic conditions is much higher than that under aerobic conditions, indicating that V O -M-Co3O4@CN X ATZ catalytic degradation can be achieved without aeration, which greatly reduces the cost of water treatment and has potential practical application value in the field of advanced oxidation wastewater treatment.

[0071] The above is only a preferred specific implementation manner of the present invention, and the protection scope of the present invention is not limited thereto. Any simple change or equivalent replacement of the technical solution that can be obviously obtained by any technician familiar with the technical field within the technical scope disclosed in the present invention falls within the protection scope of the present invention.

Claims

1. A method for preparing a durable and stable advanced oxidation catalyst without aeration and its application, characterized in that: Preparation of V by introducing oxygen-rich polymer-assisted hydrothermal method O -M-Co3O4@CN X The advanced oxidation catalyst specifically comprises the following steps: Step 1, weigh 8-12g of urea and put it into a 50-150mL covered ceramic crucible, calcine at a certain temperature and a certain heating rate, the ambient temperature is 25-35°C, and the relative humidity is about 65-85%. The obtained catalyst is named CN x ; Step 2, weigh 750-900 mg Co(NO3)2·6H2O and 1200-2000 mg 2-methylimidazole and dissolve them in methanol solution. Then stir the mixed solution rapidly and age at room temperature. The obtained precipitate is washed with ethanol and then dried at 50-80°C overnight to obtain the precursor ZIF-67; Step 3, the dried ZIF-67 precursor is kept at a certain temperature for a certain time under the protection of high-purity N2, cooled to room temperature with the furnace, and then calcined in air at a certain temperature for a certain time. The obtained catalyst is named V O -M-Co3O4; Step 4: Set a certain proportion of V O -M-Co3O4 was prepared into an aqueous solution and sealed with plastic wrap, ultrasonicated, and then stirred at a certain temperature for a period of time using a magnetic stirrer. At the same time, a certain amount of CN x Mix with oxygen-containing polymer, dilute with a certain volume of deionized water, stir for 5-20 minutes, and then add different volumes of V O -M-Co3O4 solution to a certain volume. Subsequently, the composite solution was stirred for 0.5-2h, transferred to a reactor, and after hydrothermal treatment. After cooling to room temperature, it was washed with deionized water and anhydrous ethanol, and dried at 50-80°C overnight to obtain a composite material named Y%V O -M-Co3O4@CN x ,Y represents V O -Theoretical addition amount of M-Co3O4.

2. The method for preparing a durable and stable advanced oxidation catalyst without aeration and its application according to claim 1, characterized in that: In step 1, the calcination conditions are 450-600℃ for 2℃min. -1 ,4h.

3. The method for preparing a durable and stable advanced oxidation catalyst without aeration and its application according to claim 1, characterized in that: The aging time in step 2 is 20-40h.

4. The method for preparing a durable and stable advanced oxidation catalyst without aeration and its application according to claim 1, characterized in that: The heating rate in step 3 is 1-5℃min -1 The first calcination temperature is 450-550℃, the insulation time is 10-50min, the second calcination temperature is 300-400℃, the insulation time is 1-5h.

5. The method for preparing a durable and stable advanced oxidation catalyst without aeration and its application according to claim 1, characterized in that: In step 3, the oxygen-containing polymer is polyethylene glycol (PEG), the hydrothermal reaction conditions are 100-200° C., the reaction time is 8-20 h, and the value of Y is 1-10 wt %.

6. Use of an advanced oxidation catalyst prepared by any one of claims 1 to 5 and containing an S-type carbon nitride-based heterojunction having double defect sites and not requiring aeration in catalytic water treatment.

Citation Information

Patent Citations

  • Cobaltosic oxide dodecahedron / carbon nitride nanosheet composite and application thereof in waste gas treatment

    CN110180570A

  • C3N4 / LaVO4 composite photocatalyst and preparation method thereof

    CN111036272A

  • Carbon-coated carbon nitride nanowire, preparation method thereof and application thereof in photocatalytic degradation of bisphenol A

    CN111672531A

  • Oxygen-doped carbonitride / Co3O4 heterojunction photocatalyst as well as preparation method and application thereof

    CN117861706A