Bifunctional composite catalyst for olefin metathesis and cracking

The multifunctional composite catalyst prepared by spray drying solves the problem of reducing reaction system efficiency caused by the settlement of individual catalysts, and achieves the effect of efficient production of propylene, reducing costs and improving reaction efficiency.

CN118976534APending Publication Date: 2024-11-19SAUDI ARABIAN OIL CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411063891.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-12-02
Filing Date
2020-05-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

In the prior art, when producing propylene, the settlement of the individual catalyst leads to reduced efficiency and increased costs of the reaction system, and it is unable to effectively cope with the rapid growth in the demand for propylene.

Method used

A multifunctional composite catalyst is used to prepare a catalyst precursor mixture by spray drying, so that the catalytically active compounds are deposited on the surface of the catalyst support material and zeolite particles to form evenly distributed catalyst particles, reducing settlement problems and improving reaction efficiency.

Benefits of technology

It is possible to perform multiple catalytic reactions without the need for multiple catalyst materials, reducing reactor dead zones, improving propylene selectivity and yield, and reducing production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976534A_ABST
    Figure CN118976534A_ABST
Patent Text Reader

Abstract

A composite catalyst comprises zeolite particles at least partially embedded in a catalyst support material and at least one catalytically active compound deposited on outer surfaces and pore surfaces of the catalyst support material, zeolite particles, or both. A method of preparing the composite catalyst may include preparing a catalyst precursor mixture including the zeolite, a catalyst support material, a triblock copolymer surfactant, and a catalytically active compound precursor, and spray drying the catalyst precursor mixture. The composite catalyst can be used as a single catalyst for performing olefin metathesis and cracking reactions. A process for producing propylene can include contacting a butene-containing feed with the composite catalyst.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] Description of the case

[0002] This application is a divisional application of an invention patent application with an application date of May 5, 2020, a national application number of 202080078210.6, and an invention name of “Bifunctional composite catalyst for olefin metathesis and cracking”.

[0003] CROSS-REFERENCE TO RELATED APPLICATIONS

[0004] This application claims priority to U.S. non-provisional patent application serial number 16 / 700,197, filed on December 2, 2019, the entire contents of which are incorporated by reference into this disclosure. Technical Field

[0005] The present disclosure relates to hydrocarbon processing, and in particular to composite catalysts and methods of making composite catalysts for performing olefin metathesis and cracking. Background Art

[0006] In recent years, the demand for propylene has increased dramatically to supply the growing markets for polypropylene, propylene oxide and acrylic acid. Currently, most of the propylene produced globally (74 million tons / year) is produced as a by-product from steam cracking units (57%), which mainly produce ethylene, or as a by-product from fluid catalytic cracking (FCC) units (30%), which mainly produce gasoline. These methods cannot fully cope with the rapid growth in propylene demand.

[0007] Producing propylene by butene-containing streams (such as raffinate streams or other butene-containing streams) can be accomplished by metathesis of butenes into propylene and other compounds and combined cracking, isomerization or both. Some propylene processes include metathesis, isomerization and cracking, so as to increase the overall yield and propylene selectivity of the reaction system. Each reaction in these types of reactions may require different types of catalysts, such as cracking catalysts for cracking reactions, metathesis catalysts for metathesis reactions and isomerization catalysts for isomerization reactions. In conventional reaction systems for converting butenes into propylene, separate catalysts can be separated in separate catalyst zones, such as by loading each separate catalyst into separate reactors or by loading catalysts into single reactors, and separating each catalyst with inert spacers such as quartz wool or silicon carbide. Catalyst separation into separate reactor vessels significantly increases the initial capital cost of the reaction system. In addition, separating catalysts with inert spacers can produce dead volume in the reactor, which may reduce the efficiency of the reactor.

[0008] In order to reduce costs and eliminate dead zones, a physical catalyst mixture of two or more separate solid particulate catalyst materials can be used. However, due to sedimentation with continued use and handling, these physical catalyst mixtures of different solid catalyst materials may gradually separate in the reactor over time. For example, when the physical properties of a separate solid particulate catalyst material are significantly different from other catalyst materials in the physical catalyst mixture, this separation or sedimentation effect may become more and more intense. Therefore, as the separate catalyst is separated by sedimentation, the effectiveness of the physical catalyst mixture of solid catalyst particles may decrease over time. Summary of the invention

[0009] Therefore, there is a continuing need for a multifunctional composite catalyst and a method for synthesizing a composite catalyst. The present disclosure relates to a multifunctional composite catalyst and a method for producing a composite catalyst. The composite catalyst of the present disclosure may include a plurality of composite catalyst particles and each composite catalyst particle may include a plurality of different catalytically active components. Each catalytically active component in the plurality of catalytically active components in the composite catalyst may provide different catalytic functions for the composite catalyst particles. Therefore, the multifunctional composite catalyst may combine a plurality of catalytic functions into a single particle. In particular, the composite catalyst of the present disclosure may include zeolite particles at least partially or completely embedded in a catalyst support material and catalytically active compounds deposited on the surface of the catalyst support material, the zeolite particles, or both. The composite catalyst may have a uniform distribution of catalytically active compounds on the outer surface and pore surface of the catalyst support material, the zeolite particles, or both. Therefore, the composite catalyst may have substantially uniform physical properties and may not encounter the disadvantages associated with the sedimentation of a physical catalyst mixture. The multifunctional composite catalyst may enable a single particle catalyst to be loaded into a reactor to carry out a variety of different chemical reactions, for example, such as a combination of isomerization, metathesis, and cracking for producing propylene from 2-butene.

[0010] According to an embodiment of the present disclosure, a method for preparing a composite catalyst may include: combining a catalyst support material, zeolite particles, a triblock copolymer surfactant, a catalytically active compound precursor, and a diluent to produce a catalyst precursor composition. The method may also include: mixing the catalyst precursor composition to produce a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in the diluent; and spray drying the catalyst precursor mixture. Spray drying may include: atomizing the catalyst precursor mixture to produce a plurality of droplets; and drying the plurality of droplets in a drying chamber. Drying may remove the diluent from each of the plurality of droplets to form an agglomerate comprising zeolite particles at least partially fixed within the catalyst support material. Drying may also react the catalytically active compound precursor to form a catalytically active compound deposited on the outer surface and pore surface of the catalyst support material, the zeolite particles, or both.

[0011] According to an embodiment of the present disclosure, a method for producing propylene may include: contacting a butene-containing feed with a composite catalyst at a reaction temperature. The contact may cause at least a portion of the butene to undergo a chemical reaction to produce a reaction effluent containing at least propylene. The composite catalyst may be prepared by a method that may include: combining a catalyst support material, zeolite particles, a triblock copolymer surfactant, a catalytically active compound precursor, and a diluent to produce a catalyst precursor composition. The method for preparing the composite catalyst may also include: mixing the catalyst precursor composition to produce a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in a diluent; and spray drying the catalyst precursor mixture. Spray drying may include: atomizing the catalyst precursor mixture to produce a plurality of droplets; and drying the plurality of droplets in a drying chamber. Drying may remove the diluent from each of the plurality of droplets to form an agglomerate containing zeolite particles at least partially fixed in the catalyst support material. Drying may also react the catalytically active compound precursor to form a catalytically active compound deposited on the outer surface and pore surface of the catalyst support material, the zeolite particles, or both. The method for producing propylene may further include separating at least a portion of the propylene from the reactor effluent.

[0012] Additional features and advantages of the described embodiments will be set forth in the detailed description which follows, and in part will be apparent to those skilled in the art from that detailed description or learned by practicing the described embodiments, including the detailed description, claims, and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0013] The following detailed description of certain embodiments of the present disclosure may be best understood when read in conjunction with the following drawings, in which like structures are indicated by like reference numerals, and in which:

[0014] Figure 1 schematically depicts a spray dryer system for preparing a composite catalyst according to one or more embodiments shown and described in the present disclosure;

[0015] Figure 2 schematically depicts a reactor system for performing a metathesis reaction according to one or more embodiments shown and described in the present disclosure;

[0016] Figure 3 graphically depicts an X-ray diffraction (XRD) curve of a mordenite framework inverted (MFI) structure zeolite according to one or more embodiments shown and described in the present disclosure;

[0017] Figure 4 graphically depicts an XRD curve of a prior art metathesis catalyst comprising tungsten oxide supported on a mesoporous silica support;

[0018] Figure 5 graphically depicts an XRD curve of a composite catalyst according to one or more embodiments shown and described in the present disclosure;

[0019] Figure 6 Diagrammatically depicts a schematic diagram of a device from a user according to one or more embodiments shown and described in the present disclosure. Figure 5 The total conversion rate and yield of ethylene, propylene, C5 hydrocarbons and C6+ hydrocarbons in the metathesis reaction carried out by the composite catalyst; and

[0020] Figure 7 Diagrammatically depicts the Figure 3 MFI structure zeolite and Figure 4 The total conversion rate and yield of ethylene, propylene, C5 hydrocarbons and C6+ hydrocarbons in the metathesis reaction performed by the dual catalyst system of the prior art metathesis catalyst.

[0021] For description Figure 1 and Figure 2 For the purpose of simplified schematic illustration and description, numerous valves, temperature sensors, electronic controllers, and similar processing components that may be employed in certain chemical processing operation fields and are well known to those of ordinary skill in the art are not included. In addition, accompanying components that are typically included in typical chemical processing operations, carrier gas supply systems, pumps, container agitators, compressors, furnaces, or other subsystems may not be depicted. It should be understood that these components and subsystems are within the spirit and scope of the disclosed embodiments of the present invention. However, operating components such as those described in the present disclosure may be added in the embodiments described in the present disclosure.

[0022] The arrows in the accompanying drawings refer to process streams. However, the arrows may equivalently refer to transmission lines that can be used to transmit process streams between two or more system components. In addition, arrows connected to system components can define inlets or outlets in each given system component. The direction of the arrows generally corresponds to the primary direction of movement of the material contained in the flow within the physical transmission line indicated by the arrows. In addition, arrows that do not connect two or more system components may represent product streams leaving the depicted system or system inlet streams entering the depicted system. The product streams may be further processed in accompanying systems or may be commercialized as final products.

[0023] In addition, arrows in the figures may schematically depict process steps that transport streams from one system component to another system component. For example, an arrow pointing from one system component to another system component may represent "transferring" a system component effluent to another system component, which may include: the contents of a process stream "leaving" or being "removed" from one system component and the contents of the product stream "introducing" another system component.

[0024] It should be understood that when two or more lines are Figure 1 and Figure 2 Two or more process streams are "mixed" or "combined" when they intersect in a schematic flow diagram of FIG. Mixing or combining can also include mixing by introducing the two streams directly into a system component such as a vessel, reactor, separator, or other system component. For example, it should be understood that when two streams are depicted as combining directly prior to entering a system component, the streams can equivalently be introduced into the system component and mixed within the system component.

[0025] Reference will now be made in more detail to various embodiments, some of which are illustrated in the accompanying drawings. Wherever possible, the same reference numerals will be used throughout the drawings to refer to the same or like parts. DETAILED DESCRIPTION

[0026] The present disclosure relates to a multifunctional composite catalyst and a method for preparing the composite catalyst. In particular, the composite catalyst may include: a catalyst support material; zeolite particles at least partially or completely embedded in the catalyst support material; and a catalytically active compound providing catalytically active sites at the outer surface and pore surface of the catalyst support material, the zeolite particles, or both. The composite catalyst may be prepared by a spray drying method, the spray drying method comprising: combining a catalyst support material, a zeolite particle, a triblock copolymer surfactant, at least one catalytically active compound precursor, and a diluent to produce a catalyst precursor composition. The method may also include: mixing the catalyst precursor composition to produce a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in a diluent. The method may also include: spray drying the catalyst precursor mixture, which may include atomizing the catalyst precursor mixture to produce a plurality of droplets and drying the droplets in a drying chamber. The drying may remove the diluent from the droplets to form an agglomerate containing zeolite particles at least partially fixed in the catalyst support material, and may react the catalytically active compound precursor to form a catalytically active compound deposited on the outer surface and pore surface of the catalyst support material, the zeolite particles, or both.

[0027] Composite catalyst can provide multifunctional catalyst with multiple different catalytic species, and every kind of catalytic species can be independent of other catalytic species in composite catalyst and catalyze different reactions.For example, composite catalyst can be used for converting 2-butene into propylene by metathesis, and can include zeolite particles and metal oxide (such as but not limited to tungsten oxide) as catalytically active compound.Metal oxide can have catalytic activity so that 1-butene and 2-butene cross metathesis to produce propylene, amylene and optional other C6+ olefins.Zeolite particles can catalyze amylene or other C6+ olefin cracking into propylene and other smaller olefins during metathesis reaction.

[0028] Composite catalysts can enable the reaction system to perform multiple catalytic reactions, such as metathesis and cracking, without the need to process and manage multiple catalyst materials. In addition, the use of composite catalysts can eliminate or reduce the need to install spacer materials in the reactor to separate catalyst beds with different catalysts. This can eliminate or reduce the dead zone from the reactor. The dead zone is a zone where no reaction occurs, such as due to the presence of inert spacer materials. In some conventional reaction systems, a blend or physical mixture of two separate dry particle catalysts can be prepared and loaded into the reactor. Although the dry blend of two particle catalysts can initially provide a multifunctional catalytic environment in the reactor system, one of the particle catalysts can eventually settle to the bottom of the reactor under gravity, which can form a separate zone in which the two blended catalysts are separated into the reactor. As the separate catalyst settles and forms a zone with two blended catalysts of different concentrations in the catalyst bed, this separation may cause undesirable changes in the efficiency of the reaction system. The composite catalyst described in the present disclosure can reduce or eliminate the problems associated with the blended catalysts precipitating over time in the reaction system.

[0029] As used in this disclosure, "catalyst" may refer to a solid particle comprising at least one catalytically active compound that increases the rate of a particular chemical reaction, increases the selective production of certain products in the reaction, or both.

[0030] As used throughout this disclosure, the term "mesoporous" may refer to a material having an average pore size from 2 nanometers (nm) to 50 nm.

[0031] As used in this disclosure, "catalytically active compounds" may refer to substances that increase the rate of a particular chemical reaction, increase the selective production of certain products in a reaction, or both. Catalytically active compounds and catalysts prepared using catalytically active compounds described in this disclosure may be used to promote a variety of reactions, such as, but not limited to, isomerization, metathesis, cracking, hydrogenation, demetallization, desulfurization, denitrogenation, other reactions, or combinations of these.

[0032] As used in this disclosure, "catalytic activity" may refer to the degree to which a catalyst or catalytically active compound increases the reaction rate of a reaction. A more catalytically active catalyst increases the reaction rate of a reaction compared to a less catalytically active catalyst.

[0033] As used in this disclosure, a "stable" mixture refers to a solid-liquid mixture in which the liquid portion contains dissolved solids that do not precipitate out of the liquid portion. For example, dissolved solids in the liquid portion of a stable mixture will not precipitate out during subsequent processing steps of the methods disclosed herein.

[0034] As used throughout this disclosure, the term "butene" or "butenes" may refer to a composition comprising one or more of 1-butene, trans-2-butene, cis-2-butene, isobutylene, or a mixture of these isomers. As used throughout this disclosure, the term "n-butene" may refer to a composition comprising one or more of 1-butene, trans-2-butene, cis-2-butene, or a mixture of these isomers and not comprising isobutylene. As used throughout this disclosure, the term "2-butene" may refer to trans-2-butene, cis-2-butene, or a mixture of these two isomers.

[0035] As previously mentioned, the composite catalyst can be a spray-dried catalyst, which comprises the zeolite particles that are at least partially or completely surrounded by or embedded in the following agglomerates: the agglomerates are formed by catalyst support materials and at least one catalytically active compound deposited on the surface of catalyst support materials, zeolite particles or both. The agglomerates of catalyst support materials and zeolite particles can be formed by the agglomeration of catalyst support materials during spray drying. The catalyst support material can be an oxide of a metal or metalloid, such as one or more oxides or these combinations in silicon, aluminum, titanium, cerium. The catalyst support material can be silicon dioxide, fumed silica, aluminum oxide, fumed aluminum oxide, titanium dioxide, fumed titanium dioxide, ceria, fumed ceria or these combinations.

[0036] In one or more embodiments, the catalyst support material can be silicon dioxide. The example of the silicon dioxide catalyst support material suitable for preparing the composite catalyst can include a mesoporous silica support. The mesoporous silica support can have an average pore size from 2.5 nanometers (nm) to 40nm and a total pore volume of at least 0.600 milliliters per gram (mL / g). In one or more embodiments, the silicon dioxide of the catalyst support material can have an average pore size from 2.5nm to 40nm, or from 2.5nm to 20nm, or from 2.5nm to 4.5nm, or from 2.5nm to 3.5nm, or from 8nm to 18nm, or from 12nm to 18nm. The silica support suitable for the catalyst support material can have a total pore volume of from 0.600 mL / g to 2.5 mL / g, or from 0.600 mL / g to 1.5 mL / g, or from 0.600 mL / g to 1.3 mL / g, or from 0.600 mL / g to 0.800 mL / g, or from 0.600 mL / g to 0.700 mL / g, or from 0.900 mL / g to 1.3 mL / g. The silica support suitable for the catalyst support material can have a total pore volume of from 250 square meters per gram (m 2 / g) to 600m 2 The silica carrier may have a surface area of ​​from 450 m 2 / g to 600m 2 / g, or from 250m 2 / g to 500m 2 / g, or from 275m 2 / g to 400m 2 / g, or from 275m 2 / g to 350m 2 / g of surface area.

[0037] In one or more embodiments, the silica support may be substantially free of foreign metals or elements that may adversely affect the catalytic activity of the system. As used in the present disclosure, the term "substantially free" of a certain component may refer to a composition (such as a catalyst support material, a zeolite, a catalyst, or a catalyst precursor mixture) having less than 1 weight percent (wt.%) of the component in the composition. For example, a silica support that is substantially free of foreign metals or elements may contain less than 1 wt.% of these foreign metals or elements. A suitable silica support may be Santa Barbara amorphous (SBA-15) mesoporous silica molecular sieve. Alternatively, another suitable example of a silica support may be Silica support (commercially available from Fuji Silysia Chemical Ltd, headquartered in Aichi, Japan). In one or more embodiments, the catalyst support material may be Q-10 grade silica carrier particles having an average pore size of 10 nm, a pore volume of 1 mL / g, a 2 / g surface area and an average particle size of from 75 micrometers (μm) to 150 μm. In one or more embodiments, the catalyst support material can be Q-10 grade silica particles having an average particle size from 75 μm to 500 μm.

[0038] Composite catalyst of the present disclosure and the method for preparing composite catalyst utilize prefabricated catalyst carrier particles (such as silica or other metal oxide particles) to replace other catalyst carrier sources for catalyst carrier materials. Therefore, the method for preparing composite catalyst of the present disclosure may not include the step of forming catalyst carrier materials (such as preparing silica by one or more silica precursors) by one or more precursors before spray drying, during spray drying process or during additional calcining step. Initially providing prefabricated catalyst carrier materials with the best properties of surface area, pore size and pore volume causes a uniform catalyst composition to be reliably formed. The use of silica precursor (such as tetraethyl orthosilicate) requires the additional step of forming SiO2 in a spray dryer, and uniform loading structure will not be produced. In addition, when using silica precursor, at least a portion of catalytically active compound precursor may be trapped in silica rather than being deposited on the silica surface, which may cause this part of catalytically active compound to be unable to be used, and may increase the amount of required expensive catalytically active compound precursor. Therefore, propylene selectivity and yield in metathesis reaction are affected.

[0039] The composite catalyst may include an amount of catalyst support material sufficient to form agglomerates that partially or completely surround and entrap zeolite particles within agglomerates of the catalyst support material. The composite catalyst may have from 20 wt.% to 90 wt.% of the catalyst support material, based on the total weight of the composite catalyst. The composite catalyst may contain from 20 wt.% to 85 wt.%, from 20 wt.% to 80 wt.%, from 20 wt.% to 75 wt.%, from 20 wt.% to 70 wt.%, from 20 wt.% to 60 wt.%, from 30 wt.% to 90 wt.%, from 30 wt.% to 85 wt.%, from 30 wt.% to 80 wt.%, from 30 wt.% to 100 wt.%, from 30 wt.% to 15 ...50 wt.%, from 30 wt.% to 150 wt.%, from 30 % to 75wt.%, from 30wt.% to 70wt.%, from 50wt.% to 90wt.%, from 50wt.% to 85wt.%, from 50wt.% to 80wt.%, from 50wt.% to 75wt.%, from 50wt.% to 70wt.%, from 60wt.% to 90wt.%, from 60wt.% to 85wt.% or from 60wt.% to 85wt.% of catalyst support material.

[0040] As described above, the composite catalyst may further include zeolite particles that are at least partially or completely surrounded by or embedded in the catalyst support material. The zeolite particles may include one or more than one zeolite composition. As used in the present disclosure, a zeolite composition refers to a zeolite having a specific zeolite framework structure and a specific material composition. Thus, zeolite compositions may differ from each other by framework structure, composition, or both. Zeolite compositions may be grouped into "zeolite types", such as MFI framework type zeolites (such as ZSM-5 zeolite), FAU framework type zeolites (such as Y zeolite), or *BEA framework type zeolites (such as β zeolite), each of which zeolite types is subsequently described in the present disclosure. Other zeolite types having other framework structures and compositions may also be used to produce the composite catalyst.

[0041] In one or more embodiments, the zeolite particles may comprise one or more MFI framework type zeolites, such as ZSM-5. As used in the present disclosure, "ZSM-5" refers to a zeolite having an MFI framework type according to the International Union of Pure and Applied Chemistry (IUPAC) zeolite nomenclature and consisting of silica and alumina. ZSM-5 refers to "Zeolite Socony Mobil-5" and is a pentasil family zeolite, which may be represented by the chemical formula Na n Al n Si 96 – n O 192 ·16H2O, where 0 < n < 27. Examples of commercially available zeolite ZSM-5 include, but are not limited to, CBV2314, CBV3024E, CBV5524G, and CBV28014 (available from Zeolyst International). The MFI framework type zeolites may comprise one or more phosphorus-containing compounds, such as phosphorus oxide, such as phosphorus pentoxide ("P2O5").

[0042] In one or more embodiments, the catalyst composition may comprise an FAU framework type zeolite, such as Y zeolite. As used in the present disclosure, "Y zeolite" refers to a zeolite having an FAU framework type according to the IUPAC zeolite nomenclature and consisting of silica and alumina, wherein the molar ratio of silica to alumina is at least 3. For example, the molar ratio of silica to alumina in Y zeolite may be at least 5, at least 12, or even at least 30, such as from 5 to 30, from 12 to 30, or from about 15 to about 30. The unit cell size of Y zeolite may be from about 24 angstroms to about 25 angstroms, such as 24.56 angstroms.

[0043] In one or more embodiments, the catalyst composition may include one or more *BEA framework type zeolites, such as beta zeolite. As used in the present disclosure, "beta zeolite" refers to a zeolite having a *BEA framework type according to the IUPAC zeolite nomenclature and consisting of silica and alumina. The molar ratio of silica to alumina in beta zeolite can be at least 10, at least 25, or even at least 100. For example, the molar ratio of silica to alumina in beta zeolite can be from 5 to 500, such as from 25 to 300. Examples of commercially available beta zeolite compositions may include, but are not limited to, CP814C, CP814E, and CP811C-300 (produced by Molecular Sieve Catalysts International). Beta zeolite may be in the form of H-β. H-β refers to an acidic form of beta zeolite derived from ammonium-β (NH4-β) typically via calcination. In one or more embodiments, beta zeolite can be stabilized by direct reaction with phosphoric acid (H3PO4) or by impregnation with diammonium hydrogen phosphate ((NH4)2HPO4). According to one or more embodiments, the *BEA framework-type zeolite may include one or more phosphorus-containing compounds, such as phosphorus oxide or phosphorus pentoxide ("P2O5").

[0044] The zeolite particles can have a weight ratio of silica to alumina from 10: 1 to 6000: 1. For example, the zeolite can have a weight ratio of silica to alumina from 10: 1 to 4000: 1, from 10: 1 to 2000: 1, from 10: 1 to 1000: 1, from 10: 1 to 500: 1, from 10: 1 to 300: 1, from 100: 1 to 6000: 1, from 100: 1 to 4000: 1, from 100: 1 to 2000: 1, from 100: 1 to 1000: 1, from 100: 1 to 500: 1, from 200: 1 to 6000: 1, from 2 1 to 4000: 1, from 200: 1 to 2000: 1, from 200: 1 to 1000: 1, from 200: 1 to 500: 1, from 500: 1 to 6000: 1, from 500: 1 to 4000: 1, from 500: 1 to 2000: 1, from 500: 1 to 1000: 1, from 1000: 1 to 6000: 1, from 1000: 1 to 4000: 1, or from 1000: 1 to 2000: 1. In one or more embodiments, the zeolite particles can be an MFI 2000 zeolite cracking catalyst having a silica to alumina weight ratio of 2000: 1.

[0045] The average particle size of the zeolite particles may be smaller than the average particle size of the composite catalyst. The zeolite particles may have an average particle size of less than or equal to 35 μm, less than or equal to 30 μm, less than or equal to 25 μm, or even less than or equal to 20 μm. The zeolite particles may have an average particle size greater than or equal to 5 μm, greater than or equal to 10 μm, or even greater than or equal to 15 μm. The zeolite particles may have an average particle size from 5 μm to 35 μm, from 5 μm to 30 μm, from 5 μm to 25 μm, from 5 μm to 20 μm, from 10 μm to 35 μm, from 10 μm to 30 μm, from 10 μm to 25 μm, from 10 μm to 20 μm, from 15 μm to 35 μm, from 15 μm to 30 μm, from 15 μm to 25 μm, from 15 μm to 20 μm, from 5 μm to 10 μm, or even from 5 μm to 20 μm.

[0046] The composite catalyst can include zeolite particles in an amount sufficient to carry out catalytic cracking reaction to produce propylene and other light olefins during butene metathesis. Based on the gross weight of the composite catalyst, the composite catalyst can include zeolite particles from 5wt.% to 50wt.%. Based on the gross weight of the composite catalyst, the composite catalyst can include zeolite particles from 5wt.% to 40wt.%, from 5wt.% to 30wt.%, from 10wt.% to 50wt.%, from 10wt.% to 40wt.%, from 10wt.% to 30wt.%, from 15wt.% to 50wt.%, from 15wt.% to 40wt.%, from 15wt.% to 30wt.%, or from 20wt.% to 30wt.% of zeolite particles.

[0047] In some embodiments, the composite catalyst particles of the present disclosure can be an agglomerate of a catalyst support material and a zeolite particle. For example, the catalyst support material and the zeolite particles can form an agglomerate, wherein the zeolite particles are at least partially or completely embedded in the catalyst support material. In addition, the catalytically active compound can be deposited on the surface of the entire composite catalyst particle, and catalytically active sites can be produced at the outer surface and pore surface of the catalyst support material, the zeolite particles, or both.

[0048] As previously mentioned, the composite catalyst can have at least one catalytically active compound supported by a catalyst support material, zeolite particles or both. The catalytically active compound is different from the zeolite particles and the catalyst support material. The catalytically active compound can include a compound having a catalytic activity that promotes metathesis reaction, isomerization reaction or both. The catalytically active compound can also play a role in removing pollutants and catalyst poisons from the reactant stream. The catalytically active compound can include a metathesis catalyst. In one or more embodiments, the catalytically active compound can include an isomerization catalyst.

[0049] The catalytically active compound can be a metal, a metal oxide, other catalytically active compounds or a combination of these. The catalytically active compound can be a metal, such as but not limited to platinum, gold, palladium, rhodium, iridium, chromium, other metals or a combination of these. The catalytically active compound can include a metal oxide, such as one or more than one oxide of a metal from the 6th to 10th group of the International Union of Pure and Applied Chemistry Periodic Table (IUPAC Periodic Table). The metal oxide can include at least one oxide of molybdenum, rhenium, tungsten, manganese, titanium, cerium or any combination of these. In some embodiments, the metal oxide can be tungsten oxide. The form, type and amount of the catalytically active compound deposited on the catalyst support surface can determine the catalytic activity of the composite catalyst.

[0050] The composite catalyst may comprise one or more catalytically active compounds supported by a catalyst support material, zeolite particles or both. For example, the composite catalyst may comprise 1, 2, 3, 4, 5, 6 or more catalytically active compounds. In theory, the number of different catalytically active compounds that can be incorporated into the composite catalyst may be unlimited. However, the number of different catalytically active compounds that can be included in the composite catalyst may be limited by the types of reactions that can be carried out simultaneously. The number of different catalytically active compounds may also be limited by the reactions that must be carried out in sequence. The number of different catalytically active compounds may also be limited by catalyst poisoning considerations.

[0051] The catalytically active compound can be arranged on the surface of the composite catalyst that is accessible to steam and gas, such as being deposited on the outer surface and the pore surface of the composite catalyst. The catalytically active compound can be deposited on the outer surface or the pore surface of the catalyst support material, the zeolite particles or both. The catalytically active compound can provide catalytically active sites at the surface (such as the outer surface, the pore surface or both) of the composite catalyst.

[0052] The amount of the catalytically active compound possessed by the composite catalyst may be sufficient to enable the composite catalyst to exhibit the function of the catalytically active compound. For example, the catalytically active compound may be tungsten oxide, and the composite catalyst may contain tungsten oxide in an amount sufficient to catalyze olefin metathesis reactions. Based on the gross weight of the composite catalyst, the composite catalyst may contain from 0.1wt.% to 25wt.% of the catalytically active compound. Based on the gross weight of the composite catalyst, the composite catalyst may have from 0.1wt.% to 20wt.%, from 0.1wt.% to 15wt.%, from 0.1wt.% to 10wt.%, from 0.1wt.% to 8wt.%, from 1wt.% to 25wt.%, from 1wt.% to 20wt.%, from 1wt.% to 15wt.%, from 1wt.% to 10wt.%, from 1wt.% to 8wt.%, from 4wt.% to 10wt.% .% to 25wt.%, from 4wt.% to 20wt.%, from 4wt.% to 15wt.%, from 4wt.% to 10wt.%, from 4wt.% to 8wt.%, from 8wt.% to 25wt.%, from 8wt.% to 20wt.%, from 8wt.% to 15wt.%, from 6wt.% to 8wt.%, from 6wt.% to 10wt.%, or from 6wt.% to 15wt.% of the catalytically active compound.

[0053] The composite catalyst of the present invention can be synthesized by spray drying. In the spray drying process, a catalyst precursor mixture can be prepared and then introduced into a spray dryer. The catalyst precursor mixture can be prepared in the following manner: zeolite particles, catalyst support materials, catalytically active compound precursors, surfactants and at least one diluent are mixed to form a catalyst precursor composition, and then the catalyst precursor composition is mixed to produce a catalyst precursor mixture. The zeolite particles can be any zeolite in the zeolites previously described in the present disclosure. For example, in one or more embodiments, the zeolite particles can be ZSM-5 zeolite particles. Based on the dry weight of the catalyst precursor mixture, the catalyst precursor mixture can include from 5 weight percent (wt.%) to 50wt.% of zeolite particles. As used throughout the present disclosure, the "dry weight" of the catalyst precursor mixture refers to the total weight of the catalyst precursor mixture minus the total weight of the diluent in the catalyst precursor mixture.

[0054] The catalyst support material can be any of the catalyst support materials previously described in the present disclosure. For example, in one or more embodiments, the catalyst support material can include one or more of silica, alumina, titania, ceria, or a combination of these. In one or more embodiments, the catalyst support material can be a silica support, such as a prefabricated silica support particle, which can have any of the features, characteristics, or properties previously described for the silica support. Based on the dry weight of the catalyst precursor mixture, the catalyst precursor mixture can contain from 20 wt.% to 90 wt.% of the catalyst support material. Again, dry weight refers to the weight of the catalyst precursor mixture 108 without diluent. For example, in some embodiments, based on the dry weight of the catalyst precursor mixture 108, the catalyst precursor mixture can include from 20 wt.% to 85 wt.%, from 20 wt.% to 80 wt.%, from 20 wt.% to 75 wt.%, from 20 wt.% to 70 wt.%, from 20 wt.% to 60 wt.%, from 30 wt.% to 90 wt.%, from 30 wt.% to 85 wt.%, from 30 wt.% to 80 wt.%, %, from 30wt.% to 75wt.%, from 30wt.% to 70wt.%, from 50wt.% to 90wt.%, from 50wt.% to 85wt.%, from 50wt.% to 80wt.%, from 50wt.% to 75wt.%, from 50wt.% to 70wt.%, from 60wt.% to 90wt.%, from 60wt.% to 85wt.%, or from 60wt.% to 80wt.% of catalyst support material.

[0055] The catalytically active compound precursor may be a metal such as platinum, gold, palladium, rhodium, iridium, chromium, other metals or combinations of these. Alternatively or additionally, the catalytically active compound precursor may comprise a metal salt that is soluble in a diluent. The catalytically active compound precursor may comprise a metal oxoate precursor. The metal oxoate precursor may be a metal oxide precursor of one or more oxides of a metal from Groups 6-10 of the IUPAC periodic table. The metal oxide may be at least one oxide of molybdenum, rhenium, tungsten, manganese, titanium, cerium or any combination of these. Alternatively, the metal oxoate precursor may be a tungstate precursor. Examples of tungstate precursors may include, but are not limited to, ammonium metatungstate ((NH4)6H2W 12 O 40), ammonium paratungstate, tungstic acid, phosphotungstic acid, sodium tungstate, other tungstate precursors or combinations of these. In one or more embodiments, the tungstate precursor may include ammonium metatungstate, ammonium metatungstate hexahydrate or ammonium paratungstate. In one or more embodiments, the metal oxoate precursor may be tungsten oxide (such as tungsten oxide (IV), tungsten oxide (VI)), other tungsten oxides or a combination of tungsten oxides. In one or more embodiments, the metal oxide is tungsten oxide (WO3). The catalyst precursor mixture may include a plurality of catalytically active compound precursors to produce a composite catalyst having a plurality of catalytically active compounds deposited on the outer surface and pore surface of the catalyst support material, the zeolite particles or both.

[0056] Based on the dry weight of the catalyst precursor mixture, the catalyst precursor mixture may contain from 0.1 wt.% to 25 wt.% of the catalytically active compound precursor. Based on the dry weight of the catalyst precursor mixture, the catalyst precursor mixture may contain from 0.1 wt.% to 20 wt.%, from 0.1 wt.% to 15 wt.%, from 0.1 wt.% to 10 wt.%, from 0.1 wt.% to 8 wt.%, from 1 wt.% to 25 wt.%, from 1 wt.% to 20 wt.%, from 1 wt.% to 15 wt.%, from 1 wt.% to 10 wt.%, from 1 wt.% to 8 wt.%, from 4 wt.% to 25wt.%, from 4wt.% to 20wt.%, from 4wt.% to 15wt.%, from 4wt.% to 10wt.%, from 4wt.% to 8wt.%, from 8wt.% to 25wt.%, from 8wt.% to 20wt.%, from 8wt.% to 15wt.%, from 6wt.% to 8wt.%, from 6wt.% to 10wt.%, or from 6wt.% to 15wt.% of a catalytically active compound precursor.

[0057] A polymeric surfactant may be included in the catalyst precursor mixture to enhance the dispersion of the catalytically active compound precursor in the catalyst precursor mixture, thereby improving the distribution of the catalytically active compound on the surface of the catalyst support material, the zeolite particles, or both. The surfactant may be a symmetrical triblock copolymer surfactant such as P123 surfactant (available from BASF Corporation, Florham Park, NJ, USA) is a poly(ethylene glycol)-block-poly(propylene glycol)-block-poly(ethylene glycol) copolymer (PEG-PPG-PEG copolymer). The triblock copolymer PEG-PPG-PEG is composed of poly(ethylene oxide) (PEO) and poly(propylene oxide) (PPO) comonomers and exhibits hydrophobicity at temperatures above 288 Kelvin and water solubility at temperatures below 288 Kelvin. This dual property results in the formation of micelles containing the PEG-PPG-PEG triblock copolymer. Dissolved The P123 surfactant forms micelles, which are used as a skeleton for preparing structured mesoporous silica (such as SBA-15). In contrast, the use of triblock copolymers for promoting the deposition of catalytically active compounds (such as tungsten oxide) on catalyst support materials is disclosed herein. In conventional synthesis, a surfactant is added to a metal precursor, and the mixture is then subjected to heat treatment. The metal precursor decomposes to generate a metal oxide. In the methods and compositions of the present disclosure, a surfactant can be used to enhance the mixing between a catalyst support material (such as a silica support) and a catalytically active compound precursor (such as a tungsten precursor) in a catalyst precursor mixture. The enhanced mixing provided by the surfactant can improve the distribution of catalytically active compounds (such as tungsten oxide) on the surface of a catalyst support material and zeolite particles after heat treatment. Surfactant properties (such as whether the surfactant is ionic, cationic or nonionic) play an important role in the effectiveness of polymeric surfactants. The use of triblock copolymers makes the large-scale preparation method of the composite catalyst disclosed herein easy and reliable.

[0058] The catalyst precursor mixture may have a surfactant in an amount sufficient to uniformly disperse the catalytically active compound precursor throughout the catalyst precursor mixture. Based on the dry weight of the catalyst precursor mixture, the catalyst precursor mixture may include from 1 wt.% to 20 wt.% of a surfactant. Based on the dry weight of the catalyst precursor mixture, the catalyst precursor mixture may include from 1 wt.% to 15 wt.%, from 1 wt.% to 18 wt.%, from 1 wt.% to 15 wt.%, from 5 wt.% to 20 wt.%, from 5 wt.% to 18 wt.%, from 5 wt.% to 15 wt.%, from 8 wt.% to 20 wt.%, from 8 wt.% to 18 wt.%, from 8 wt.% to 15 wt.%, from 10 wt.% to 20 wt.%, from 10 wt.% to 18 wt.%, or from 10 wt.% to 15 wt.% of a surfactant.

[0059] The diluent may be a combination of water, an organic solvent or water and at least one organic solvent. An exemplary organic solvent may include a combination of methanol, ethanol, acetone or a solvent. In one or more embodiments, the diluent may be water so that the catalyst precursor mixture is an aqueous catalyst precursor mixture. The diluent may also include water in combination with an alcohol (such as ethanol), which may improve the ability to dissolve the triblock copolymer surfactant in the diluent during the preparation of the catalyst precursor mixture. The catalyst precursor mixture may have a diluent in an amount sufficient to atomize the catalyst precursor mixture in the spray dryer. The catalyst precursor mixture may have a diluent in an amount sufficient to produce the desired average particle size of the composite catalyst particles prepared by spray drying. For example, due to the reduced concentration of catalyst support material, zeolite particles, catalytically active compound precursors and surfactants in each droplet, increasing the amount of the diluent may reduce the average particle size of the composite catalyst. Based on the gross weight of the catalyst precursor mixture, the catalyst precursor mixture may include a diluent from 50wt.% to 95wt.%. For example, the catalyst precursor mixture can contain from 50 wt.% to 90 wt.%, from 50 wt.% to 85 wt.%, from 50 wt.% to 80 wt.%, from 70 wt.% to 95 wt.%, from 70 wt.% to 90 wt.%, from 70 wt.% to 85 wt.%, from 80 wt.% to 95 wt.%, or from 80 wt.% to 90 wt.% of diluent, based on the total weight of the catalyst precursor mixture.

[0060] refer to Figure 1 ,exist Figure 1The catalyst precursor mixture represented by reference numeral 142 in the figure can be prepared in the following manner: a catalyst support material, zeolite particles, a catalytically active compound precursor, a triblock copolymer surfactant and a diluent are combined to form a catalyst precursor composition, and then the catalyst precursor composition is mixed to produce a catalyst precursor mixture. The catalyst precursor composition can be prepared by one or more mixing processes. The preparation of the catalyst precursor mixture 142 may include a first mixing process 102, which may include: combining zeolite particles 104, a catalyst support material 105 and a first portion 106 of a diluent to produce a first mixture 108. The first mixing process 102 may also include: mixing the first mixture 108 under conditions sufficient to disperse the solid zeolite particles and the solid catalyst support material in the diluent. The first mixing process 102 can be carried out in a container having a mixer or agitator. In one or more embodiments, the container can be a feed container for a spray dryer 150. The first mixture 108 can be mixed at a speed greater than or equal to 600 revolutions per minute (rpm), greater than or equal to 700 rpm, or even greater than or equal to 800 rpm, such as from 800 rpm to 1200 rpm. The first mixture 108 can be mixed for at least 30 minutes, such as from 30 minutes to 24 hours.

[0061] Preparation of the catalyst precursor mixture 142 may include a second mixing process 110, wherein a surfactant 112 (such as a triblock copolymer surfactant) may be combined with a second portion 114 of a diluent and mixed until the surfactant is completely dissolved in the diluent to produce a second mixture 118. When the surfactant is a triblock copolymer surfactant, the second portion 114 of the diluent may include an alcohol 116, such as, for example, ethanol, which may be added to the second portion 114 of the diluent. The ethanol 116 may help dissolve the surfactant 112 to form a homogenous second mixture 118. The second mixture 118 may be prepared in a container having a mixer or agitator and may be mixed under conditions sufficient to completely dissolve the surfactant 112 in the diluent. For example, the second mixture 118 may be mixed at a speed greater than or equal to 600 rpm, greater than or equal to 700 rpm, or greater than or equal to 800 rpm, such as from 600 rpm to 2000 rpm, or from 700 rpm to 1500 rpm. The second mixture 118 may be mixed for a period of at least 30 minutes, such as from 30 minutes to 24 hours.

[0062] Preparation of the catalyst precursor mixture 142 may also include a third mixing process 110, wherein at least one catalytically active compound precursor 122 may be combined with a third portion 124 of a diluent (such as water) and mixed until the catalytically active compound precursor 122 is completely dissolved in the third portion 124 of the diluent to produce a third mixture 128. The third mixture 128 may be prepared in a container having a mixer or agitator and may be mixed under conditions sufficient to completely dissolve the catalytically active compound precursor 122 in the diluent. For example, the third mixture 128 may be mixed at a speed greater than or equal to 600 rpm, greater than or equal to 700 rpm, or greater than or equal to 800 rpm, such as from 600 rpm to 2000 rpm, or from 700 rpm to 1500 rpm. The third mixture 128 may be mixed for a period of at least 30 minutes (such as from 30 minutes to 24 hours).

[0063] Still reference Figure 1 , the preparation of the catalyst precursor mixture 142 can include combining the second mixture 118 and the third mixture 128 to produce a fourth mixture 132, the fourth mixture comprising the surfactant 112 and the at least one catalytically active compound precursor 122 dissolved in the diluent. The fourth mixture 132 can be mixed under conditions sufficient to produce a homogenous mixture of the surfactant and the catalytically active compound precursor.

[0064] The fourth mixture 132 can be added to the first mixture 108, which contains zeolite particles and catalyst support materials dispersed in a diluent to produce a catalyst precursor composition. The fourth mixture 132 and the first mixture 108 can be combined in the feed container 140 of the spray dryer 150. The catalyst precursor composition can be mixed to produce a catalyst precursor mixture 142, wherein the catalyst support material and the zeolite particles are suspended in the diluent, and will not precipitate or settle out from the catalyst precursor mixture 142 during spray drying. The catalyst precursor composition can be mixed under conditions sufficient to reduce or prevent the catalyst support material, zeolite particles or both from precipitating or settling during spray drying. The catalyst precursor composition can be mixed with a rotation speed of up to 700rpm (such as from 500rpm to 700rpm). The catalyst precursor composition can be mixed for a sufficient period of time to produce a catalyst precursor mixture, which can be a colloidal mixture, wherein the catalyst support particles, zeolite particles or both do not precipitate or settle during spray drying. The catalyst precursor composition can be mixed for a period of time greater than or equal to 72 hours (such as from 72 hours to 120 hours, or from 72 hours to 96 hours) to produce a catalyst precursor mixture 142. After mixing, the catalyst precursor mixture 142 can be a colloidal solution, which can be a stable mixture. In other words, after mixing, the catalyst precursor mixture 142 can be a homogeneous colloidal mixture, which can have a reduced tendency of solids to escape from the solution and settle compared to the catalyst precursor composition before mixing. When the mixing time is less than 72 hours, the catalyst precursor mixture 142 may not form a stable colloidal solution, and may show sedimentation of the catalyst support material during spray drying, which may have an adverse effect on the composite catalyst produced by the method. This sedimentation may affect the efficiency of the spray drying process, which may reduce the product yield when the composite catalyst is used in the metathesis process.

[0065] Based on the dry weight of the catalyst precursor mixture 142, the catalyst precursor mixture can include from 20.0 wt.% to 85.0 wt.% of the catalyst support material 104, from 5.0 wt.% to 50.0 wt.% of the zeolite particles 105, from 1 wt.% to 20 wt.% of the surfactant, and from 0.1 wt.% to 25.0 wt.% of the catalytically active compound precursor. The catalyst precursor mixture 142 can have solids in an amount from 1 wt.% to 50 wt.%, from 1 wt.% to 30 wt.%, from 1 wt.% to 20 wt.%, from 5 wt.% to 50 wt.%, from 5 wt.% to 30 wt.%, from 5 wt.% to 20 wt.%, from 10 wt.% to 50 wt.%, from 10 wt.% to 30 wt.%, from 10 wt.% to 20 wt.%, from 15 wt.% to 50 wt.%, from 15 wt.% to 30 wt.%, from 15 wt.% to 20 wt.%, or from 20 wt.% to 50 wt.%, based on the total weight of the catalyst precursor mixture 142, wherein the solids include zeolite particles, catalyst support material, catalytically active compound precursors, and copolymer surfactants (all materials except diluents).

[0066] Reference again Figure 1, the catalyst precursor mixture 142 can be spray dried in a spray dryer 150 to produce a composite catalyst. The spray dryer 150 can be any commercially available spray dryer system. The spray dryer 150 can include a drying chamber 151, which includes a cylindrical portion 152 and a conical portion 154. The spray dryer 150 can also include a spray nozzle 156, which is disposed in the drying chamber 151 and is operable to atomize the catalyst precursor solution 142 in the drying chamber 151. A heated gas 144 can be introduced into the drying chamber 151. The gas can be air or an inert gas, such as but not limited to nitrogen, helium, argon or other inert gases. In addition, water 146 can be fluidly connected to the spray nozzle 156 for use during the startup of the spray dryer 150. Before the catalyst precursor mixture 142 is introduced into the spray nozzle 156, the catalyst precursor mixture 142 can be heated to a spray temperature. The spray temperature of the catalyst precursor mixture 142 may be greater than or equal to 50° C., greater than or equal to 75° C., or even greater than or equal to 100° C. The spray temperature of the catalyst precursor mixture may be from 50° C. to 150° C., from 50° C. to 125° C., from 75° C. to 150° C., from 75° C. to 125° C., from 100° C. to 150° C., or even from 100° C. to 125° C. If the spray temperature is too low, the evaporation of the diluent from the droplets of the catalyst precursor mixture 142 in the drying chamber 151 may not be sufficient at the surface temperature of the drying chamber 151. If the spray temperature is too high, the evaporation of the diluent may be too fast, resulting in a decrease in the cohesion within the composite catalyst, which may affect the durability of the composite catalyst.

[0067] During steady-state operation of the spray dryer 150, the catalyst precursor mixture 142 can be delivered to the spray nozzle 156 by the catalyst precursor pump 143. The spray nozzle 156 can atomize the catalyst precursor mixture 142 into a plurality of droplets of the catalyst precursor mixture 142. The type of the spray nozzle 156 may affect the average droplet size of the droplets of the catalyst precursor mixture 142 in the drying chamber 151, which may affect the average particle size of the composite catalyst recovered from the spray dryer 150. For example, a spray nozzle 156 configured to produce droplets of smaller size can produce a composite catalyst with a smaller average particle size. In addition, the pressure, flow rate, or both of the catalyst precursor mixture 142 delivered to the spray nozzle 156 may also affect the droplet size and average particle size of the composite catalyst.

[0068] refer to Figure 1, droplets of the catalyst precursor mixture 142 are atomized into the spray drying chamber 151, where the droplets are heated by the heated gas 144. The drying chamber 151 of the spray dryer 150 can be maintained at a surface temperature sufficient to evaporate the diluent 106 from the droplets of the catalyst precursor mixture 142 to form a plurality of solid composite catalyst particles. The surface temperature of the drying chamber 151 refers to the temperature measured at the inner surface of the drying chamber 151. The heated gas 144 can be heated to a temperature sufficient to maintain the surface temperature of the drying chamber 151. The drying chamber 151 may be maintained at a surface temperature of from 200° C. to 300° C., such as from 200° C. to 285° C., from 200° C. to 280° C., from 200° C. to 275° C., from 250° C. to 300° C., from 250° C. to 285° C., from 250° C. to 280° C., from 250° C. to 275° C., from 260° C. to 300° C., from 260° C. to 285° C., from 260° C. to 280° C., or from 260° C. to 275° C. If the surface temperature of the drying chamber is too low, the diluent in the droplets of the catalyst precursor mixture 142 may not be completely evaporated to produce solid composite catalyst particles.

[0069] In the drying chamber 151, the heat from the heated gas 144 can cause the diluent to be removed from the droplets of the catalyst precursor mixture 142, such as by evaporation of the diluent. As the diluent evaporates from the droplets of the catalyst precursor mixture 142, the volume of each droplet in the catalyst precursor mixture 142 can decrease, and the catalyst support material of the catalyst support precursor 142 can aggregate to form agglomerates, which can at least partially or completely surround and fix or capture the zeolite particles within the catalyst support material to form composite catalyst particles.

[0070] As the diluent is removed, the catalytically active compound precursor can be deposited on the surface of the catalyst support material, zeolite particles or both. The triblock copolymer surfactant in the catalyst precursor mixture can be operated to separate the catalytically active compound precursor and prevent the catalytically active compound precursor from solidifying into larger crystals or agglomerates during the drying process. This can make the catalytically active compound precursor more evenly distributed on the surface (external surface and pore surface) of the catalyst support material, zeolite particles or both. As the diluent is removed from the droplets of the catalyst precursor mixture 142 in the drying chamber 151, the catalytically active compound precursor deposited on the surface of the catalyst support material, zeolite particles or both can undergo a chemical reaction to be converted from the catalytically active compound precursor to a catalytically active compound. For example, a catalytically active compound precursor comprising a tungsten compound (such as ammonium metatungstate) can be oxidized at a temperature in the drying chamber 151 to convert the tungsten compound into tungsten oxide. Therefore, the composite catalyst recovered from the drying chamber 151 of the spray dryer 150 can include a catalytically active compound deposited on the outer surface and pore surface of the catalyst support material, zeolite particles or both.

[0071] Reference again Figure 1 , the spray dryer 150 may include one or more catalyst outlets in the drying chamber 151, each outlet fluidly connected to a solid separator and a blower 190, the blower being operable to draw air and the spray-dried composite catalyst out of the drying chamber 151. A first composite catalyst stream 160 may be removed from a first outlet at a converging end of a conical portion 154 of the drying chamber 151. The conversion end of the conical portion 154 may be disposed at the bottom end of the drying chamber 151 so that the first outlet is at the bottom of the drying chamber 151. The composite catalyst spray-dried in the drying chamber 151 may eventually descend to the conical portion 154 of the drying chamber 151. The first composite catalyst stream 160 may flow out of the drying chamber 151 and enter the first solid separator 170. The first solid separator 170 can be fluidly coupled to a blower 190, which can be operable to draw a first composite catalyst stream 160 containing a composite catalyst and heated air out of the drying chamber 151 from the first catalyst outlet, and transmit the first composite catalyst stream 160 to the first solid separator 170. The first solid separator 170 can be operable to separate the first composite catalyst 180 from the heated air in the first composite catalyst stream 160. The first solid separator 170 can be a cyclone separator, a filter or other solid-gas separation device. The first composite catalyst 180 can be recovered from the first solid separator 170. The heated gas can be sucked through the first solid separator by the blower 190 and removed from the process.

[0072] A second composite catalyst stream 162 may be removed from a second outlet of the drying chamber 151. The second outlet may be disposed upstream of the first outlet relative to the flow of composite catalyst passing downward through the drying chamber 151. The second outlet may be disposed in the cylindrical portion 152 of the drying chamber 151 or near the diverging end of the conical portion 154 of the drying chamber 151. As droplets of the catalyst precursor mixture 142 are converted into solid composite catalyst particles in the drying chamber 151, heavier solid composite catalyst particles may be transported along the drying chamber 151 relative to the flow of composite catalyst passing downward through the drying chamber 151. Figure 1 The -Z direction of the coordinate axis in the drying chamber 151 decreases more rapidly downward. As used throughout this disclosure, "heavier" composite catalyst particles may refer to composite catalyst particles having a greater density or a larger average particle size than "lighter" composite catalyst particles. Thus, during steady-state operation of the spray dryer 150, the gradient of particle density, average particle size, or both may be in the drying chamber 151 along the vertical direction ( Figure 1The + / -Z direction of the coordinate axis in the drying chamber 151 is formed. Removing the composite catalyst from different vertical positions of the drying chamber 151 can enable the recovery of composite catalysts with different average particle sizes, different densities, or both. Typically, removing the composite catalyst particles from a higher position (at a larger +Z position) in the drying chamber 151 can produce a composite catalyst stream that contains a composite catalyst with a smaller density, average particle size, or both than the first composite catalyst 180 recovered from the bottom of the drying chamber 151.

[0073] The second composite catalyst stream 162 can flow out of the drying chamber 151 and enter the second solid separator 172. The second solid separator 172 can be fluidly coupled to a blower 190, which can be operable to extract the second composite catalyst stream 162 containing composite catalyst and heated air from the second catalyst outlet to the drying chamber 151, and transmit the second composite catalyst stream 162 to the second solid separator 172. The second solid separator 172 can be operable to separate the second composite catalyst 182 from the heated gas in the second composite catalyst stream 162. The second solid separator 172 can be a cyclone separator, a filter or other solid-gas separation device. The second composite catalyst 182 can be recovered from the second solid separator 172. The heated gas can be sucked through the second solid separator 172 by the blower 190 and removed from the process. Compared with the first composite catalyst 180 recovered from the bottom of the drying chamber 151, the second composite catalyst 182 can have a smaller density, a smaller average particle size, or both. Although a first composite catalyst 180 and a second composite catalyst 182 are described, it should be understood that one or more composite catalyst streams may be removed from the drying chamber at different locations to produce a plurality of composite catalysts, each composite catalyst having a different average particle size, average density, or both.

[0074] After spray drying of the composite catalyst, the composite catalyst, such as the first composite catalyst, the second composite catalyst, or both, may be calcined in a calciner. The calcination process may be a two-step calcination process. This two-step calcination process may ensure decomposition of the triblock copolymer surfactant (such as P123 surfactant), and the formation of a stable and active catalytically active compound from a catalytically active compound precursor. For example, calcination can ensure that a stable and active tungsten oxide species is formed from a tungsten precursor (such as ammonium metatungstate). Calcination can be carried out in the presence of one or more of the following gases: air, oxygen, hydrogen and nitrogen. Calcination can be carried out at a calcination temperature of from 200°C to 700°C. Thermal treatment conditions, including the type of gas environment and the calcination temperature, may affect the tungsten oxide species formed. The type of tungsten oxide species formed affects the stability and metathesis activity of the catalyst composition, including propylene yield. The two-step calcination process described here can produce a stable tungsten oxide phase for self-metathesis and cross-metathesis. The first step of the calcination process is to convert ammonium metatungstate into tungsten oxide after thermal decomposition. In an embodiment, the first step is carried out at about 200°C to 250°C in the presence of air. The tungsten precursor has a significant weight loss. The degradation of the tungsten precursor and the conversion of the tungsten precursor to tungsten oxide continue until the second step, which is carried out at a calcination temperature of from 500°C to 600°C, at which time the weight loss of the tungsten precursor stabilizes and an active tungsten oxide species for metathesis is formed. In one or more embodiments, the composite catalyst can be first subjected to calcination at 250°C for 2 hours and then subjected to calcination at 550°C for 8 hours, wherein the heating rate before reaching the first temperature is 1°C per minute and the heating rate before reaching the second temperature is 3°C per minute. Although the calcination process has been described for a composite catalyst having tungsten oxide as a catalytically active compound, it should be understood that the calcination process can be used to complete the formation of a composite catalyst having other catalytically active compounds.

[0075] The evaluation of the physical properties of the spray-dried composite catalyst shows that the catalytically active material (such as tungsten oxide) is uniformly dispersed on the outer surface and the pore surface of the catalyst support material. Compared with the conventional metathesis catalyst prepared by conventional techniques (such as wet impregnation or incipient wet impregnation), this uniform dispersion of the catalytically active material can be converted into a higher conversion rate of the composite catalyst and higher propylene and ethylene yields.

[0076] Compared with the average particle size of the metathesis catalyst prepared by conventional techniques (such as wet impregnation or initial wet impregnation), the composite catalyst prepared by spray drying according to the present disclosure can have a reduced average particle size. The composite catalyst can have an average particle size less than or equal to 80 microns (μm), less than or equal to 50 μm, less than or equal to 30 μm, or even less than or equal to 20 μm. The composite catalyst of the present disclosure can have an average particle size from 1 μm to 80 μm, from 1 μm to 50 μm, from 1 μm to 30 μm, from 1 μm to 20 μm, from 5 μm to 80 μm, from 5 μm to 50 μm, from 5 μm to 30 μm, from 5 μm to 20 μm, from 8 μm to 80 μm, from 8 μm to 50 μm, from 8 μm to 30 μm, or from 8 μm to 20 μm. The average particle size can be determined by scanning electron microscopy (SEM) or other known analytical methods.

[0077] Composite catalysts comprising zeolite particles embedded in catalyst support materials and catalytically active compounds deposited on the outer surface and pore surface of catalyst support materials, zeolite particles or both can be used in metathesis reaction processes to convert butene into propylene, ethylene and other olefins. Metathesis reaction processes can include metathesis reactions combined with butene isomerization, cracking or both. As shown in reaction 1 (RXN 1), the isomerization of 2-butene to 1-butene and the isomerization of 1-butene to 2-butene are equilibrium reactions, as shown in the single-headed bidirectional arrows. The isomerization of 2-butene and 1-butene can be achieved with an isomerization catalyst. As used in the present disclosure, the term "isomerization catalyst" can refer to a catalyst that promotes the isomerization of olefins (including, for example, the isomerization of 2-butene to 1-butene). As shown in reaction 2 (RXN 2), the cross metathesis of 1-butene and 2-butene can produce 1-propylene and 2-pentene. As used in the present disclosure, the term "cross-metathesis" may refer to an organic reaction involving the redistribution of olefin fragments by the rupture and regeneration of carbon-carbon double bonds. In the case of the cross-metathesis between 2-butene and 1-butene, the redistribution of these carbon-carbon double bonds by metathesis produces propylene and C5-C6 olefins. The cross-metathesis of 1-butene and 2-butene can be achieved with a metathesis catalyst (such as tungsten oxide). As used in the present disclosure, the term "metathesis catalyst" may refer to a catalyst that promotes the metathesis reaction of olefins to form other olefins. A metathesis catalyst may also isomerize 2-butene to 1-butene by a "self-metathesis" reaction mechanism.

[0078]

[0079] With reference to RXN 1 and RXN 2, isomerization and metathesis reactions are not limited to these reactants and products; however, RXN 1 and RXN 2 provide a simplified description of the reaction method. As shown in RXN 2, metathesis reactions can occur between two olefins. The groups of carbon atoms bonded to the carbon-carbon double bond can be exchanged between molecules to produce two new olefins with exchanged groups. The specific metathesis catalyst selected can generally determine whether cis-isomers or trans-isomers are formed, because the formation of cis-isomers or trans-isomers can depend at least in part on the coordination of olefins with the catalyst. 1-Butene can also self-metathesis to produce ethylene and 3 hexenes by a similar reaction mechanism in the presence of a metathesis catalyst.

[0080] Further, as shown in the following reaction 3 (RXN 3) provided later in this disclosure, "cracking" can refer to the catalytic conversion of C4+ olefins into propylene and other alkanes, alkenes, or alkanes and alkenes, e.g., C2-C3 olefins. The cracking reaction is not limited to the reactants and products shown in RXN3; however, RXN 3 provides a simplified illustration of the cracking reaction.

[0081]

[0082] By contacting the butene-containing feedstock with the composite catalyst of the present disclosure under reaction conditions sufficient to carry out metathesis reaction, butene can be converted into propylene and other olefins by metathesis and cracking. In one or more embodiments, the composite catalyst can include ZSM-5 zeolite particles embedded in the catalyst support material containing mesoporous silica. The composite catalyst can also include tungsten oxide dispersed on the outer surface and pore surface of the mesoporous silica catalyst support, ZSM-5 zeolite particles or both as a catalytically active compound. The metathesis process can optionally include additional isomerization catalysts to maintain the equilibrium concentration of 1-butene and 2-butene in the reactor. The isomerization catalyst can be a separate particle catalyst arranged upstream of the composite catalyst or mixed with the composite catalyst.

[0083] Reference now Figure 2 , schematically depicts a reactor system 200 for performing butene metathesis. The reactor system 200 may include a metathesis reactor 210 and a metathesis effluent separation system 230 downstream of the metathesis reactor 210. The metathesis reactor 210 may be a fixed bed reactor or any other type of reactor suitable for performing a metathesis reaction. The metathesis reactor 210 may include a plurality of metathesis reactors connected in series or in parallel. The metathesis reactor 210 may be operable to contact a butene-containing feed 202 with a composite catalyst of the present disclosure in a metathesis reaction zone 212. The metathesis reactor 210 may include an inert packing material 216 upstream and downstream of the metathesis reaction zone 212 to fix the composite catalyst in the metathesis reaction zone 212.

[0084] The butene-containing feed 202 may contain 1-butene, trans-2-butene, cis-2-butene, or a combination thereof. The butene-containing feed 202 may further contain other C1-C6 components. Based on the total weight of the butene-containing feed 202, the butene-containing feed 202 may contain from 10 wt.% to 100 wt.% of 1-butene. For example, based on the total weight of the butene-containing feed 202, the butene-containing feed 202 may contain from 10 wt.% to 80 wt.%, from 10 wt.% to 60 wt.%, from 10 wt.% to 40 wt.%, from 10 wt.% to 20 wt.%, from 20 wt.% to 100 wt.%, from 20 wt.% to 80 wt.%, from 20 wt.% to 60 wt.%, from 20 wt.% to 40 wt.%, from 40 wt.% to 100 wt.%, from 40 wt.% to 80 wt.%, from 40 wt.% to 60 wt.%, from 60 wt.% to 100 wt.%, from 60 wt.% to 80 wt.%, or from 80 wt.% to 100 wt.% of 1-butene. The butene-containing feed 202 may contain from 10 wt.% to 100 wt.% 2-butene (ie, cis-2-butene, trans-2-butene, or both), based on the total weight of the butene-containing feed 202. For example, feedstock 140 may contain from 10 wt.% to 80 wt.%, from 10 wt.% to 60 wt.%, from 10 wt.% to 40 wt.%, from 10 wt.% to 20 wt.%, from 20 wt.% to 100 wt.%, from 20 wt.% to 80 wt.%, from 20 wt.% to 60 wt.%, from 20 wt.% to 40 wt.%, from 40 wt.% to 100 wt.%, from 40 wt.% to 80 wt.%, from 40 wt.% to 60 wt.%, from 60 wt.% to 100 wt.%, from 60 wt.% to 80 wt.%, or from 80 wt.% to 100 wt.% of 2-butene, based on the total weight of butene-containing feedstock 202. In addition, butene-containing feedstock 202 may be substantially free of ethylene. For example, the butene-containing feed 202 , which may be substantially free of ethylene, may contain less than 1 wt. % ethylene, based on the total weight of the butene-containing feed 202 .

[0085] In one or more embodiments, the butene-containing feed 202 can be a C4 raffinate stream, such as, but not limited to, a raffinate-2 stream. The raffinate is a residual C4 stream after one or more components are removed from a naphtha cracking process or a gas cracking process (the C4 stream typically contains n-butane, 1-butene, 2-butene, isobutylene, and 1,3-butadiene as its major components and optionally some isobutane that together with the major components forms up to 95% or more of the C4 stream). The butene-containing feed 202 can include a raffinate-1 stream. Raffinate-1 is a C4 residue obtained after separating 1,3-butadiene from a C4 raffinate stream, and primarily contains 2-butene, 1-butene, and isobutylene, which can account for from 55 wt.% to 99 wt.% of the raffinate-1 stream. For example, based on the total weight of the raffinate-1 stream, the raffinate-1 stream may contain from 10 wt.% to 30 wt.% of 2-butene, from 25 wt.% to 50 wt.% of 1-butene, and from 20 wt.% to 50 wt.% of isobutylene. The butene-containing feed 202 may contain a raffinate-2 stream. Raffinate-2 is a C4 residue obtained after separating 1,3-butadiene and isobutylene from a C4 raffinate stream, and mainly contains 2-butene, 1-butene, and normal butane, which may account for from 45 wt.% to 99 wt.% of the raffinate-2 stream. For example, based on the total weight of the raffinate-2 stream, the raffinate-2 stream may contain from 20 wt.% to 60 wt.% of 2-butene, from 10 wt.% to 60 wt.% of 1-butene, and from 15 wt.% to 25 wt.% of normal butane. The butene-containing feed 202 may include a raffinate-3 stream. Raffinate-3 is a C4 residue obtained after separating 1,3-butadiene, isobutylene, and 1-butene from a C4 raffinate stream, and mainly includes 2-butene, normal butane, and unseparated residual 1-butene, which may account for from 40 wt.% to 99 wt.% of the raffinate-3 stream in combination. For example, based on the total weight of the raffinate-3 stream, the raffinate-3 stream may include from 30 wt.% to 70 wt.% of 2-butene and from 10 wt.% to 30 wt.% of normal butane. The presence of isobutylene, inert gas, and non-olefins (such as normal butane) in the butene-containing feed 202 may not have a negative impact on the target metathesis reaction, but may undergo a cracking reaction by contacting with the zeolite particles in the composite catalyst.

[0086] like Figure 1As shown, a butene-containing feed 202 can be introduced into a metathesis reactor 210 and contacted with a composite catalyst in a metathesis reaction zone 212, the composite catalyst can include: ZSM-5 zeolite particles embedded in a mesoporous silica catalyst support material; and tungsten oxide, which is dispersed as a catalytically active compound on the outer surface and pore surface of the mesoporous silica catalyst support, the ZSM-5 zeolite particles, or both. The contact of the butene-containing feed 202 with the composite catalyst can cause at least a portion of the butenes in the butene-containing feed 202 to react to form propylene and other olefins. The reaction can include cross-metathesis, cracking, or both.

[0087] Metathesis reaction zone 212 can be maintained at a metathesis reaction temperature sufficient to promote the cross metathesis reaction of 2-butene and 1-butene. The metathesis reaction temperature can be from 100 degrees Celsius (° C.) to 600° C. For example, metathesis reaction zone 212 can be maintained at from 100° C. to 550° C., from 100° C. to 450° C., from 100° C. to 400° C., from 100° C. to 300° C., from 100° C. to 250° C., from 100° C. to 150° C., from 150° C. to 600° C., from 150° C. to 550° C., from 150° C. to 450° C., from 150° C. to 400° C., from 150° C. to 300° C., from 150° C. to 250° C., from 250° C. to 600° C., from 150° C. to 550° C., from 150° C. to 450° C., from 150° C. to 400° C., from 150° C. to 300° C., from 150° C. to 250° C., from 250° C. to 600° C., from The metathesis reaction temperature is from 250°C to 550°C, from 250°C to 450°C, from 250°C to 400°C, from 250°C to 300°C, from 300°C to 600°C, from 300°C to 550°C, from 300°C to 450°C, from 300°C to 400°C, from 400°C to 600°C, from 400°C to 550°C, from 400°C to 450°C, from 450°C to 600°C, from 450°C to 550°C, or from 550°C to 600°C.

[0088] Compared with conventional metathesis catalysts prepared by conventional techniques (such as wet impregnation or initial wet impregnation), and compared with the dual catalyst system comprising a combination of a metathesis catalyst and a cracking catalyst, the composite catalyst prepared by the spray drying method of the present disclosure can show enhanced metathesis performance. The catalytic activity of the spray-dried composite catalyst of the present disclosure was evaluated in a fixed bed reactor for the conversion of butene to propylene, and its performance was compared with a dual catalyst reaction system, wherein the dual catalyst reaction system comprises a conventional metathesis catalyst prepared by wet impregnation and a separate zeolite cracking catalyst. The spray-dried composite catalyst has a high degree of activity and stability, and its performance can be comparable to a dual catalyst system with a conventional metathesis catalyst and a separate cracking catalyst. Therefore, the composite catalyst of the present disclosure can provide a metathesis performance comparable to a single catalyst, and it does not need to prepare a catalyst mixture or isolate and separate two or more reaction zones in a metathesis reactor (which may result in unused dead zones in the reactor).

[0089] Metathesis effluent 214 comprising propylene and other olefins can flow out from metathesis reactor 210.Metathesis effluent 214 can flow to metathesis effluent separation system 230, which is operable to separate metathesis effluent 214 into multiple product streams, such as but not limited to ethylene stream 232, propylene stream 234, C4 stream 236, C5+ stream 238 or a combination of these.Ethylene stream 232, propylene stream 234 or both can be passed to downstream processing units to purify ethylene, propylene or both.Ethylene, propylene or both can be used as valuable intermediates in the production of polymers and other valuable chemical products.C4 stream 236 can be recycled back to metathesis reactor 210 or be passed to one or more downstream processing operations.C5+ stream 238 can be passed to one or more downstream processing operations for further processing.

[0090] Examples

[0091] The following examples illustrate one or more additional features of the disclosure previously described. It should be understood that these examples are not intended to limit the scope of the disclosure or the appended claims in any way.

[0092] Example 1: Preparation of zeolite - MFI 2000 cracking catalyst

[0093] In a typical synthesis, 17.04 g of tetrapropylammonium bromide (TPABr) and 2.96 g of ammonium fluoride were dissolved in 300 g of deionized water and stirred thoroughly for 20 minutes to produce a TPABr solution. 48 g of fumed silica and 0.30 g of aluminum nitrate were gradually added to the TPABr solution simultaneously while stirring vigorously. Once the solution gelled, the gel was mixed with a spatula for about 10 minutes until homogenized. The obtained gel was placed on a plate lined with The gel was placed in an acid digestion bomb and kept at 200°C for 2 days. After two days, the digestion bomb was removed from the oven and quenched in cold water for 30 minutes. The contents of the digestion bomb were filtered and washed with 1 liter of deionized water. The molar composition of the gel was 1SiO2:0.0005Al2O3:0.08(TPA)Br:0.10NH4F:20H2O. The solid product obtained was washed with water and dried at 80°C overnight. The template was removed by calcination at 750°C in air at a heating rate of 4°C per minute for 6 hours.

[0094] The MFI-2000 cracking catalyst of Example 1 was analyzed using X-ray diffraction (XRD). Figure 3 , the XRD chart of the MFI-2000 cracking catalyst of Example 1 shows characteristic peaks of the MFI-2000 cracking catalyst at 2θ equal to 8 degrees (°), 9°, 23°, and 24°.

[0095] Comparative Example 2: Tungsten Oxide on Silica Metathesis Catalyst Prepared by Wet Impregnation

[0096] In Comparative Example 2, a comparative metathesis catalyst comprising tungsten oxide supported on a mesoporous silica support was prepared. The metathesis catalyst of Comparative Example 2 was prepared by a wet impregnation technique. About 2 grams of silica support material and about 0.235 g of ammonium metatungstate (based on 99.99% trace metals) were added to a round bottom flask. The silica support material was obtained from Fuji Silicon Chemical Co., Ltd. Q-10 grade mesoporous silica and calcined at 200°C for 3 hours and then at 575°C for five hours, with a heating rate of 3°C per minute. About 20 mL of deionized water was then added to the flask. A magnetic stirring bar was added to the flask, and the flask was placed on a stirring plate programmed to run at 500 rpm for approximately two hours. The magnetic stirring bar was removed from the flask, and the flask was connected to a rotary evaporator. The operating conditions of the rotary evaporator were: the speed was set to 171 rpm, the water bath temperature was set to 80°C, the vacuum was set to 292 mbar, and the coolant (50% water and 50% ethylene glycol) was maintained at 6°C. Thereafter, the catalytic composition was placed in a drying oven at 80°C overnight. The dried catalyst was calcined at 250°C for 2 hours and at 550°C for 8 hours, with a heating rate of 1°C per minute before reaching the first temperature and a heating rate of 3°C per minute before reaching the second temperature. The calcination of these samples was carried out at The tungsten oxide was heated to 400 rpm in a 3-550 furnace (commercially available from Dentsply Ceramco, headquartered in York, Pennsylvania, USA). The comparative metathesis catalyst of Comparative Example 2 included a tungsten oxide loading of 10 weight percent based on the total weight of the comparative metathesis catalyst.

[0097] The metathesis catalyst of Comparative Example 2 was analyzed using X-ray diffraction (XRD). The XRD data for the examples of the present disclosure were collected using a D4 Endeavor X-ray diffractometer from Bruker AXS GmbH (Karlsruhe, Germany) and analyzed using DIFFRAC.EVAV4.1.1 version (available from Bruker) with a built-in PDF library that matches perfect scans. The analysis was performed at room temperature over a 2-theta range of 20 to 80 degrees. Figure 4 As shown, the XRD chart of the metathesis catalyst of Comparative Example 2 includes a characteristic peak of silicon dioxide and a characteristic peak of tungsten oxide, which are within the 2-θ range between 20° and 30°.

[0098] Additionally, the metathesis catalyst of Comparative Example 2 was subjected to scanning electron microscopy (SEM) to determine the average particle size. The metathesis catalyst of Comparative Example 2 prepared by wet impregnation without spray drying had an average particle size of 81.012 micrometers (μm).

[0099] Example 3: Preparation of composite catalyst

[0100] In Example 3, a composite catalyst was prepared according to the method of the present invention using the MFI-2000 cracking catalyst of Example 1. A first solution was prepared by combining 33.55 grams of silica, 13 grams of the MFI-2000 cracking catalyst from Example 1, and 250 milliliters (mL) of water. The silica was CATiRAC from Fuji Silicon Chemical Co., Ltd. TM Q-10 grade silica. A mixture of silica and MFI-2000 cracking catalyst in water was stirred at a speed of greater than 800 revolutions per minute (rpm) for 30 minutes. A second solution containing 7 grams of surfactant, 35 mL of water and 70 mL of ethanol was prepared and stirred at a speed of greater than 800 rpm for 30 minutes to completely dissolve the surfactant. The surfactant was obtained from Sigma Aldrich P123 poly (ethylene glycol) -block - poly (propylene glycol) -block - poly (ethylene glycol) surfactant. The third solution was prepared by mixing 4 grams of tungsten precursor (ammonium metatungstate hexahydrate) with 40mL water, and the third solution was shaken vigorously until all tungsten precursors were dissolved. The third solution was then combined with the second solution, and the resulting mixture was stirred for 10 minutes. The combined mixture of the second solution and the third solution was then added to the first solution comprising silica and MFI-2000 cracking catalyst to prepare a spray dryer solution. The spray dryer solution was stirred for three days at a speed greater than 700rpm. The resulting spray dryer solution was milky and homogeneous in appearance.

[0101] Then use the GEANiro spray dryer MOBILE MINOR TM The spray dryer solution was spray dried for aqueous feed. The drying chamber of the spray dryer had a main body size of 793 millimeters (mm), a height of 660 mm, and a cone angle of 60 degrees. Spray drying was performed with a target feed flow rate of 240 milliliters per minute (mL / min), but the flow rate was constantly adjusted to maintain the exhaust temperature below 110°C. The surface temperature of the drying chamber was maintained at 275°C, and the fan speed of the fan that extracted air and composite catalyst from the drying chamber was set to 2009 rpm.

[0102] To start the spray drying process, the spray dryer is turned on and gradually heated while adding deionized water. Once the surface temperature of the drying chamber reaches the target temperature of 275°C and the temperature of the outlet air is stable, the spray dryer solution is introduced into the spray dryer to replace the deionized water. The composite catalyst is removed from the spray dryer at two locations: the bottom of the tapered portion of the drying chamber, and the position on the side of the drying chamber just above the tapered portion of the drying chamber. The composite catalyst removed from the bottom of the drying chamber is referred to as composite catalyst 3A, and the composite catalyst removed from the side of the drying chamber is referred to as composite catalyst 3B. Composite catalyst 3B contains catalyst particles that are lighter in density and slightly smaller in average particle size than composite catalyst 3A.

[0103] Composite Catalyst 3A and Composite Catalyst 3B were calcined according to the calcination process previously described in Example 1. Composite Catalyst 3A of Example 3 was analyzed using X-ray diffraction (XRD). Figure 5 The XRD graph of the composite catalyst 3A of Example 3 includes characteristic peaks of the MFI-2000 cracking catalyst of Example 1 at 2θ equal to 8 degrees (°), 9°, 23° and 24° and a characteristic peak of tungsten oxide at 2θ equal to about 23.3°.

[0104] In addition, composite catalyst 3A, composite catalyst 3B and a mixture of composite catalyst 3A and 3B in a weight ratio of 50:50 were subjected to scanning electron microscopy (SEM) to determine the average particle size. The values ​​of the average particle size of the composite catalyst of Example 3 and the metathesis catalyst of Comparative Example 2 are provided in Table 1. As shown in Table 1, the average particle size of the composite catalyst produced by the spray drying process in Example 3 is significantly smaller than the average particle size of conventional metathesis catalysts (such as those prepared in Comparative Example 2) prepared by wet impregnation.

[0105] Table 1

[0106]

[0107] Example 4: Butene metathesis using the composite catalyst of Example 2

[0108] In Example 4, the metathesis of a butene-containing feed was performed using the composite catalyst 3B of Example 3. The metathesis reaction was performed in a fixed bed reactor at atmospheric pressure. The fixed bed reactor is a 16-fold high throughput reactor unit. A fixed amount of 0.2 gram of composite catalyst 3B was loaded into the reactor between two layers of silicon carbide. Silicon carbide was used as an inert filler material to keep the catalyst in the reactor and not participate in the metathesis reaction.

[0109] The composite catalyst 3B of Example 2 is first pre-treated and activated for 24 hours at a temperature of 550 ℃ under nitrogen with a flow rate of 120 milliliters per minute (mL / min). The temperature of the fixed-bed reactor is adjusted to 500 ℃ at atmospheric pressure, and the butene-containing feed is introduced into the fixed-bed reactor. Based on the gross weight of the butene-containing feed, the butene-containing feed comprises 10wt.% of isobutane, 20wt.% of normal butane, 12.5wt.% of trans-2-butene, 12.5wt.% of cis-2-butene and 45wt.% of 1-butene. The butene-containing feed is heated at 7.175 (h / min) per hour. -1 ) was passed through the fixed bed reactor for 30 hours at a weight hourly space velocity (WHSV). The reactor effluent was quantitatively analyzed using a gas chromatograph (commercially available as Agilent GC-7890B) with a thermal conductivity detector (TCD) and two flame ionization detectors (FID).

[0110] refer to Figure 6 , provides the total conversion of butenes and the yield of each of ethylene, propylene, five-carbon hydrocarbons (C5), and hydrocarbons with 6 or more carbons (C6+) in percentage form. Figure 6 The conversions and yields are averages of 11 samples taken periodically over a 30-hour experimental run time. Composite catalyst 3B of Example 3 yielded an overall conversion of 53.7%, a propylene yield of 19.3%, and an ethylene yield of 5.9%.

[0111] Comparative Example 5: Butene Metathesis Using a Dual Catalyst System

[0112] In Comparative Example 5, a butene-containing feed was contacted with a dual catalyst system comprising the metathesis catalyst of Comparative Example 2 and the MFI-2000 cracking catalyst of Example 1. The metathesis catalyst of Comparative Example 2 (0.1 g) and the MFI-2000 catalyst of Example 1 (0.1 g) were charged into a fixed bed reactor, wherein the metathesis catalyst was disposed upstream of the MFI-2000 cracking catalyst. The metathesis catalyst of Comparative Example 2 was placed upstream of the MFI-2000 cracking catalyst of Example 1.

[0113] The catalyst of the dual catalyst system of Comparative Example 5 was pretreated and activated according to the process described in Example 4. After pretreatment, the reactor temperature was adjusted to 500° C. at atmospheric pressure, and the butene-containing feed was introduced into the fixed bed reactor. The butene-containing feed was heated at 7.175 (h 2 ) / h. -1 ) was passed through the fixed bed reactor for 30 hours at a weight hourly space velocity (WHSV). The reactor effluent was quantitatively analyzed using a gas chromatograph (commercially available as Agilent GC-7890B) with a thermal conductivity detector (TCD) and two flame ionization detectors (FID).

[0114] refer to Figure 7 , provides the total conversion of butenes and the yield of each of ethylene, propylene, five-carbon hydrocarbons (C5), and hydrocarbons with 6 or more carbons (C6+) in percentage form. Figure 7 The conversions and yields are averages of 11 samples taken periodically over a 30-hour experimental run time. The dual catalyst system of Comparative Example 5 yielded an overall conversion of 53.2%, a propylene yield of 20%, and an ethylene yield of 5.9%.

[0115] like Figure 6 and Figure 7 As shown, Example 3 ( Figure 6 ) of the composite catalyst produced results comparable to those of Example 5 with the metathesis catalyst of Comparative Example 2 and Example 1 ( Figure 7 ) of zeolite is suitable.In fact, the composite catalyst of Example 3 shows higher butene total conversion, which shows a generally higher catalytic activity compared with the metathesis catalyst of Comparative Example 2.It is not intended to be bound by any particular theory, it is believed that compared with the metathesis catalyst of Comparative Example 2 prepared by wet impregnation, the method for preparing the composite catalyst of Example 3 according to the present disclosure reduces the average particle size, and increases the surface area of ​​the composite catalyst and the dispersion of catalytically active compounds on the composite catalyst surface.It is believed that compared with the metathesis catalyst prepared by conventional wet impregnation or initial wet impregnation synthesis method, this smaller average particle size, larger surface area and catalytically active compounds on the surface of the larger dispersion cause the composite catalyst prepared by the method of the present disclosure to have a higher catalytic activity.

[0116] Example 6: Metathesis of Butene - Effect of Average Particle Size of Composite Catalyst of Example 3 on Overall Conversion and Yield ring

[0117] In Example 6, the effect of the average particle size of the composite catalyst of Example 3 on the metathesis of butene was studied by performing metathesis reactions according to the method in Example 4 using composite catalyst 3A, composite catalyst 3B, and a composite catalyst mixture comprising both 3A and 3B. As previously mentioned, the average particle size of composite catalyst 3A is greater than the average particle size of composite catalyst 3B. For each of the composite catalyst and the composite catalyst mixture, butene metathesis reactions were performed at temperatures of 450°C, 500°C, and 550°C according to the method described in Example 4. The composite catalyst mixture comprises composite catalyst 3A and composite catalyst 3B in equal weights. The average yields of propylene, ethylene, C5 hydrocarbons, and C6+ hydrocarbons obtained from each butene metathesis reaction of Example 6 are provided in Table 2 below.

[0118] Table 2

[0119]

[0120] As shown in the results in Table 2, composite catalyst 3B having a smaller average particle size produces better selectivity for propylene at higher metathesis temperatures than composite catalyst 3A having a larger average particle size. Composite catalyst 3A provides better metathesis performance in terms of propylene selectivity at lower temperatures.

[0121] Calculation method

[0122] The determination of "conversion rate" was calculated according to Equation 1.

[0123] Conversion = 100 - (cis-butene yield + trans-butene yield) (1) Similarly, the determination of "Conversion - C4" was calculated according to Formula 2.

[0124] Conversion rate - C4 = 100 - (cis-butene yield + trans-butene yield + iso-butene yield + 1-butene yield) (2) The determination of "selectivity" was calculated according to formula 3.

[0125]

[0126] The first aspect of the present disclosure relates to a method for preparing a composite catalyst. The method may include: combining a catalyst support material, zeolite particles, a triblock copolymer surfactant, a catalytically active compound precursor, and a diluent to produce a catalyst precursor composition. The method may also include: mixing the catalyst precursor composition to produce a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in a diluent; and spray drying the catalyst precursor mixture. Spray drying may include: atomizing the catalyst precursor mixture to produce a plurality of droplets; and drying the plurality of droplets in a drying chamber. Drying may remove the diluent from each of the plurality of droplets to form an agglomerate comprising zeolite particles at least partially fixed within the catalyst support material. Drying may also react the catalytically active compound precursor to form a catalytically active compound deposited on the outer surface and pore surface of the catalyst support material, the zeolite particles, or both.

[0127] A second aspect of the present disclosure may include the first aspect, wherein the catalyst support material may comprise solid particles comprising at least one of silica, fumed silica, alumina, fumed alumina, titania, fumed titania, or a combination thereof.

[0128] A third aspect of the present disclosure may include any of the first or second aspects, wherein the catalyst support material may comprise mesoporous silica.

[0129] A fourth aspect of the present disclosure may include any one of the first to third aspects, wherein the catalyst support material may include a prefabricated catalyst support material.

[0130] A fifth aspect of the present disclosure may include any one of the first to fourth aspects, wherein the method may not include synthesizing the catalyst support material from one or more precursors.

[0131] A sixth aspect of the present disclosure may include any one of the first to fifth aspects, wherein the catalyst support material may have an average pore size from 2.5 nanometers to 40 nanometers.

[0132] A seventh aspect of the present disclosure may include any one of the first to sixth aspects, wherein the catalyst support material may have a total pore volume of at least 0.600 milliliters per gram.

[0133] An eighth aspect of the present disclosure may include any one of the first to seventh aspects, wherein the catalyst support material may have a surface area of ​​from 250 square meters per gram to 600 square meters per gram.

[0134] A ninth aspect of the present disclosure may include any one of the first to eighth aspects, wherein the zeolite particles may include a mordenite framework inversion structure zeolite.

[0135] A tenth aspect of the present disclosure may include any one of the first to ninth aspects, wherein the zeolite particles may include ZSM-5 zeolite.

[0136] An eleventh aspect of the present disclosure may include any one of the first to tenth aspects, wherein the zeolite particles may include silica and alumina, and a weight ratio of silica to alumina is from 10:1 to 6000:1.

[0137] A twelfth aspect of the present disclosure may include any one of the first to eleventh aspects, wherein the zeolite particles may have an average particle size of from 5 microns to 35 microns.

[0138] A thirteenth aspect of the present disclosure may include any one of the first to twelfth aspects, wherein the triblock copolymer surfactant may be poly(ethylene glycol)-block-poly(propylene glycol)-block-poly(ethylene glycol).

[0139] A fourteenth aspect of the present disclosure may include any of the first to thirteenth aspects, including mixing the catalyst precursor mixture for a sufficient period of time to produce a stable catalyst precursor mixture.

[0140] A fifteenth aspect of the present disclosure may include any of the first to fourteenth aspects, including mixing the catalyst precursor composition for a period of greater than or equal to 72 hours.

[0141] The sixteenth aspect of the present disclosure may include any one of the first to fifteenth aspects, wherein the combination may include preparing a first mixture, a second mixture, and a third mixture. The first mixture may include a catalyst support material, zeolite particles, and a first portion of a diluent. The second mixture may include a triblock copolymer surfactant and a second portion of a diluent. The third mixture may include a catalytically active compound precursor and a third portion of a diluent.

[0142] A seventeenth aspect of the present disclosure may include the sixteenth aspect, wherein the combining may further include combining the second mixture and the third mixture to produce a fourth mixture, and combining the first mixture and the fourth mixture to produce a catalyst precursor composition.

[0143] An eighteenth aspect of the present disclosure may include any one of the first to seventeenth aspects, wherein the catalyst precursor mixture may further include an alcohol.

[0144] A nineteenth aspect of the present disclosure may include any one of the first to eighteenth aspects, wherein the drying chamber is maintained at a temperature of from 200°C to 300°C.

[0145] The twentieth aspect of the present disclosure may include the nineteenth aspect, further comprising: removing the first composite catalyst from the drying chamber at a first outlet disposed at the bottom of the drying chamber, and removing the second composite catalyst from the drying chamber at a second outlet upstream of the first outlet.

[0146] A twenty-first aspect of the present disclosure may include the twentieth aspect, wherein an average particle size of the second composite catalyst may be smaller than an average particle size of the first composite catalyst.

[0147] A twenty-second aspect of the present disclosure may include any one of the twentieth or twenty-first aspects, wherein a density of the second composite catalyst may be less than a density of the first composite catalyst.

[0148] A twenty-third aspect of the present disclosure may include any one of the first to twenty-second aspects, further comprising calcining the composite catalyst at a temperature of from 200°C to 700°C.

[0149] A twenty-fourth aspect of the present disclosure may include any one of the first to twenty-third aspects, wherein the catalytically active compound precursor may comprise a metal selected from molybdenum, rhenium, tungsten, manganese, titanium, cerium, or any combination of these.

[0150] A twenty-fifth aspect of the present disclosure may include any one of the first to twenty-fourth aspects, wherein the catalytically active compound precursor may include tungsten.

[0151] A twenty-sixth aspect of the present disclosure may include any one of the first to twenty-fifth aspects, wherein the catalytically active compound precursor may include ammonium metatungstate hydrate.

[0152] A twenty-seventh aspect of the present disclosure may include any one of the first to twenty-fourth aspects, wherein the catalytically active compound may comprise an oxide of a metal selected from molybdenum, rhenium, tungsten, manganese, titanium, cerium, or any combination of these.

[0153] A twenty-eighth aspect of the present disclosure may include any one of the first to twenty-seventh aspects, wherein the catalytically active compound may include tungsten oxide.

[0154] A twenty-ninth aspect of the present disclosure may include any one of the first to twenty-eighth aspects, wherein the catalyst precursor mixture may include from 5 weight percent to 50 weight percent of zeolite particles based on the dry weight of the catalyst precursor mixture.

[0155] A thirtieth aspect of the present disclosure may include any one of the first to twenty-ninth aspects, wherein the catalyst precursor mixture may include from 20 weight percent to 90 weight percent of the support material based on the dry weight of the catalyst precursor mixture.

[0156] A thirty-first aspect of the present disclosure may include any one of the first to thirtieth aspects, wherein the catalyst precursor mixture may include from 0.1 weight percent to 25 weight percent of the catalytically active compound precursor based on the dry weight of the catalyst precursor mixture.

[0157] A thirty-third aspect of the present disclosure may include any one of the first to thirty-second aspects, wherein the catalyst precursor mixture may include from 1 weight percent to 20 weight percent of the triblock copolymer surfactant based on the dry weight of the catalyst precursor mixture.

[0158] A thirty-fourth aspect of the present disclosure may include any one of the first to thirty-third aspects, wherein the catalyst precursor mixture may include from 50 weight percent to 95 weight percent of the diluent based on the total weight of the catalyst precursor mixture.

[0159] A thirty-fifth aspect of the present disclosure may include any one of the first to thirty-fourth aspects, wherein the catalyst precursor mixture may contain from 1 weight percent to 50 weight percent of solids.

[0160] A thirty-sixth aspect of the present disclosure may include any one of the first to thirty-fifth aspects and may relate to a catalyst prepared by the method of any one of the first to thirty-fifth aspects.

[0161] A thirty-seventh aspect of the present disclosure may include any one of the first to thirty-sixth aspects, wherein the composite catalyst may have an average particle size of from 1 micrometer to 80 micrometers.

[0162] A thirty-eighth aspect of the present disclosure may include any one of the first to thirty-seventh aspects, wherein the composite catalyst may include from 5 weight percent to 50 weight percent of the zeolite particles based on the total weight of the composite catalyst.

[0163] A thirty-ninth aspect of the present disclosure may include any one of the first to thirty-eighth aspects, wherein the composite catalyst may contain from 20 weight percent to 90 weight percent of the catalyst support material based on the total weight of the composite catalyst.

[0164] A fortieth aspect of the present disclosure may include any one of the first to thirty-ninth aspects, wherein the composite catalyst may contain from 0.1 weight percent to 25 weight percent of the catalytically active compound based on the total weight of the composite catalyst.

[0165] The forty-first aspect of the present disclosure may include any of the first to fortieth aspects and may relate to a method for producing propylene. The method may include contacting a butene-containing feed with a composite catalyst at a reaction temperature, wherein the composite catalyst may be prepared by any of the methods of the first to fortieth aspects. The contact may cause at least a portion of the butenes to undergo a chemical reaction to produce a reaction effluent comprising at least propylene. The method may also include separating at least a portion of the propylene from the reactor effluent.

[0166] The forty-second aspect of the present invention may relate to a method for producing propylene. The method may include contacting a butene-containing feed with a composite catalyst at a reaction temperature. The contact may cause at least a portion of the butene to undergo a chemical reaction to produce a reaction effluent containing at least propylene. The composite catalyst may be prepared by a method that may include: combining a catalyst support material, zeolite particles, a triblock copolymer surfactant, a catalytically active compound precursor, and a diluent to produce a catalyst precursor composition. The method for preparing the composite catalyst may also include: mixing the catalyst precursor composition to prepare a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in a diluent; and spray drying the catalyst precursor mixture. Spray drying may include: atomizing the catalyst precursor mixture to produce a plurality of droplets; and drying the plurality of droplets in a drying chamber. Drying may cause the diluent to be removed from each of the plurality of droplets to form an agglomerate containing zeolite particles at least partially fixed in the catalyst support material. Drying may also cause the catalytically active compound precursor to react to form a catalytically active compound deposited on the outer surface and pore surface of the catalyst support material, the zeolite particles, or both. The method for producing propylene may further include separating at least a portion of the propylene from the reactor effluent.

[0167] A forty-third aspect of the present disclosure may include any one of aspects forty-first to forty-second, wherein the butene-containing feed may comprise 1-butene, trans-2-butene, cis-2-butene, or a combination of these.

[0168] A forty-fourth aspect of the present disclosure may include any of aspects forty-one to forty-three, wherein the butene-containing feed may be substantially free of ethylene, such as comprising less than 1 weight percent ethylene.

[0169] A forty-fifth aspect of the present disclosure may include any one of aspects forty-one to forty-four, wherein the butene-containing feed may comprise a raffinate-2 stream, a raffinate-3 stream, or a combination of these.

[0170] A forty-sixth aspect of the present invention may include any one of the forty-first to forty-fifth aspects, wherein the reaction temperature may be from 400°C to 600°C.

[0171] A forty-seventh aspect of the present disclosure may include any one of aspects forty-first to forty-sixth, further comprising: contacting a butene-containing feed with an isomerization catalyst to produce an isomerization effluent, and contacting the isomerization effluent with a composite catalyst to produce a reaction effluent containing propylene.

[0172] A forty-eighth aspect of the present disclosure may include any of aspects forty-one to forty-seven, including separating the reaction effluent into a plurality of product streams.

[0173] A forty-ninth aspect of the present disclosure may include the forty-eighth aspect, wherein the product stream may comprise at least one of an ethylene stream, a propylene stream, a C4 stream, a C5+ stream, or a combination of these.

[0174] It should be noted that one or more of the following claims utilize the term "wherein" as a transitional term. For the purposes of defining the present technology, it should be noted that the term is introduced in the claims as an open transitional phrase that is used to introduce a recitation of a series of features of a structure and should be interpreted in the same manner as the more commonly used open introductory term "comprising."

[0175] It should be understood that any two quantitative values ​​assigned to a certain characteristic can constitute the scope of the characteristic, and all combinations of the scope formed by all the quantitative values ​​of a given characteristic are contained in the present disclosure.It should be understood that the composition range of the chemical composition in a stream or reactor should be understood as a mixture of the isomers comprising the composition in some embodiments, for example, the composition range of specified butenes can include the isomers of various butenes.It should be understood that these examples provide the composition range of various streams, and the total amount of the isomers of a specific chemical composition can constitute a scope.

[0176] The subject matter of the present disclosure has been described in detail and with reference to specific embodiments, it should be noted that the various details described in the present disclosure should not be considered to imply that these details relate to elements that are essential components of the various embodiments described in the present disclosure, even where specific elements are shown in each of the drawings accompanying the description of the present disclosure. Indeed, the appended claims should be considered to be the only indication of the breadth of the present disclosure and the corresponding scope of the various embodiments described in the present disclosure. In addition, it is apparent that modifications and changes can be made without departing from the scope of the appended claims.

Claims

1. A method for preparing a composite catalyst, the method comprising: combining a catalyst support material, zeolite particles, a triblock copolymer surfactant, a catalytically active compound precursor, and a diluent to produce a catalyst precursor composition; mixing the catalyst precursor composition to produce a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in the diluent; spray drying the catalyst precursor mixture, wherein the spray drying comprises: atomizing the catalyst precursor mixture to produce a plurality of droplets; and drying the plurality of droplets in a drying chamber, wherein drying removes the diluent from each of the plurality of droplets to form agglomerates comprising the zeolite particles at least partially immobilized within the catalyst support material, and reacts the catalytically active compound precursor to form a catalytically active compound deposited on the exterior and pore surfaces of the catalyst support material, the zeolite particles, or both, removing a first composite catalyst from the drying chamber at a first outlet disposed at a bottom of the drying chamber; and A second composite catalyst is removed from the drying chamber at a second outlet upstream of the first outlet, wherein the average particle size or density of the second composite catalyst is smaller than the average particle size or density of the first composite catalyst, respectively.

2. The method according to claim 1, wherein the catalyst support material comprises solid particles, and the solid particles comprise at least one of silicon dioxide, fumed silicon dioxide, aluminum oxide, fumed aluminum oxide, titanium dioxide, fumed titanium dioxide, or a combination of these.

3. The method according to claim 1, wherein the zeolite particles comprise a mordenite framework inversion zeolite, more preferably a ZSM-5 zeolite.

4. The method of claim 1, wherein the zeolite particles have an average particle size of 5 microns to 35 microns.

5. The method of claim 1, wherein the triblock copolymer surfactant is poly(ethylene glycol)-block-poly(propylene glycol)-block-poly(ethylene glycol).

6. The method according to any one of claims 1 to 5, wherein the combination comprises: A first mixture, a second mixture, and a third mixture are prepared, wherein: The first mixture comprises: The catalyst support material; said zeolite particles; and a first portion of said diluent; The second mixture comprises: The triblock copolymer surfactant; and a second portion of said diluent; The third mixture comprises: said catalytically active compound precursor; and a third portion of said diluent; combining the second mixture and the third mixture to produce a fourth mixture, and The first mixture and the fourth mixture are combined to produce the catalyst precursor composition.

7. The method according to any one of claims 1 to 5, wherein the drying chamber is maintained at a temperature of 200 to 300°C.

8. The method according to any one of claims 1 to 5, wherein the catalytically active compound precursor comprises: a metal selected from molybdenum, rhenium, tungsten, manganese, titanium, cerium, oxides of these metals, or any combination of these.

9. The process according to any one of claims 1 to 5, wherein the catalyst precursor mixture comprises 5 wt.% to 50 wt.% of zeolite particles based on the dry weight of the catalyst precursor mixture.

10. The method of claim 1, wherein the catalyst precursor mixture comprises from 20 wt.% to 90 wt.% of catalyst support material based on the dry weight of the catalyst precursor mixture.

11. The method according to any one of claims 1 to 5, wherein the average particle size of the second composite catalyst is smaller than the average particle size of the first composite catalyst.

12. A method for producing propylene, the method comprising: contacting a butene-containing feed with a first composite catalyst or a second composite catalyst at a reaction temperature, wherein contacting causes at least a portion of the butenes to undergo a chemical reaction to produce a reaction effluent comprising at least propylene, wherein the composite catalyst is prepared by a process comprising: combining a catalyst support material, zeolite particles, a triblock copolymer surfactant, a catalytically active compound precursor, and a diluent to produce a catalyst precursor composition; mixing the catalyst precursor composition to produce a catalyst precursor mixture, wherein the catalyst support material and the zeolite particles are suspended in the diluent; spray drying the catalyst precursor mixture, wherein the spray drying comprises: atomizing the catalyst precursor mixture to produce a plurality of droplets; and drying the plurality of droplets in a drying chamber, wherein drying removes the diluent from each of the plurality of droplets to form an agglomerate comprising the zeolite particles at least partially immobilized within the catalyst support material, and reacts the catalytically active compound precursor to form a catalytically active compound deposited on the exterior and pore surfaces of the catalyst support material, the zeolite particles, or both; removing a first composite catalyst from the drying chamber at a first outlet disposed at a bottom of the drying chamber; removing a second composite catalyst from the drying chamber at a second outlet upstream of the first outlet, wherein the second composite catalyst has an average particle size or density that is smaller than the average particle size or density of the first composite catalyst, respectively, and At least a portion of the propylene is separated from the reactor effluent.

13. The process of claim 12, wherein the butene-containing feed comprises 1-butene, trans-2-butene, cis-2-butene, or a combination of these.

14. The method according to any one of claims 12 or 13, wherein the reaction temperature is 400°C to 600°C.

15. The method according to any one of claims 12 or 13, wherein the average particle size of the second composite catalyst is smaller than the average particle size of the first composite catalyst.