Titanium-silicon catalyst with porous structure as well as preparation method and application of titanium-silicon catalyst
Through the preparation method of porous structure titanium silicon catalyst, the problem of insufficient activity in the olefin epoxidation reaction is solved, and efficient peroxide conversion and epoxidation product selectivity is achieved, the process is simplified and the process is reduced. It is cost-effective and suitable for industrial applications.
Patent Information
- Application Number
- CN202411054276.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
The existing titanium silicon catalysts are relatively low in olefin epoxidation reaction, especially for macromolecular olefins and ethylbenzene hydrogen peroxide or isopropylbenzene hydrogen peroxide as oxidizing agents, and the preparation process is complex and costly. Limits its industrial applications.
The titanium silicon catalyst preparation method is adopted to form a spray-dried spherical structure intermediate through hydrolysis reactions of surfactant, template agent, polymer latex spheres and silicon source, and a porous nanostructure is formed during the calcination process. Simplify the process and reduce costs.
The activity of the catalyst and the selectivity of the target product are improved, and the peroxide conversion rate is higher than 99.9% and the selectivity of the epoxidation product is higher than 97.0%, which is suitable for large-scale industrial production.
Smart Images

Figure CN118976536A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of propylene epoxidation catalyst and preparation thereof, and in particular relates to a porous titanium silicon catalyst and a preparation method and application thereof. Background Art
[0002] Epoxy compounds are a common intermediate raw material for synthesizing epoxy resins, surfactants, coatings, adhesives, surface coating agents and other chemicals widely used in life and industry, and are in great demand. The traditional production process for synthesizing epoxy compounds is generally the chlorohydrin method, but this method has the disadvantages of heavy pollution, large equipment corrosion, many by-products and high cost.
[0003] Therefore, many companies at home and abroad are committed to developing green production technologies for olefin epoxidation that are simple, clean and economical. One of the development directions is to use H2O2, tert-butyl hydroperoxide (TBHP), ethylbenzene hydroperoxide (EBHP) or isopropylbenzene hydroperoxide (CHP) as oxidants to react with olefins to prepare epoxides. The core of the development of green production processes for olefin epoxidation is to develop a catalyst with high activity and epoxidation selectivity, good stability, applicable to different olefin reactant systems, and easy preparation methods. In the 1980s, research on heterogeneous olefin epoxidation catalysts began at home and abroad. Among them, titanium silicalite has good catalytic activity for the selective oxidation of olefins and is a representative catalyst. Titanium-containing heteroatom molecular sieves developed in the early 1980s, such as TS-1 and TS-2, are representative. Such catalysts generally have only micropores (e.g., about 0.55 nm) and small pores. Since the oxidant and olefin can only undergo catalytic reaction in the Ti active center to produce epoxy compounds after diffusing in the pores of the titanium silicon molecular sieve, TS-1 and TS-2 molecular sieves are only suitable for reactions of small molecule olefins and H2O2 as oxidants. For reactions of large molecule olefins with a higher carbon number and ethylbenzene hydroperoxide and isopropylbenzene hydroperoxide as oxidants, it is difficult to diffuse in conventional titanium silicon molecular sieves with only micropores and then undergo catalytic reactions due to the large molecular dynamics diameter.
[0004] Therefore, the development of titanium silicon catalysts with large pore structures has become one of the hot spots in the industry. For example, patent applications CN1250775A and CN1248579A disclose a process for producing propylene oxide by epoxidation of propylene using ethylbenzene hydroperoxide as an oxidant and Ti-MCM-41 molecular sieve as a catalyst; US patent application US5783167A discloses a method for synthesizing titanium-containing mesoporous material Ti-MCM-41 by hydrothermal method, and patent application US6323147B1 discloses a process for preparing propylene oxide using isopropylbenzene hydroperoxide as an oxidant and Ti-MCM-41 molecular sieve as a catalyst; patent CN1500004A discloses a synthesis method of a titanium-containing catalyst Ti-MCM-41 with a mesoporous structure developed by Sumitomo Corporation of Japan; patent application CN106582809A discloses a synthesis method of a modified titanium silicon molecular sieve, the pore size of the molecular sieve is more than 10nm. The above methods all adopt the hydrothermal method to synthesize the catalyst. By using a template agent with a specific molecular weight and structure, a titanium silicon catalyst with a larger pore size (>2.0nm) is prepared under high temperature hydrothermal conditions. The synthesis process of this type of mesoporous molecular sieve is complicated, and a large amount of template agent is required during the synthesis process, resulting in a high cost for catalyst preparation, which limits its application in industry.
[0005] In addition, patent applications US3829392A, US3923843A, and US4021454A disclose a method of using macroporous SiO2 as a carrier, loading a titanium source onto the carrier surface by vapor deposition or liquid impregnation, and obtaining a titanium silicon catalyst by drying, calcining, and silanization. Since the titanium source used is easily hydrolyzed during the loading process to form acidic free TiO2, and it is difficult to increase the loading amount of titanium when preparing the catalyst by the impregnation method, the catalyst activity is low and the conversion rate of olefins is not high during the catalytic olefin epoxidation process.
[0006] The current methods for preparing titanium silicon composite oxide catalysts are mainly vapor deposition and sol-gel methods. Both vapor deposition and sol-gel methods have the following disadvantages: the preparation process is cumbersome, the operation is complicated, the conditions are harsh and difficult to control, and the reaction time is long. In addition, once the conditions are improperly controlled, the resulting catalyst is prone to generate more extra-framework titanium compounds (mainly free titanium dioxide), the catalyst surface acidity is strong, and the effective utilization rate of organic peroxides is low when used for propylene epoxidation reaction.
[0007] In summary, the conventional microporous titanium silicate molecular sieves have low activity in olefin epoxidation reactions due to their small pore size, which limits their application in olefin epoxidation reactions; mesoporous molecular sieve materials such as Ti-MCM-41 and Ti-SBA-15 can be used for epoxidation reactions of large molecular olefins and with EBHP or CHP as oxidants, but these catalysts are difficult to synthesize, the templates used are difficult to prepare and are expensive, resulting in high costs and limiting their industrial applications; titanium silicate catalysts prepared by vapor deposition or liquid impregnation using SiO2 as a carrier have low catalyst selectivity and reaction activity due to the presence of acidic free TiO2 on the surface and a low loading of titanium active centers.
[0008] Based on the defects in the above-mentioned prior art, it is necessary to provide a new catalyst for olefin epoxidation reaction, avoid the use of expensive non-scale plate agents, reduce the production cost of the catalyst, and solve the problem of low activity of conventional catalysts when used for epoxidation of large molecular olefins and epoxidation reactions using EBHP or CHP as oxidants. Summary of the invention
[0009] The object of the present invention is to provide a porous titanium silicon catalyst and a preparation method and application thereof. The preparation method is simple in process and easy for large-scale industrial production. The titanium silicon catalyst is used for olefin epoxidation reaction and has the advantages of high peroxide conversion rate and high selectivity for epoxidation target product.
[0010] In order to achieve the purpose of the invention, the present invention adopts the following technical solutions:
[0011] In a first aspect, the present invention provides a method for preparing a porous titanium silicon catalyst, the preparation method comprising the following steps:
[0012] (1) stirring and mixing a surfactant, a template, polymer latex balls and deionized water to uniformly mix, and then adding a silicon source to fully hydrolyze to obtain gel A;
[0013] (2) After uniformly mixing the titanium source and the organic solvent, slowly dripping them into the gel A, stirring them uniformly and removing the organic solvent to obtain the titanium silica gel B, and transferring the titanium silica gel B to a hydrothermal reactor for crystallization reaction to obtain a crystallization mother liquor;
[0014] (3) The crystallization mother liquid in step (2) is spray-dried and calcined in sequence to obtain the porous titanium silicon catalyst.
[0015] In the present invention, the silicon source in step (1) is one of tetraethyl orthosilicate, tetramethyl orthosilicate, tetrapropyl orthosilicate, tetrabutyl orthosilicate, or a mixture of two or more thereof, or at least one of silica sol and white carbon black. Typical but non-limiting examples of the combination include: a combination of tetraethyl orthosilicate and tetrapropyl orthosilicate, a combination of tetrapropyl orthosilicate and tetrabutyl orthosilicate, etc.
[0016] The template agent in step (1) of the present invention includes one or a mixture of two or more of tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrapropylammonium chloride, and tetrapropylammonium fluoride. Typical but non-limiting examples of the combination include: a combination of tetrapropylammonium hydroxide and tetrapropylammonium bromide, a combination of tetrapropylammonium chloride and tetrapropylammonium fluoride, etc.
[0017] The polymer in the polymer latex ball in step (1) of the present invention is any one of PMMA (polymethyl methacrylate), ABS (acrylonitrile-butadiene-styrene copolymer), PAA (polystyrene), PEEK (polyetheretherketone) or PET (polyethylene terephthalate), or a combination of at least two thereof;
[0018] Preferably, in the present invention, the polymer is in a monodisperse latex sphere state;
[0019] Preferably, the particle size of the polymer latex spheres is 150 to 500 nm, for example, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm or 500 nm, but is not limited to the listed values, and other values not listed within the numerical range are also applicable; the present invention selects polymers of a specific particle size so that they can be stably dispersed in the solution after mixing in step (1).
[0020] In the present invention, the surfactant in step (1) is a nonionic surfactant, which can make the polymer latex spheres disperse stably without agglomeration; preferably, it includes any one of coconut glucoside, lauryl glucoside, cetearyl glucoside, glyceryl monostearate or polysorbate, or a combination of at least two of them. Typical but non-limiting examples of the combination include: a combination of coconut glucoside and lauryl glucoside, a combination of lauryl glucoside and cetearyl glucoside, or a combination of glyceryl monostearate and polysorbate, etc.
[0021] In the present invention, the temperature of the hydrolysis reaction of adding the silicon source in step (1) is 40-60°C, and the reaction time is 4-8h. In a specific embodiment, the hydrolysis reaction is carried out by slowly adding the silicon source under stirring. In the present invention, the titanium source in step (2) is one or more of titanium tetrachloride, titanium tetrabromide, tetrapropyl titanate, tetrabutyl titanate, isopropyl titanate or tetraethyl titanate, and the organic solvent is one or more of methanol, ethanol, butanol and isopropanol. The titanium source and the organic solvent are mixed to obtain a titanium source solution, and the concentration of the titanium source solution is 12-15wt%.
[0022] In the present invention, the removal of the solvent in step (2) can be carried out by a conventional desolventizing method. In a specific embodiment, the removal can be carried out by vacuum distillation. Specifically, the operation is carried out in a flask, the pressure in the flask is controlled to 40-60 kPa, and the solution is heated to 40-60° C. until the organic solvent is completely removed.
[0023] In the present invention, the crystallization reaction temperature in step (2) is 150-170° C., and the crystallization time is 16-72 h, preferably 20-30 h.
[0024] In the present invention, the mass ratio of silicon source converted to SiO2, titanium source converted to TiO2, template, surfactant, polymer latex ball and deionized water is 1: (0.01-0.033): (0.15-0.3): (0.01-0.03): (0.3-0.5): (10-25).
[0025] In the present invention, the spray drying in step (3) is: spray drying is performed using a spray drying device to obtain a spherical structure intermediate of the polymer-titanium silicate molecular sieve.
[0026] Preferably, the feeding rate of the crystallization mother solution in the spray drying device is 2 to 15 kg / h, for example, 2 kg / h, 4 kg / h, 6 kg / h, 8 kg / h, 10 kg / h, 12 kg / h or 15 kg / h, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0027] Preferably, the inlet temperature of the drying air in the spray drying device is 300-450°C, for example, 300°C, 330°C, 350°C, 370°C, 390°C, 400°C, 420°C, 440°C or 450°C, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0028] Preferably, the outlet temperature of the drying air in the spray drying device is 150-220°C, for example, 150°C, 170°C, 190°C, 200°C, 210°C or 220°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable;
[0029] Preferably, the flow rate of the drying air in the spray drying device is 100-300 Nm 3 / h, for example, it can be 100Nm 3 / h、150Nm 3 / h、200Nm 3 / h、250Nm 3 / h or 300Nm 3 / h, etc., but not limited to the listed values, other values not listed in the numerical range are also applicable;
[0030] Preferably, the spray drying device comprises a centrifugal spray dryer or a pressure spray dryer, the rotation speed of the centrifugal spray dryer is 5000-20000 rpm, and the pressure of the pressure spray dryer is 6-30 kg / cm 2 .
[0031] In the present invention, during the spray drying process, the polymer latex spheres are self-assembled into droplets, and the titanium silicalite material is coated around the polymer latex spheres to obtain a spherical structure intermediate with inorganic titanium silicalite on the outside and organic polymer on the inside.
[0032] In the spray drying process of the present invention, the average diameter of the spherical structure intermediate can be regulated by changing the rotation speed of the centrifugal spray dryer, the pressure of the pressure spray dryer, the feed rate or other control parameters of the spray drying device, and the concentration of the crystallization mother solution.
[0033] In the present invention, the calcination in step (3) can be carried out in an air atmosphere; preferably, the heating rate of the calcination in step (3) is 20 to 50°C / min, for example, it can be 20°C / min, 25°C / min, 30°C / min, 35°C / min, 40°C / min or 50°C / min, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0034] In the present invention, the organic polymer inside the prepared spherical structure intermediate is decomposed and burned to generate gas by rapid heating in an air atmosphere, so that the inorganic titanium silicon oxide forms a porous nanostructure. At the same time, the template agent of the titanium silicalite is removed during the calcination process, so that the pore structure of the catalyst is richer.
[0035] Preferably, the temperature rise end point of the calcination in step (3) is 650-800°C, for example, it can be 650°C, 670°C, 700°C, 720°C, 740°C, 760°C, 780°C or 800°C, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0036] Preferably, the calcination in step (3) is followed by heat preservation for 4 to 8 hours, for example, 4 hours, 5 hours, 6 hours, 7 hours or 8 hours, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0037] In a second aspect, the present invention provides a titanium silicon catalyst with a porous structure, and the titanium silicon catalyst is prepared by the preparation method described in the first aspect.
[0038] Preferably, the pore size of the titanium silicon catalyst is 50-120 nm, for example, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, 110 nm or 120 nm, but is not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0039] The titanium silicon catalyst of the present invention is a cage-like porous structure with a nanometer-level pore size, which is beneficial to the adsorption and diffusion of materials and improves the activity of the catalyst and the selectivity for the target product.
[0040] As a preferred technical solution of the present invention, the particle size of the titanium silicon catalyst is 1.0-5.0 μm, for example, 1.0 μm, 1.5 μm, 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm or 5.0 μm, but not limited to the listed values, and other values not listed in the numerical range are also applicable. Preferably, the specific surface area of the titanium silicon catalyst is 400-700 m 2 / g, for example, 400m 2 / g, 450m 2 / g, 480m 2 / g、500m 2 / g, 550m 2 / g、600m 2 / g or 700m 2 / g, etc., but are not limited to the listed values, and other unlisted values within the numerical range are also applicable.
[0041] In a third aspect, the present invention provides the use of the porous structured titanium silicon catalyst as described above, wherein the titanium silicon catalyst is used for catalyzing the epoxidation of olefins to prepare epoxy compounds.
[0042] Preferably, the olefin is propylene or butene, and the epoxy compound is propylene oxide or butylene oxide. The specific steps of using the titanium silicon catalyst to catalyze the epoxidation of olefins to prepare the epoxy compound are: loading the catalyst into a reactor, and then introducing the olefin and peroxide solution to undergo epoxidation reaction to obtain the epoxy compound.
[0043] Preferably, the pressure of the epoxidation reaction is 3.0-4.5 MPa, for example, 3.0 MPa, 3.5 MPa, 4.0 MPa or 4.5 MPa, but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0044] Preferably, the temperature of the epoxidation reaction is 60-90°C, for example, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C or 90°C, etc., but is not limited to the listed values, and other values not listed within the numerical range are also applicable.
[0045] Preferably, the peroxide in the peroxide solution can be selected from peroxides commonly used in the art, such as ethylbenzene hydroperoxide, cumene hydroperoxide, tert-butyl hydroperoxide or cyclohexyl hydroperoxide.
[0046] Other conditions in the method for preparing epoxy compounds by catalyzing olefin epoxidation using the titanium silicon catalyst of the present invention can adopt the conditions commonly used in the art and can be specifically adjusted by those skilled in the art.
[0047] The numerical range described in the present invention not only includes the point values listed above, but also includes any point values between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values included in the range.
[0048] Compared with the prior art, the present invention has the following beneficial effects:
[0049] (1) Compared with conventional titanium silicon molecular sieve catalysts, the porous titanium silicon catalyst of the present invention has a cage-type porous structure, which is more conducive to the adsorption and diffusion of materials, and can improve the activity of the catalyst and the selectivity for the target product;
[0050] (2) The preparation method of the present invention obtains an organic-inorganic mixed spherical intermediate by spray drying, and then the organic polymer inside is decomposed and burned to produce gas during the roasting process, so that the titanium silicon catalyst forms a porous nanostructure. At the same time, the titanium silicon molecular sieve produces a richer pore structure during the roasting process. The process flow is simple and easy to realize industrial large-scale production;
[0051] (3) The titanium silicon catalyst prepared in the present invention can achieve efficient conversion of peroxide and high selectivity of epoxidation products at relatively low pressure and temperature, with a peroxide conversion rate of ≥99.9% and an epoxidation product selectivity of ≥97.0%. BRIEF DESCRIPTION OF THE DRAWINGS
[0052] Figure 1 This is a SEM image (2 μm) of the porous titanium silicon catalyst prepared in Example 1 of the present invention;
[0053] Figure 2 This is a SEM image (200 nm) of the porous titanium silicon catalyst prepared in Example 1 of the present invention;
[0054] Figure 3 This is the pore size distribution diagram of the porous titanium silicon catalyst prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0055] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.
[0056] Where specific experimental steps or conditions are not specified in the examples, the corresponding conventional experimental steps or conditions in the art can be used. The reagents or instruments used without specifying the manufacturer are all conventional products that can be purchased commercially.
[0057] PMMA latex microspheres: MSI-PM300NM, Shanghai Zhenzhun Biological Company;
[0058] PEEK latex microspheres: Victrex PEEK 450CA30;
[0059] PET latex microspheres: DuPont PET 408NC010;
[0060] <Testing Equipment>
[0061] SEM characterization: JEOL JSM-5900LV scanning electron microscope;
[0062] BET characterization: PoreMaster 33 series mercury porosimeter from Anton Paar.
[0063] Example 1
[0064] The preparation method of the porous titanium silicon catalyst comprises the following steps:
[0065] (1) 1.0 g of coco-glucoside, 15.4 g of tetrapropylammonium hydroxide, 30.7 g of monodisperse PMMA latex microspheres (average particle size 270 nm, MSI-PM300 nm) and 2050 g of deionized water were mixed evenly, and then 356 g of tetraethyl orthosilicate was added and fully stirred and hydrolyzed at 40° C. for 5 h to prepare gel A;
[0066] (2) 8.4 g of tetrabutyl titanate was dissolved in 61.5 g of isopropanol and mixed evenly to obtain a titanium source solution, and the titanium source solution was added dropwise to gel A. After the addition was completed, the temperature was raised to 60° C., the stopper of the three-necked flask was opened, and the alcohol was removed by stirring at 60° C. for 1 h to prepare titanium silicalose gel B;
[0067] (3) The titanium silica gel B was transferred to a hydrothermal reactor and crystallized at 170° C. for 24 h. After the reaction was completed, the crystallization mother liquor was spray-dried using a pressure spray dryer at a feed rate of 2.0 kg / h to obtain a spherical structure intermediate with a PMMA polymer as the core and a titanium silicalite molecular sieve as the outer portion;
[0068] The pressure of the pressure spray dryer is 20kg / cm 2 The inlet temperature of the dry air in the pressure spray dryer is 420°C, the outlet temperature is 200°C and the flow rate is 300Nm 3 / h;
[0069] (4) The spherical structure intermediate of the polymer-titanium silicon molecular sieve described in step (3) is heated to 650°C at a heating rate of 30°C / min in an air atmosphere and calcined. After keeping the temperature for 4 hours, the temperature is lowered to room temperature to obtain the porous structure titanium silicon catalyst described in the present invention.
[0070] The porous titanium silicon catalyst prepared in this example was characterized by SEM and BET. The SEM characterization results are as follows: Figure 1 and Figure 2 As shown in the figure, it can be seen that the titanium silicon catalyst has a cage-like porous nanostructure with a particle size of 1.0-5.0 μm; the BET characterization results are shown in Figure 3 As shown, the macropore diameter of the titanium silicon catalyst is 80nm and the specific surface area is 500m 2 / g.
[0071] Example 2
[0072] The preparation method of the porous titanium silicon catalyst comprises the following steps:
[0073] (1) 2.1 g of polysorbate, 20.5 g of tetrapropylammonium hydroxide, 35.9 g of monodisperse PEEK latex microspheres (average particle size 180 nm) and 2050 g of deionized water were mixed evenly, and then 356 g of tetraethyl orthosilicate was added and fully stirred for hydrolysis at 40° C. for 6 h to prepare gel A;
[0074] (2) 12.7 g of tetrabutyl titanate was dissolved in 72 g of isopropanol and mixed evenly to obtain a titanium source solution, and the titanium source solution was added dropwise to gel A. After the addition was completed, the temperature was raised to 60° C., the stopper of the three-necked flask was opened, and the alcohol was removed by stirring at 60° C. for 1 h to prepare titanium silicalose gel B;
[0075] (3) The titanium silica gel B was transferred to a hydrothermal reactor and crystallized at 160° C. for 24 h. After the reaction was completed, the crystallization mother liquor was spray-dried using a pressure spray dryer at a feed rate of 5.0 kg / h to obtain a spherical structure intermediate with a PEEK polymer as the core and a titanium silicalite molecular sieve as the outer portion;
[0076] The pressure of the pressure spray dryer is 20kg / cm 2 The inlet temperature of the dry air in the pressure spray dryer is 450°C, the outlet temperature is 220°C and the flow rate is 300Nm 3 / h;
[0077] (4) The spherical structure intermediate of the polymer-titanium silicon molecular sieve described in step (3) is heated to 650°C at a heating rate of 30°C / min in an air atmosphere and calcined. After keeping the temperature for 5 hours, the temperature is lowered to room temperature to obtain the porous structure titanium silicon catalyst described in the present invention.
[0078] The porous titanium silicon catalyst prepared in this example was characterized by SEM and BET. The titanium silicon catalyst was a cage-like porous structure with a particle size of 2-5 μm. The macropore diameter of the porous titanium silicon catalyst was 70 nm and the specific surface area was 550 m 2 / g.
[0079] Example 3
[0080] The preparation method of the porous titanium silicon catalyst comprises the following steps:
[0081] (1) 3.1 g of glyceryl monostearate, 30.7 g of tetrapropylammonium hydroxide, 41.0 g of monodisperse PET latex microspheres (average particle size 200 nm) and 2050 g of deionized water were mixed uniformly, and then 135 g of white carbon black (fumed SiO2) was added and fully stirred and hydrolyzed at 40° C. for 5 h to prepare gel A;
[0082] (2) 5.5 g of tetrabutyl titanate was dissolved in 40.3 g of ethanol and mixed evenly to obtain a titanium source solution, and the titanium source solution was added dropwise to gel A. After the addition was completed, the temperature was raised to 40° C., the stopper of the three-necked flask was opened, and the alcohol was removed by stirring at 40° C. for 3 h to prepare titanium silicalite gel B;
[0083] (3) The titanium silica gel B was transferred to a hydrothermal reactor and crystallized at 170° C. for 40 h. After the reaction was completed, the crystallized mother liquor was spray-dried using a pressure spray dryer at a feed rate of 12.0 kg / h to obtain a spherical structure intermediate with a core of PET polymer and an outer portion of titanium silicalite molecular sieve;
[0084] The pressure of the pressure spray dryer is 20kg / cm 2 The inlet temperature of the dry air in the pressure spray dryer is 400°C, the outlet temperature is 180°C and the flow rate is 300Nm 3 / h;
[0085] (4) The spherical structure intermediate of the polymer-titanium silicon molecular sieve described in step (3) is heated to 700°C at a heating rate of 20°C / min in an air atmosphere and calcined. After keeping the temperature for 8 hours, the temperature is lowered to room temperature to obtain the porous structure titanium silicon catalyst described in the present invention.
[0086] The porous titanium silicon catalyst prepared in this example was characterized by SEM and BET. The titanium silicon catalyst was a cage-like porous structure with a particle size of 1.5-4.0 μm. The macropore diameter of the porous titanium silicon catalyst was 50 nm and the specific surface area was 600 m 2 / g.
[0087] Example 4
[0088] This embodiment provides a porous titanium silicon catalyst and a preparation method thereof. Except that the crystallization time in step (3) is 72 hours, other conditions are the same as those in Example 1.
[0089] The porous titanium silicon catalyst prepared in this example was characterized by SEM and BET. The titanium silicon catalyst was a cage-like porous structure with a particle size of 2-5 μm. The macropore diameter of the porous titanium silicon catalyst was 50 nm and the specific surface area was 600 m 2 / g.
[0090] Example 5
[0091] This embodiment provides a porous titanium silicon catalyst and a preparation method thereof. Except that the heating rate of the calcination process in step (4) is 50°C / min, other conditions are the same as those in Example 1.
[0092] The porous titanium silicon catalyst prepared in this example was characterized by SEM and BET. The titanium silicon catalyst was a cage-like porous structure with a particle size of 1.0-5.0 μm. The macropore diameter of the porous titanium silicon catalyst was 120 nm and the specific surface area was 400 m 2 / g.
[0093] Example 6
[0094] This embodiment provides a porous titanium silicon catalyst and a preparation method thereof. Except that the heating end point of the calcination in step (4) is 800° C., other conditions are the same as those in Example 1.
[0095] The porous titanium silicon catalyst prepared in this example was characterized by SEM and BET. The titanium silicon catalyst was a cage-like porous structure with a particle size of 1.0-4.0 μm. The macropore diameter of the porous titanium silicon catalyst was 70 nm and the specific surface area was 500 m 2 / g.
[0096] Comparative Example 1
[0097] This comparative example provides a titanium silicon catalyst and a preparation method thereof. Except that in step (1), "30.7 g of monodisperse PMMA latex microspheres (average particle size 270 nm)" is replaced with PMMA latex microspheres with an average particle size of 45 nm (brand: MSI-PM045NM), other conditions are the same as those in Example 1.
[0098] Comparative Example 2
[0099] This comparative example provides a titanium silicon catalyst and a preparation method thereof. Except that "30.7 g of monodisperse PMMA latex microspheres (average particle size 270 nm) and 1.0 g of coconut oil glucoside" are not added in step (1), other conditions are the same as those in Example 1.
[0100] Comparative Example 3
[0101] This comparative example provides a titanium silicon catalyst and a preparation method thereof. Except that 1.0 g of coconut glucoside is not added in step (1), other conditions are the same as those in Example 1.
[0102] Comparative Example 4
[0103] This comparative example provides a titanium silicon catalyst and a preparation method thereof. Except that the spray drying in step (3) is adjusted to drying in an oven at 200° C., other conditions are the same as those in Example 1.
[0104] Comparative Example 5
[0105] This comparative example uses 20.0 g of titanium silicalite commercial catalyst (purchased from China Catalyst Company, brand: TS-1).
[0106] The catalysts in Examples 1-6 and Comparative Examples 1-5 were respectively tested for their activity in catalyzing the epoxidation of propylene to prepare propylene oxide. The conditions were as follows: the prepared epoxidation catalyst was loaded into a fixed bed reactor with an inner diameter of 30 mm, the loading amount of the catalyst was controlled to be 20 g, propylene was used as a raw material, ethylbenzene hydroperoxide (EBHP) and cumene hydroperoxide (CHP) were used as oxidants to test the catalytic activity of the epoxidation reaction, the molar ratio of propylene to EBHP was controlled to be 6:1 during the EBHP oxidant process, and the feed mass space velocity was 3 h -1 , the reaction pressure was 4.0 MPa, the reaction temperature was 60 ° C, and the conversion rate of EBHP and the selectivity of propylene oxide were tested. The results are shown in Table 2. In the process of using CHP as the oxidant, the molar ratio of propane to CHP was controlled to be 8:1, and the feed mass space velocity was 5h -1 , the reaction pressure was 4.0 MPa, the reaction temperature was 80°C, and the conversion rate of CHP and the selectivity of propylene oxide were obtained. The results are shown in Table 2.
[0107] The conversion rate of EBHP / CHP was determined by iodine titration. The potentiometric titrator used in the iodine titration was produced by Swiss Metrohm Company, model 916Ti-Touch. The calculation formula was:
[0108]
[0109] Among them, V Na2S2O3 is the volume of Na2S2O3 solution consumed, C Na2S2O3 is the molar concentration of the Na2S2O3 solution used;
[0110]
[0111] The selectivity of propylene oxide was determined by gas chromatography, and the gas chromatograph used was Shimadzu's GC-2010 Plus. The mass concentration of propylene oxide in the reaction product after the catalytic activity test was calculated by gas chromatograph using the internal standard method, with DMF (dimethylformamide) as the solvent and DT (dioxane) as the internal standard. The operating parameters of the gas chromatograph are shown in Table 1.
[0112] The selectivity of propylene oxide = (mass concentration of propylene oxide × mass of reaction product) / mass of propylene oxide produced by theoretically oxidizing propane with the oxidant actually converted × 100%.
[0113] Table 1 Gas chromatograph operating parameters
[0114]
[0115] Table 2 Oxidant conversion and selectivity of propylene oxide
[0116]
[0117] It can be seen from Table 2 that the catalyst prepared by the method of the present invention has high activity. Under the same conditions, the EBHP / CHP conversion rate is high and the PO selectivity is high, which means that the well-developed pore structure of the catalyst is conducive to the adsorption and diffusion of the reactants, and the catalyst has significantly better conversion rate of the oxidant and selectivity of the PO product.
[0118] (1) It can be seen from Example 1 and Comparative Example 1 that when the particle size of the added polymer latex ball is too small, the porous cage structure formed has a small pore size, resulting in poor catalyst activity and low peroxide conversion rate; it can be seen from Example 1 and Comparative Examples 2 and 3 that when no surfactant is added, the polymer is easy to agglomerate, resulting in poor catalyst activity and low peroxide conversion rate;
[0119] (2) Based on Example 1 and Comparative Example 4, it can be seen that when the conventional drying method is used, the process of latex spheres self-assembling into droplets cannot be achieved, resulting in poor catalyst activity and low peroxide conversion rate;
[0120] (3) Comparative Example 5 shows that the commercially available titanium silicon molecular sieve catalyst has insufficient reaction activity, a low peroxide raw material conversion rate, and a low PO selectivity.
[0121] The applicant declares that the present invention illustrates the detailed structural features of the present invention through the above-mentioned embodiments, but the present invention is not limited to the above-mentioned detailed structural features, that is, it does not mean that the present invention must rely on the above-mentioned detailed structural features to be implemented. Those skilled in the art should understand that any improvement of the present invention, equivalent replacement of the components selected by the present invention, addition of auxiliary components, selection of specific methods, etc., all fall within the protection scope and disclosure scope of the present invention.
Claims
1. A method for preparing a porous titanium silicon catalyst, characterized in that: The preparation method comprises the following steps: (1) stirring and mixing a surfactant, a template, polymer latex balls and water, and then adding a silicon source for hydrolysis to obtain gel A; (2) mixing the titanium source and the organic solvent evenly, adding the mixture to the gel A, stirring evenly and removing the organic solvent to obtain the titanium silicalite gel B; (3) The titanium silicalite gel B is transferred to a hydrothermal reactor for crystallization reaction to obtain a crystallization mother liquor, and the crystallization mother liquor is spray-dried and calcined to prepare a titanium silicalite catalyst with a porous structure.
2. The preparation method according to claim 1, characterized in that: The silicon source in step (1) is one of tetraethyl orthosilicate, tetramethyl orthosilicate, tetrapropyl orthosilicate, tetrabutyl orthosilicate, or a mixture of two or more thereof, or at least one of silica sol and white carbon black; Preferably, the template in step (1) is selected from one or a mixture of two or more of tetrapropylammonium hydroxide, tetrapropylammonium bromide, tetrapropylammonium chloride, and tetrapropylammonium fluoride; Preferably, the polymer latex spheres in step (1) are selected from any one or a combination of at least two of PMMA, ABS, PAA, PEEK or PET; Preferably, the particle size of the polymer latex spheres in step (1) is 150 to 500 nm; Preferably, the surfactant in step (1) is selected from any one of coconut glucoside, lauryl glucoside, cetearyl glucoside, glyceryl monostearate or polysorbate, or a combination of at least two thereof; preferably, the hydrolysis temperature in step (1) is 40-60° C. and the time is 4-8 h.
3. The preparation method according to claim 1 or 2, characterized in that: The titanium source in step (2) is any one or more of titanium tetrachloride, titanium tetrabromide, tetraethyl titanate, tetrapropyl titanate, isopropyl titanate or tetrabutyl titanate; Preferably, the organic solvent in step (2) is one or more of methanol, ethanol, isopropanol, and butanol; Preferably, the mass fraction of the titanium source after mixing with the organic solvent in step (2) is 12-15wt%.
4. The preparation method according to any one of claims 1 to 3, characterized in that In the present invention, the mass ratio of silicon source converted into SiO2, titanium source converted into TiO2, template, surfactant, polymer latex ball and water is 1: (0.01-0.033): (0.15-0.3): (0.01-0.03): (0.3-1.5): (10-25).
5. The preparation method according to claim 1, characterized in that: In step (3), the crystallization temperature is 150-170° C., and the crystallization time is 16-72 h, preferably 20-30 h.
6. The preparation method according to claim 1, characterized in that: The spray drying in step (3) is performed by using a spray drying device, wherein the spray drying device is selected from a pressure spray dryer or a centrifugal spray dryer; Preferably, the feeding rate of the crystallization mother solution in the spray drying device is 2 to 15 kg / h; Preferably, the inlet temperature of the drying air in the spray drying device is 300-450°C; Preferably, the outlet temperature of the drying air in the spray drying device is 150-220°C; Preferably, the flow rate of the drying air in the spray drying device is 100-300 Nm 3 / h.
7. The preparation method according to any one of claims 1 to 6, characterized in that: The calcination in step (3) is carried out in an air atmosphere; Preferably, the heating rate of the calcination in step (3) is 20 to 50°C / min; Preferably, the temperature end point of the calcination in step (3) is 650-800°C; Preferably, the calcination in step (3) is followed by insulation, and more preferably the insulation time is 4 to 8 hours.
8. A porous titanium silicon catalyst, characterized in that: The titanium silicon catalyst is prepared by the preparation method described in any one of claims 1 to 7, and the titanium silicon catalyst has a cage-like porous structure; Preferably, the pore size of the titanium silicon catalyst is 50-120 nm; preferably, the particle size of the titanium silicon catalyst is 1.0-5.0 μm; preferably, the specific surface area of the titanium silicon catalyst is 400-700 m 2 / g.
9. An application of the porous titanium silicon catalyst as claimed in claim 8, characterized in that: The titanium silicon catalyst is used for catalyzing the liquid phase epoxidation of olefins to prepare epoxy compounds.
10. A method for preparing an epoxy compound, characterized in that: The preparation method comprises: loading the titanium silicon catalyst according to claim 8 into a reactor, and then introducing olefin and peroxide solution to carry out epoxidation reaction to obtain an epoxy compound; Preferably, the olefin is propylene or butene; Preferably, the peroxide in the peroxide solution is selected from ethylbenzene hydroperoxide, cumene hydroperoxide, tert-butyl hydroperoxide or cyclohexyl hydroperoxide; Preferably, the epoxy compound is propylene oxide or butylene oxide; Preferably, the reaction pressure is 3.0-4.5 MPa; Preferably, the reaction temperature is 60-90°C.
Citation Information
Patent Citations
Ordered macropore-mesopore hierarchical pore titanium silicalite molecular sieve TS-1 single crystal with opal structure and synthesis method thereof
CN106276958A
Modification method and application of spray-molded microspheric titanium silicalite molecular sieve
CN111115653A
Preparation method and application of Au-TS-1 nano-microsphere catalyst for propylene gas-phase epoxidation
CN115845916A
Multi-stage porous titanium-silicon zeolite preparation method and its uses in catalytic oxidation
CN1807244A
Epoxidation process using titanium-rich silicalite catalysts
US5262550A