Flotation reagent and flotation separation method for copper-molybdenum-sulfur metal ore

By using a combination of inhibitors such as guar gum and collectors such as ethyl thiocarbamate, along with a cascade flotation process, the problem of separating low-grade copper, molybdenum, and sulfur resources was solved, achieving efficient separation and high-grade recovery of copper, molybdenum, and sulfur, simplifying the process flow and reducing energy consumption.

CN118976602AActive Publication Date: 2024-11-19JIANGXI COPPER +1
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411064154.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Existing technologies are insufficient to effectively separate low-grade associated copper, molybdenum, and sulfur resources, resulting in inadequate recovery rates and grades of copper, molybdenum, and sulfur. Furthermore, the processes are complex and energy-intensive.

Method used

A specific combination of flotation reagents, including guar gum, locust bean gum, or fenugreek gum as inhibitors, and ethyl thiocarbamate-O-(1-methylethyl) ester, diethyl phthalate, and amidothiourea as collectors, combined with a step-flotation process, is used to achieve efficient separation of copper, molybdenum, and sulfur.

Benefits of technology

It achieves efficient separation and high-grade recovery of copper, molybdenum and sulfur, reduces reagent usage, simplifies the process, and reduces energy consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004978882820000121
    Figure BDA0004978882820000121
  • Figure BDA0004978882820000131
    Figure BDA0004978882820000131
Patent Text Reader

Abstract

The invention provides a flotation reagent and a flotation separation method for copper-molybdenum-sulfur metal ore, and relates to the technical field of ore dressing. Specifically, the flotation reagent comprises an inhibitor and a collecting agent; wherein the inhibitor comprises at least one of guar gum, locust bean gum or fenugreek gum; and the collecting agent comprises at least one of ethyl thiocarbamic acid-O-(1-methyl ethyl) ester, diethyl phthalate or amidino thiourea. Based on a lead-zinc-copper-molybdenum-sulfur mixed flotation separation process in the prior art, in order to overcome the defects that the product grade or the recovery rate is insufficient, or the technological process is complex and the like, the invention provides a novel sulfur mineral collecting and inhibiting agent and an efficient, simple and convenient short-flow process from the angle of combination of a flotation reagent and the technological process. Therefore, the copper-molybdenum-sulfur mixed flotation and efficient separation thereof are realized, and the method has a good application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of mineral processing, and in particular to a flotation agent and a flotation separation method for copper, molybdenum and sulfur metal ores. Background Art

[0002] As the main copper-containing mineral, chalcopyrite usually coexists with pyrite, molybdenite and other sulfide-containing minerals to form copper-molybdenum-sulfur polymetallic sulfide deposits; therefore, the effective separation of copper, molybdenum and sulfur is of great significance for the efficient development of copper resources. At present, for low-grade co-existing copper, molybdenum and sulfur resources, a mixed flotation process is often used, that is, copper is recovered by adding a large amount of activator and sulfide ore collector, which makes it difficult to effectively separate molybdenum and sulfur after mixed flotation, and thus cannot be effectively utilized.

[0003] Patent CN202111332583.4 discloses a separation and recovery method for ultra-low-grade difficult-to-select copper-molybdenum sulfide ores. By developing a combined separation and recovery process of magnetic separation and flotation, the copper-molybdenum mixed sulfide ore is first subjected to mixed flotation to obtain a copper-molybdenum mixed rough concentrate, and then the copper-molybdenum mixed rough concentrate is pre-separated by magnetic separation to obtain magnetic concentrate copper sulfide and magnetic tailings molybdenum sulfide; finally, the magnetic concentrate and tailings are re-enriched by flotation, and finally copper sulfide and molybdenum sulfide concentrate products are obtained respectively. This process can realize the economical and efficient recovery of copper-molybdenum mixed sulfide ore resources of different grades, and can greatly reduce the amount of sodium sulfide, improve the working environment, and reduce environmental risks; however, this method does not realize the separation of copper and molybdenum from sulfur, and involves magnetic separation steps, a long process flow, and high energy consumption.

[0004] Patent CN201911248477.0 discloses a flotation method for separation of copper, molybdenum and sulfur, including: mixing the raw ore with lime for grinding, and then adding flotation agent A (dextrin, TS-1, 2# oil) for one roughing, one concentrating and one scavenging to obtain copper concentrate and tailings A; then adding flotation agent B (TM-8) to tailings A for one roughing, four concentrating and one scavenging to obtain molybdenum concentrate and tailings B; then adding flotation agent C (sulfur, butyl xanthate) to tailings B for one roughing, two concentrating and one scavenging to obtain sulfur concentrate and tailings D. This method realizes multi-element separation and has comprehensive recovery value; however, the grade and recovery rate of copper, molybdenum and sulfur in this method still cannot achieve a high level.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The first purpose of the present invention is to provide a flotation agent for copper-sulfur minerals, which is particularly suitable for the inhibition or capture of sulfur in copper-molybdenum-sulfur polymetallic ores, and improves the flotation effect by adopting specific functional groups and compound combinations.

[0007] The second purpose of the present invention is to provide a flotation separation method for copper-molybdenum-sulfur metal ore. Based on the existing lead-zinc, copper-molybdenum-sulfur mixed flotation separation process in the prior art, in order to solve the defects of insufficient product grade or recovery rate, or complicated process flow, the present invention provides a new type of sulfur mineral inhibitor and an efficient and simple short-process process from the perspective of combining flotation agents and process flow to achieve efficient separation of copper-molybdenum-sulfur after mixed flotation.

[0008] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:

[0009] A flotation reagent for copper-sulfur minerals, comprising a depressant and a collector;

[0010] wherein the inhibitor comprises at least one of guar gum, locust bean gum or fenugreek gum;

[0011] The collector includes at least one of ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea.

[0012] A flotation separation method for copper-molybdenum-sulfur metal ore adopts the flotation agent for copper-sulfur minerals.

[0013] Compared with the prior art, the present invention has the following beneficial effects:

[0014] (1) The sulfur mineral inhibitor provided by the present invention uses at least one of guar gum, locust bean gum or fenugreek gum, which can achieve effective separation of copper-sulfur minerals. In the synergistic effect of the gum agents, metal ions are combined with -COOH to selectively adsorb Fe atoms on the surfaces of pyrite and chalcopyrite, thereby achieving efficient separation of chalcopyrite and pyrite.

[0015] (2) The present invention adopts specific flotation reagents and cascade flotation process for copper, molybdenum and sulfur polymetallic minerals, which reduces the dosage of reagents and realizes efficient separation and high-grade recovery of copper, molybdenum and sulfur. DETAILED DESCRIPTION

[0016] The technical scheme of the present invention will be clearly and completely described below in conjunction with specific embodiments, but those skilled in the art will appreciate that the following described embodiments are part of embodiments of the present invention, rather than all embodiments, and are only used to illustrate the present invention, and should not be considered as limiting the scope of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work are within the scope of protection of the present invention. Those who do not specify specific conditions in the embodiments are carried out according to conventional conditions or conditions recommended by the manufacturer. Those who do not specify the manufacturer for reagents or instruments used are conventional products that can be purchased commercially. In addition, the terms "one", "two", "1", "2" are only used for descriptive purposes and cannot be interpreted as indicating or implying relative importance.

[0017] The first aspect of the present invention is to provide a flotation agent for copper-sulfur minerals; wherein the flotation agent includes an inhibitor and a collector, the inhibitor includes at least one of guar gum, locust bean gum or fenugreek gum, and the collector includes at least one of ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate or guanylthiourea.

[0018] As a preferred embodiment, the inhibitor comprises a combination of guar gum, locust bean gum and fenugreek gum; in some more preferred embodiments, the mass ratio of the guar gum, the locust bean gum and the fenugreek gum is (2-6): (1-2): (2-6).

[0019] As a preferred embodiment, based on the high viscosity and thickening performance of the inhibitor component, the thickener is dispersed in an aqueous solution before the inhibitor is used and added in the form of an aqueous solution.

[0020] As a preferred embodiment, the collector comprises a combination of ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea; in some more preferred embodiments, the mass ratio of the ethylthiocarbamate-O-(1-methylethyl) ester, the diethyl phthalate and the guanylthiourea is (4-7):(1-5):(4-9).

[0021] The three optional collector components used in the present invention are all compounds with fixed molecular formula and molecular structure; among them, the CAS number of ethylthiocarbamate-O-(1-methylethyl) ester is 141-98-0, the CAS number of diethyl phthalate is 84-66-2, and the CAS number of guanylthiourea is 2114-02-5. In the implementation process of the present invention, the corresponding commercially available industrial grade pure products can be used as collectors.

[0022] The second aspect of the present invention is to provide a flotation separation method for copper-molybdenum-sulfur metal ore, using the flotation agent for copper-sulfur minerals as described in the first aspect above.

[0023] The flotation separation method mainly comprises the following steps: (1) copper-sulfur mixed flotation: subjecting the pulp of the copper-molybdenum-sulfur metal ore to a roughing operation, subjecting the roughing tailings to three scavenging operations, and obtaining a copper-molybdenum-sulfur mixed flotation concentrate and tailings; (2) copper-sulfur separation flotation: subjecting the pulp of the copper-molybdenum-sulfur mixed flotation concentrate to a second roughing operation, three second scavenging operations and two second concentrating operations, and obtaining a copper-molybdenum concentrate and a sulfur-containing tailings.

[0024] As a preferred embodiment, in step (1), the concentration of the copper-molybdenum-sulfur metal ore slurry is 30% to 40%, and the pH of the slurry is adjusted to 6 to 8; in the present invention, the solvent of the slurry is water by default.

[0025] As a preferred embodiment, the flotation reagent involved in step (1) includes the inhibitor and the collector as described in the first aspect, and a frother; in some more preferred embodiments, the frother includes pine oil.

[0026] As a preferred embodiment, in step (1), the dosage of the roughing agent includes: based on the mass of the slurry, 1000-2000 g / t of inhibitor, 50-200 g / t of collector and 20-50 g / t of frother; in some optional embodiments, the dosage of the inhibitor includes but is not limited to any one of 1000, 1100, 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000 (g / t) or a numerical range consisting of any two of them; the dosage of the collector includes but is not limited to any one of 50, 60, 80, 100, 120, 150, 175, 180, 190, 200 (g / t) or a numerical range consisting of any two of them; the dosage of the frother includes but is not limited to any one of 20, 30, 40, 50 (g / t) or a numerical range consisting of any two of them.

[0027] As a preferred embodiment, in step (1), the dosage of the agent for the selection includes: based on the mass of the slurry, the dosage of the inhibitor in the first selection is 200-500 g / t, and the dosage of the inhibitor in the second selection is 50-150 g / t; in some optional embodiments, the dosage of the inhibitor in the first selection includes but is not limited to any one of 200, 250, 300, 350, 400, 450, 500 (g / t) or a numerical range consisting of any two of them, and the dosage of the inhibitor in the second selection includes but is not limited to any one of 50, 60, 80, 100, 120, 125, 140, 150 (g / t) or a numerical range consisting of any two of them.

[0028] As a preferred embodiment, in step (1), the amount of the scavenging agent includes: based on the mass of the slurry, the amount of the collector in the first scavenging is 50-100 g / t, and the amount of the collector in the second scavenging is 10-30 g / t; in some optional embodiments, the amount of the collector in the first scavenging includes but is not limited to any one of 50, 60, 70, 80, 90, 100 (g / t) or a numerical range consisting of any two of them, and the amount of the collector in the second scavenging includes but is not limited to any one of 10, 15, 20, 25, 30 (g / t) or a numerical range consisting of any two of them.

[0029] It can be understood that in some preferred embodiments, in step (1), only inhibitors are added during the selection process, only collectors are added during the scanning process; and no additional agents are added during the third scanning process.

[0030] As a preferred embodiment, in step (2), the concentration of the slurry of the copper-molybdenum-sulfur mixed flotation concentrate is 20% to 30%, and the pH of the slurry is adjusted to 8 to 9; in the present invention, the solvent of the slurry is water by default.

[0031] As a more preferred embodiment, in steps (1) and (2), the acid and alkali reagents used to adjust the pH of the slurry include but are not limited to quicklime and lime products, hydrochloric acid, etc.

[0032] As a preferred embodiment, the flotation reagent involved in step (2) includes the inhibitor and the collector as described in the first aspect, and a frother; in some more preferred embodiments, the frother includes pine oil.

[0033] As a preferred embodiment, in step (2), the dosage of the second roughing agent includes: based on the mass of the slurry, 1200-2500 g / t of inhibitor, 50-250 g / t of collector and 10-15 g / t of frother; in some optional embodiments, the dosage of the inhibitor includes but is not limited to 1200, 1300, 1400, 1500, 1600, 1700, 1800, 1900, 2000, 2100, 2200, 2300, The dosage of the collector includes but is not limited to any one of 50, 60, 80, 100, 125, 150, 175, 200, 225, 240, 250 (g / t) or the numerical range formed by any two of them; the dosage of the foaming agent includes but is not limited to any one of 10, 11, 12, 13, 14, 15 (g / t) or the numerical range formed by any two of them.

[0034] As a preferred embodiment, in step (2), the dosage of the second concentration reagent includes: based on the mass of the slurry, the dosage of the inhibitor in the first second concentration is 100-350 g / t, and the dosage of the inhibitor in the second second concentration is 50-150 g / t; in some optional embodiments, the dosage of the inhibitor in the first second concentration includes but is not limited to any one of 100, 125, 150, 175, 200, 225, 250, 275, 300, 325, 350 (g / t) or a numerical range formed by any two of them, and the dosage of the inhibitor in the second second concentration includes but is not limited to any one of 50, 60, 80, 100, 120, 125, 140, 150 (g / t) or a numerical range formed by any two of them.

[0035] As a preferred embodiment, in step (2), the dosage of the reagent for the second scavenging includes: based on the mass of the slurry, the dosage of the collector in the first second scavenging is 50-100 g / t, the dosage of the collector in the second second scavenging is 80-120 g / t, and the dosage of the collector in the third second scavenging is 30-50 g / t; in some optional embodiments, the dosage of the collector in the first second scavenging includes but is not limited to any one of 50, 60, 70, 80, 90, 100 (g / t) or a numerical range consisting of any two of them, the dosage of the collector in the second second scavenging includes but is not limited to any one of 80, 90, 100, 110, 120 (g / t) or a numerical range consisting of any two of them, and the dosage of the collector in the third second scavenging includes but is not limited to any one of 30, 35, 40, 45, 50 (g / t) or a numerical range consisting of any two of them.

[0036] It can be understood that, in some preferred embodiments, in step (2), only the inhibitor is added during the selection process, and only the collector is added during the scanning process.

[0037] The mineral sources of the following embodiments of the present invention are all low-grade copper mines in Jiangxi Province, and the specific mineral composition includes: chalcopyrite, pyrite, molybdenite, quartz, mica, etc. After testing, in the mineral raw materials: the copper grade is 0.3%, the molybdenum grade is 0.01%, and the sulfur grade is 1.5%.

[0038] Example 1

[0039] The agents used in this embodiment are: inhibitor (guar gum, locust bean gum and fenugreek gum, mass ratio is 4:1:4), collector (ethylthiocarbamic acid-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea, mass ratio is 2:1:2), and foaming agent (pine oil).

[0040] This embodiment performs flotation separation according to the following steps:

[0041] (S1) Grinding and slurry preparation:

[0042] Grind the raw ore to -0.074mm, accounting for 65%, and add water to adjust the pulp concentration to 35%.

[0043] (S2) Copper-sulfur mixed flotation:

[0044] First, the pH value of the ore pulp is adjusted to 8 with hydrochloric acid / quicklime, and based on the mass of the ore pulp, 2000g / t of inhibitor, 200g / t of collector and 50g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing.

[0045] The roughing tailings were scavenged three times. Based on the mass of the slurry, the collector used in the first scavenging was 100 g / t, and the collector used in the second scavenging was 30 g / t. The scavenged concentrates in this step were all discarded and not recycled.

[0046] The rougher concentrate was subjected to two concentration operations. Based on the mass of the slurry, the inhibitor was 500g / t in the first concentration and 150g / t in the second concentration. The tailings from this step were all discarded and not refluxed. The concentrate after the second concentration was used as a copper-molybdenum-sulfur mixed flotation concentrate for the next step of separation flotation.

[0047] (S3) Copper-sulfur separation flotation:

[0048] First, the pH value of the ore pulp is adjusted to 9 with hydrochloric acid / quicklime. Based on the mass of the ore pulp, 2500 g / t of inhibitor, 250 g / t of collector and 15 g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing.

[0049] The roughing tailings were scavenged three times. Based on the mass of the slurry, the collector used in the first scavenging was 100 g / t, the collector used in the second scavenging was 120 g / t, and the collector used in the third scavenging was 50 g / t. The scavenged concentrates in this step were all abandoned and not refluxed; the tailings after the third scavenging were used as sulfur-containing tailings.

[0050] The rough concentrate was subjected to two concentration operations. Based on the mass of the slurry, the inhibitor was 350g / t in the first concentration and 150g / t in the second concentration. The tailings from this step were all discarded and not recycled; the concentrate after the second concentration was used as copper-molybdenum concentrate.

[0051] Example 2

[0052] It is basically the same as Example 1, except for the flotation reagent:

[0053] Inhibitors: guar gum, locust bean gum, and fenugreek gum, in a mass ratio of 3:1:3;

[0054] Collector: ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea, with a mass ratio of 7:5:9.

[0055] Example 3

[0056] It is basically the same as Example 1, except for the flotation reagent:

[0057] Inhibitors: guar gum, locust bean gum, and fenugreek gum, mass ratio 2:1:2;

[0058] Collector: ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea, with a mass ratio of 5:3:7.

[0059] Example 4

[0060] This embodiment performs flotation separation according to the following steps:

[0061] (S1) Grinding and slurry preparation:

[0062] Grind the raw ore to -0.074mm, accounting for 65%, and add water to adjust the pulp concentration to 45%.

[0063] (S2) Copper-sulfur mixed flotation:

[0064] First, the pH value of the slurry is adjusted to 8 with hydrochloric acid / quicklime, and based on the mass of the slurry, 1000 g / t of inhibitor, 50 g / t of collector and 20 g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing.

[0065] The roughing tailings were scavenged three times. Based on the mass of the slurry, the collector used in the first scavenging was 50 g / t, and the collector used in the second scavenging was 10 g / t. The scavenged concentrates in this step were all discarded and not recycled.

[0066] The rougher concentrate was subjected to two concentration operations. Based on the mass of the slurry, the inhibitor was 200g / t in the first concentration and 50g / t in the second concentration. The tailings from this step were all discarded and not refluxed; the concentrate after the second concentration was used as copper-molybdenum-sulfur mixed flotation concentrate for the next step of separation flotation.

[0067] (S3) Copper-sulfur separation flotation:

[0068] First, the pH value of the slurry is adjusted to 8.5 with hydrochloric acid / quicklime, and based on the mass of the slurry, 1200 g / t of inhibitor, 50 g / t of collector and 10 g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing.

[0069] The roughing tailings were scavenged three times. Based on the mass of the slurry, the collector was 50 g / t in the first scavenging, 80 g / t in the second scavenging, and 30 g / t in the third scavenging. The scavenged concentrates in this step were all abandoned and not refluxed; the tailings after the third scavenging were used as sulfur-containing tailings.

[0070] The rough concentrate is subjected to two concentration operations. Based on the mass of the slurry, the inhibitor is 100g / t in the first concentration and 50g / t in the second concentration. The tailings from this step are all discarded and not recycled; the concentrate after the second concentration is used as copper-molybdenum concentrate.

[0071] Example 5

[0072] This embodiment performs flotation separation according to the following steps:

[0073] (S1) Grinding and slurry preparation:

[0074] Grind the raw ore to -0.074mm, accounting for 65%, and add water to adjust the pulp concentration to 35%.

[0075] (S2) Copper-sulfur mixed flotation:

[0076] First, the pH value of the slurry is adjusted to 7 with hydrochloric acid / quicklime, and based on the mass of the slurry, 1500g / t of inhibitor, 125g / t of collector and 35g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing.

[0077] The roughing tailings were scavenged three times. Based on the mass of the slurry, the collector used in the first scavenging was 75 g / t, and the collector used in the second scavenging was 20 g / t. The scavenged concentrates in this step were all discarded and not recycled.

[0078] The rougher concentrate was subjected to two concentration operations. Based on the mass of the slurry, the inhibitor was 350 g / t in the first concentration and 100 g / t in the second concentration. The tailings from this step were all discarded and not refluxed. The concentrate after the second concentration was used as a copper-molybdenum-sulfur mixed flotation concentrate for the next step of separation flotation.

[0079] (S3) Copper-sulfur separation flotation:

[0080] First, the pH value of the slurry is adjusted to 8.5 with hydrochloric acid / quicklime, and based on the mass of the slurry, 1800 g / t of inhibitor, 150 g / t of collector and 12 g / t of frother are added to perform a roughing operation to obtain a roughing concentrate and a roughing tailing.

[0081] The roughing tailings were scavenged three times. Based on the mass of the slurry, the collector used in the first scavenging was 75g / t, the collector used in the second scavenging was 100g / t, and the collector used in the third scavenging was 40g / t. The scavenged concentrates in this step were all abandoned and not refluxed; the tailings after the third scavenging were used as sulfur-containing tailings.

[0082] The rough concentrate was subjected to two concentration operations. Based on the mass of the slurry, the inhibitor was 225 g / t in the first concentration and 100 g / t in the second concentration. The tailings from this step were all discarded and not recycled; the concentrate after the second concentration was used as copper-molybdenum concentrate.

[0083] Example 6

[0084] It is basically the same as Example 1, except for the flotation reagent:

[0085] Inhibitors: guar gum and fenugreek gum, mass ratio 1:1;

[0086] Collector: ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate, mass ratio is 7:5.

[0087] Example 7

[0088] It is basically the same as Example 1, except for the flotation reagent:

[0089] Inhibitors: locust bean gum and fenugreek gum, mass ratio 1:4;

[0090] Collector: diethyl phthalate and guanylthiourea, mass ratio is 5:9.

[0091] Example 8

[0092] It is basically the same as Example 1, except for the flotation reagent:

[0093] Inhibitor: guar gum;

[0094] Collector: ethylthiocarbamate-O-(1-methylethyl) ester.

[0095] Comparative Example 1

[0096] It is basically the same as Example 1, except for the flotation reagent:

[0097] The inhibitors (guar gum, locust bean gum and fenugreek gum) were replaced with lime.

[0098] Comparative Example 2

[0099] It is basically the same as Example 1, except for the flotation reagent:

[0100] The collectors (ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea) were replaced with sodium butyl xanthate.

[0101] Table 1 below provides information on the grade and recovery rate of the copper-molybdenum concentrate and sulfur-containing tailings of each embodiment and comparative example.

[0102] Table 1

[0103]

[0104]

[0105] Although the present invention has been illustrated and described with specific embodiments, it should be appreciated that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Those skilled in the art should understand that the technical solutions described in the above embodiments may be modified, or some or all of the technical features thereof may be replaced by equivalents without departing from the spirit and scope of the present invention. However, these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. Therefore, this means that all such replacements and modifications within the scope of the present invention are included in the appended claims.

Claims

1. A flotation reagent for copper-sulfur minerals, characterized in that: The flotation reagents include depressants and collectors; wherein the inhibitor comprises at least one of guar gum, locust bean gum or fenugreek gum; The collector includes at least one of ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate or guanylthiourea.

2. The flotation reagent for copper-sulfur minerals according to claim 1, characterized in that: The inhibitor is a combination of guar gum, locust bean gum and fenugreek gum; The mass ratio of the guar gum, the locust bean gum and the fenugreek gum is (2-6):(1-2):(2-6).

3. The flotation reagent for copper-sulfur minerals according to claim 1, characterized in that: The collector is a combination of ethylthiocarbamate-O-(1-methylethyl) ester, diethyl phthalate and guanylthiourea; The mass ratio of the ethylthiocarbamate-O-(1-methylethyl) ester, the diethyl phthalate and the guanylthiourea is (4-7):(1-5):(4-9).

4. A flotation separation method for copper-molybdenum-sulfur metal ore, characterized in that: The flotation separation method adopts the flotation agent for copper-sulfur minerals as described in any one of claims 1 to 3.

5. The flotation separation method of copper-molybdenum-sulfur metal ore according to claim 4, characterized in that: The flotation separation method comprises the following steps: (1) Copper-sulfur mixed flotation: The slurry of the copper-molybdenum-sulfur metal ore is subjected to one roughing separation, three scavenging separations and two concentrating separations to obtain a copper-molybdenum-sulfur mixed flotation concentrate and tailings; (2) Copper-sulfur separation flotation: The slurry of the copper-molybdenum-sulfur mixed flotation concentrate is subjected to one second roughing selection, three second scavenging selections and two second concentrating selections to obtain copper-molybdenum concentrate and sulfur-containing tailings.

6. The flotation separation method of copper-molybdenum-sulfur metal ore according to claim 4, characterized in that: The flotation reagent of the flotation separation method also includes a frother; The foaming agent includes pine oil.

7. The flotation separation method of copper-molybdenum-sulfur metal ore according to claim 5, characterized in that: In step (1), the concentration of the copper-molybdenum-sulfur metal ore slurry is 30% to 40%, and the pH of the slurry is adjusted to 6 to 8.

8. The flotation separation method of copper-molybdenum-sulfur metal ore according to claim 5, characterized in that: In step (1), the amount of flotation reagent used, based on the mass of the slurry, includes at least one of the following (a) to (c): (a) In the rough selection, 1000-2000 g / t of inhibitor, 50-200 g / t of collector and 20-50 g / t of frother; (b) the amount of the collector used in the first sweep is 50 to 100 g / t, and the amount of the collector used in the second sweep is 10 to 30 g / t; (c) The amount of the inhibitor used in the first concentration is 200-500 g / t, and the amount of the inhibitor used in the second concentration is 50-150 g / t.

9. The flotation separation method of copper-molybdenum-sulfur metal ore according to claim 5, characterized in that: In step (2), the concentration of the slurry of the copper-molybdenum-sulfur mixed flotation concentrate is 20% to 30%, and the pH of the slurry is adjusted to 8 to 9.

10. The flotation separation method of copper-molybdenum-sulfur metal ore according to claim 5, characterized in that: In step (2), the amount of flotation reagent used, based on the mass of the slurry, includes at least one of the following (A) to (C): (A) In the second rough selection, 1200-2500 g / t of inhibitor, 50-250 g / t of collector and 10-15 g / t of frother; (B) the amount of the inhibitor used in the first step of the second concentration is 100 to 350 g / t, and the amount of the inhibitor used in the second step of the second concentration is 50 to 150 g / t; (C) The amount of collector used in the first second sweep is 50-100 g / t, the amount of collector used in the second sweep is 80-120 g / t, and the amount of collector used in the third second sweep is 30-50 g / t.

Citation Information

Patent Citations

  • Sulfide flotation collector and preparation method

    CN101698160A

  • Combined collector for floatation of porphyry copper-molybdenum mine and floatation method thereof

    CN101844107A

  • Beneficiation method for low-grade mixed copper ore containing molybdenum

    CN105435953A

  • Inhibitor for copper lead sulphide minerals and method for conducting flotation separation with inhibitor

    CN107350087A

  • Flotation method for talc-containing molybdenum-zinc ore

    CN112403685A