Method and apparatus for producing surface structure

By applying liquid B to the resin and removing polymerized liquid B, the structural alignment and control problems in digital printing are solved, and the rapid, easy and low-cost embossing effect on the surface of different materials is achieved, suitable for versatile and microstructures. Application, providing high accuracy and tolerance.

CN118976679APending Publication Date: 2024-11-19乔治马可
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411048907.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2019-05-28
Filing Date
2019-08-21
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art is difficult to achieve aligned embossed structures on different material surfaces quickly, easily and inexpensively, especially in digital printing, structural control is limited and application to other types of varnishes besides light crosslinked varnishes.

Method used

Liquid B is applied by digital printing when the resin has not yet cured or partially cured, and resin A and liquid B are polymerized at different times, and then the polymerized liquid B is removed, thereby creating a three-dimensional structure, using materials of different hardness for mechanical removal, maintaining more Tough material.

Benefits of technology

Achieves efficient reproducing aligned structure on the substrate, with flexibility and high precision, suitable for versatile and microstructure applications, providing the desired tolerance and hardness characteristics for protecting surfaces such as floors and furniture .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976679A_ABST
    Figure CN118976679A_ABST
Patent Text Reader

Abstract

The invention relates to a novel method and apparatus for producing a surface structure, comprising the following steps: A) applying a resin A to a surface of a material; b) applying a liquid B to at least a portion of the resin A when the resin A is in a liquid state or a portion thereof is cured; c) further polymerizing the resin A and the liquid B, respectively; and D) removing the polymerized liquid B.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application with an application date of August 21, 2019, application number 201980055028.6, and invention name “Method and device for generating surface structure”. Technical Field

[0002] The invention relates to a method and a device for producing a surface structure.

[0003] In particular, the present invention relates to a method for producing three-dimensional structures on a substrate by digital printing.

[0004] The present invention is part of the technical field of materials and methods for producing three-dimensionality and embossing on the surface of manufactured articles, substrates, supports made of different types of materials, such as panels for producing floors, coverings, furnishings and more generally for architectural and design surfaces. The technical object of the present invention can further be used to reproduce microstructures that can be used in the biological, optical and electronic fields.

[0005] The present invention exploits a combination of the properties of conventional technology that provides high mechanical, chemical-physical performance and low cost, and the versatility of digital technology that allows full customizability and high precision. Background Art

[0006] Digital printing, and especially inkjet printing, is increasingly showing itself in the industrial sector, replacing traditional methods based on analog printing. The advantages of digital printing are obvious and include high flexibility, the possibility of printing small batches and reducing the waste of consumables.

[0007] In particular, the reproduction of wood on various materials is a typical application of digital printing in the production of flooring, furniture panels, skirting boards, profiles and generally in the fields of design and architecture.

[0008] Typically, the material may consist of wood and derivatives (MDF / HDF / chipboard / plywood), plastic (PVC / polyolefins), metal, onto which the image is printed and then usually protected with a varnish to increase its resistance to abrasion and scratches.

[0009] In particular, in the case of flooring and furniture panels, the finish after printing is provided using a melamine resin layer (laminate) or a varnish applied using common techniques (roller coating / spray coating / curtain coating / die coating). The varnish can be a photo-crosslinked epoxy resin, polyurethane, hot melt with various properties and can contain water and / or solvents to control its viscosity.

[0010] When reproducing natural materials such as wood and stone, in addition to the image, its surface structure must also be reproduced, resulting in a material that is more similar to the original material and feels better to the touch.

[0011] Embossing is usually carried out on the surface layer and can be obtained by various methods, traditionally by pressing with a die, roller or belt to reproduce the structure to be printed thereon. The method can be carried out by pressing on a resin that is not completely hardened, a thermoplastic material, a photo-crosslinking resin and simultaneously irradiating and photopolymerizing it.

[0012] Always with the aim of faithfully reproducing the natural material, a desired feature is to align the embossed structures with the printed image, i.e. to obtain a match between the depressions / reliefs and the printed image. With conventional processes, embossing in alignment (EIR) is not easy to achieve due to the necessary precision and due to the need to have multiple moulds corresponding to the various structures to be printed with the respective image.

[0013] Even in the case of digital printing to easily produce different images, a method to obtain the surface structure in a simple and effective manner would be suitable.

[0014] Indeed, modern scanners such as the METISDRS2000 for acquiring images of materials also allow simultaneous acquisition of surface structures which can advantageously be used to align the embossing.

[0015] Considering the widespread use of embossing, it should be simple and low-cost.

[0016] Therefore, it is currently desirable to find a new method for embossing the surface of an object, which method can be applied quickly, easily and in alignment on surfaces of different materials at low cost.

[0017] In the past, different techniques have been proposed for forming surface structures on photo-crosslinked liquid formulations by using photo-crosslinked formulations applied by inkjet technology:

[0018] Patent EP 2 555 878 B1 describes a method for producing a periodic structure.

[0019] Patent US20100092688A1 describes a method for forming structures on organic films by locally applying an immiscible liquid.

[0020] Patent EP 3 109 056 A1 provides for the use of UV preparations applied by inkjet printing on non-polymeric UV varnishes for producing three-dimensional structures that simulate wood grain.

[0021] Although the above techniques provide three-dimensional structures through digital technology, they are subject to limitations related to the structural control that can be obtained and are plagued by the fact that the varnish needs to be properly developed to maximize the 3D effect. In particular, they are limited when the varnish to be embossed contains anti-abrasion fillers such as aluminum oxide (corundum). In addition, although the above techniques can be used with photocrosslinking varnishes, they can hardly be applied to other types of varnishes. Summary of the invention

[0022] According to one aspect of the present invention, applicants have discovered a method for producing three-dimensional structures on a substrate by digital printing techniques.

[0023] The method of the present invention advantageously applies liquid B to resin A and / or ink and / or varnish containing it by digital printing when resin A has not yet been cured or is partially cured. Then, resin A and liquid B are also cured / polymerized at different times. In a subsequent step, the polymerized liquid B is removed from the polymerized resin A, thereby generating a three-dimensional structure.

[0024] The method of the present invention takes advantage of the different hardnesses of the applied materials, thereby subsequently removing the more brittle material while leaving the tougher material intact.

[0025] According to a first aspect, the invention thus relates to a method for generating a three-dimensional surface, said method comprising the steps of:

[0026] A) applying resin A to the surface of the material;

[0027] B) applying liquid B to at least a portion of the resin A when the resin A is liquid or partially cured;

[0028] C) also polymerizing resin A and liquid B separately;

[0029] D) removing the polymerized liquid B.

[0030] Embodiments of the invention as defined above or as defined in claim 1 will now be described.

[0031] The method of the present invention faithfully reproduces the aligned structure in an efficient and economical manner.

[0032] Unlike the background art which provides embossing in register (EIR) of the erosion of a roller or die corresponding to the underlying printed image, the method of the present invention uses digital printing technology to emboss the substrate.The method of the present invention is flexible and can manage a single file.

[0033] Furthermore, the embossed structures obtained with the process object of the invention have the desired properties of resistance and hardness, since the embossing is carried out on the same protective varnish as is used to protect the substrate, as is the case with floor panels or furniture or furnishings and accessories.

[0034] The versatility and resolution obtainable by the method of the invention allow its use also in applications using microstructures typical of the field of microfluidics.

[0035] Four embodiment variants of the method according to the invention can be provided which are within the more general definition and which alternatively provide only one of the following steps:

[0036] - Use of a Liquid B composition that produces a filtration effect that inhibits polymerization;

[0037] - using monomers with a low Tg, in particular a Tg below 20°C, and at least a liquid B whose Tg is such that the Tg of the mixture of resin A combined with liquid B is lower than the Tg of the polymerized resin A;

[0038] - As the liquid B, a liquid partially miscible or immiscible with the resin such as water and PEG acrylate is used;

[0039] - Using water as liquid B to produce a structure with pores in the area where the water is applied, whereby said area is mechanically weakened relative to the area to which the liquid B is not applied. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Two schematic renditions of steps A) to D) of the process according to the invention are depicted.

[0041] Figure 2 An embodiment of a device for the purpose of reproducing the method of the invention is depicted.

[0042] Figure 3 An enlarged example and a perspective view of a "pierced" structure are shown, which is obtained by projecting water droplets by means of an inkjet application technique onto a not yet polymerized or partially polymerized resin A. On the right side a measurement table of the area containing the holes is shown, while on the left side a diagram of the size of the area of ​​the holes is shown.

[0043] Figure 4 Shows Figure 3 Example after the step of removing material of the area subjected to the projection of embossing liquid particles. DETAILED DESCRIPTION

[0044] According to one aspect, the present invention relates to a method for producing a three-dimensional coating embossed on a substrate, comprising the steps of:

[0045] A) applying resin A or a varnish or ink containing it to the surface of a substrate ( Figure 2-1 ), thereby forming a coating ( Figure 2-2 );

[0046] B) applying liquid B to at least a portion of resin A ( Figure 2-3 );

[0047] C) also polymerize / cure resin A and liquid B respectively ( Figure 2-4 and Figure 2 -5);

[0048] D) Removal of polymerized / solidified Liquid B ( Figure 2 -6).

[0049] In the following paragraphs, the terms polymerisation and / or curing will not be used explicitly to identify that a solid product will be obtained at the end of the process.

[0050] The method of the present invention takes advantage of the different hardnesses of the applied materials, thereby subsequently removing the more brittle material while leaving the tougher material intact.

[0051] Typically, resin A can be of various chemistries such as, but not limited to, polyurethane, epoxy, photo-crosslinked acrylate acrylic resins.

[0052] Preferably, Resin A is composed of 100% solids to maximize the layer that can be embossed and to hinder the effect of Liquid B due to evaporation of any solvent and / or water. On the other hand, Resin A may contain water and / or solvents, typically between 5% and 30%, as required by the application.

[0053] In a preferred embodiment of the invention, resin A has photocrosslinking properties, as described, for example, in the text “Radiation Curing: Science and Technology” (Pappas).

[0054] Photo-crosslinking resins have in common the fact that they polymerize and harden due to energy irradiated by ultraviolet devices and / or by EB (electron beam), and are divided into two types according to the crosslinking mechanism: 1) Free radical resins, generally derived from vinyl monomers and acrylate resins, which are divided into different subcategories: epoxy resin-acrylate, urethane-acrylate, polyester-acrylate, polyether-acrylate, amino-acrylate, silicon-acrylate, polyisoprene-acrylate, polybutadiene-acrylate and acrylate monomers. Among the vinyl monomers, N-vinyl caprolactam (NVC), acryloyl morpholine (ACMO), diethylene glycol divinyl ether (DVE-2), triethylene glycol divinyl ether (DVE-3) and mixtures thereof can be cited.

[0055] The term acrylate refers to both acrylate and methacrylate resins.

[0056] 2) Cationic resins such as epoxy resins, polyols, and monomers such as oxetanes and vinyl ethers.

[0057] Applicants have also unexpectedly discovered that by varying the surface tension of Liquid B and Resin A, Liquid B may penetrate more or less into Resin A and thereby alter the three-dimensional structure obtained after polymerized Liquid B is removed.

[0058] Generally, the more significant the surface tension difference between Liquid B and Resin A is, the higher the corresponding embossing effect will be.

[0059] The surface tension of Liquid B and Resin A can be adjusted by selecting the chemical properties of their base materials as well as by adding specific additives. For example, resins containing polar groups such as hydroxyl, amine and aromatic groups will have higher surface tension than resins containing hydrocarbon-type linear structures.

[0060] For example, regarding the choice of raw materials, the surface tensions of the more common photocrosslinking monomers are shown in the table below:

[0061]

[0062]

[0063] About the use of additives:

[0064] - Additives that reduce surface tension: silicones, polyether silicones, acrylate silicones, acrylate polyether silicones, fluorinated surfactants, alkoxylated alcohols. Such compounds are readily available on the market, for example commercialized by BYK (BYK-UV) and EVONIK (Tego Rad, Tego Wet, Tego Glide).

[0065] - Additives that increase the surface tension: amines, polyether macromonomer-modified polyacrylates, silicon and polyether macromonomer-modified polyacrylates. Such compounds are readily available on the market, for example commercially by BYK (BYK 3560, BYK 3565).

[0066] Typically, the additive is added in an amount between 0.01 and 20%, or better still between 0.01 and 10%, or better still between 0.01 and 2%.

[0067] In a preferred embodiment of the present invention, resin A may be in the form of a hot melt such as Henkel-Technomelt.

[0068] In another embodiment of the present invention, resin A may be composed of non-photocrosslinkable materials such as polyurethane, epoxy resin, PLASTISTOL, hot melt (eg Kleiberit-Hotcoating) resin.

[0069] In non-photocrosslinking systems, PLASTISOL has attracted great interest as a mixture of PVC, plasticizers, additives and possible solvents. PLASTISOL is often used as a wear layer on PVC floors such as LVT (Luxury Vinyl Tile). PLASTISOL is applied as a liquid at about 150-500 g / m2 and then cured by heat treatment at 180-200°C for 2-4 minutes.

[0070] In a preferred embodiment of the present invention, resin A: is generally used to protect floors and furniture surfaces from wear, scratches and abrasion; contains one or more photo-crosslinking resins, photoinitiators; and may contain loads, such as aluminum oxide (corundum) to improve abrasion resistance, talc to improve its rheology, silicon dioxide to reduce its brilliance, calcium carbonate as a filler load, pigments to impart color, additives such as leveling agents, wetting agents, slip agents, rheology modifiers. The preparation of the photo-crosslinking resin may contain a rheology modifier, such as a thixotropic agent that has the function of better maintaining the embossing shape in terms of both depth and clarity.

[0071] In a preferred embodiment, Liquid B is immiscible or partially miscible with Resin A and, once polymerized, is mechanically removed from Resin A. Liquid B thus has the sole function of creating three-dimensionality without changing the chemical-physical properties of Resin A. Polymerized Liquid B is more brittle than polymerized Resin A and thus can be mechanically removed from Resin A without damaging Resin A. Thus, if Resin A is to have predominantly non-polar properties, Liquid B will preferably be polar and vice versa.

[0072] In a preferred embodiment of the invention, the majority of Liquid B consists of a photocrosslinkable resin. To be applied by inkjet, Liquid B must have a viscosity of 10-15 cps at the jetting temperature (40-50° C.). Therefore, similar to other formulations (varnishes and inks) that can be photocrosslinked by inkjet printing, Liquid B will be mainly formed by (meth)acrylates and / or vinyl monomers. On the other hand, in order to control the rheology and achieve the desired degree of hardness, Liquid B may contain acrylate oligomers in addition to the monomers.

[0073] In order to obtain a brittle and easily removable formulation, ingredients characterized by a low Tg can be used, such as isodecyl acrylate of various molecular weights (200, 300, 400, 600 Daltons), 2-(2-ethoxyethoxy)ethyl acrylate, octyldecyl acrylate, tridecyl acrylate, lauryl acrylate, polyethylene glycol diacrylate,

[0074] In another preferred embodiment of the present invention, Liquid B has a sufficiently high surface tension relative to Resin A to facilitate penetration into Resin A while maintaining the shape and thereby produce a complex structure. On the contrary, if the surface tension of Liquid B is too low relative to the surface tension of Resin A, clarity will be lost, resulting in the fact that Liquid B will wet the surface of Resin A.

[0075] In a preferred embodiment of the present invention, Liquid B is able to penetrate and mix with Resin A quickly and efficiently.

[0076] In another still preferred embodiment of the present invention, Liquid B is able to penetrate quickly and is not mixed or partially mixed with Resin A.

[0077] In a preferred embodiment of the present invention, liquid B contains a substance suitable for inhibiting the polymerization of resin A, so that after polymerization, the area printed with liquid B will be more brittle than resin A. For example, if resin A is composed of a photo-crosslinking resin, liquid B may contain an inhibitor, such as: UV absorbers such as 2-hydroxyphenyl-benzophenone (BP), 2-(2-hydroxyphenyl)-benzotriazole (BTZ) and 2-hydroxyphenyl-s-triazine (HPT); hindered amines (HALS) such as 2,2,6,6-tetramethylpiperidine (TMP); antioxidants (AO) such as hindered phenols, secondary sulfides, phosphites; stabilizers (in-can stabilizers) such as quinone methides, free radical scavengers.

[0078] In another embodiment of the present invention, once polymerized Liquid B has a lower Tg (Tg is defined as the glass transition temperature) than Resin A, the areas printed with Liquid B will therefore be easier to remove than polymerized Resin A.

[0079] In some embodiments, Liquid B contains additives for modifying properties such as rheology and / or printability and / or color, and may include photoinitiators, leveling agents, oils, light stabilizers, antioxidants, biocides, pigments, rheology modifiers, wetting agents, defoamers, and mixtures thereof.

[0080] In a preferred embodiment of the present invention, Liquid B has a higher surface tension than Resin A.

[0081] Similar to Resin A, the surface tension of Liquid B can be adjusted by selecting raw materials and using additives, the same as described above to modify Resin A.

[0082] Besides changing the surface tension to give a more or less pronounced penetration effect, the addition of a surface tension modifier also helps to improve the printability of Liquid B, especially when using an inkjet printer.

[0083] The depth of Liquid B in Resin A can be controlled in different ways:

[0084] - by applying more Liquid B;

[0085] - by the passage of more or less time between the application of Liquid B and the subsequent polymerization of Resin A and Liquid B;

[0086] - By using a waveform to vary the droplet speed of Liquid B, where faster drops will be able to sink deeper into Resin A.

[0087] Preferably, Liquid B has low viscosity and high solvency for Resin A. For example, the following monomers are listed according to the degree of solvency: EOEOEA>THFA>HDDA>DPGDA.

[0088] Substrates which can be used in the process according to the invention can be materials of different nature, for example: wood and derivative products such as MDF, HDF, particleboard, multilayer wood; cellulose-based materials such as paper or cardboard; metals; plastic materials (PVC, polyester, polyolefins); stone; glass; ceramics and composites thereof.

[0089] The substrate is selected according to the application of the method according to the invention (for example for the coating of furniture, floors, blinds and frames, profiles).

[0090] The substrate may have a variable thickness depending on the application, for example in the case of decorative panels for furniture it is generally between 8 and 20 mm, while for the production of flooring the thickness is between 2 and 6 mm. The process of the invention can also be used to produce structures on films, generally plastic or paper films, which are generally used for the coating and decoration of furniture and other furnishing surfaces.

[0091] The resin A covering the substrate has a variable thickness. For example, when the density of the resin A is 1 g / ml, the thickness of the resin A can be in the range of 1-500 μ, which is equivalent to 1-500 g / m 2 Usually, to protect high traffic floors, use 80-120g / m 2 Obviously, there is nothing to prevent a greater number of applications simply to obtain deeper structures.

[0092] In one embodiment of the present invention, the thickness of resin A in the non-embossed portion is from 1 to 200μ, from 2 to 100μ, from 3 to 50μ, and the thickness in the embossed area is in the range of from 0.05 to 100μ, from 0.5 to 50μ, from 1 to 25μ.

[0093] The method of the present invention and the apparatus for implementing it will become more apparent from the following description, wherein reference is made to the accompanying drawings. Figure 1 , 2 and 3 describe the implementation scheme.

[0094] According to some embodiments, using digital technology such as Figure 2 Resin A or a varnish or ink to be embossed containing it can be applied to the substrate by using inkjet printing or by using conventional techniques such as roller coating / spray coating / curtain coating / die coating / slot die coating as shown in point 3 in FIG.

[0095] In one embodiment of the invention, resin A is a photocrosslinkable printing varnish and / or a photocrosslinkable printing ink applied by digital printing.

[0096] In some embodiments of the invention, application of Liquid B occurs over uncured resin A of the underlying printed image or over a varnish or ink containing it.

[0097] Typically, photopolymerization by UV irradiation can be performed using one or more Hg lamps and / or LED lamps, e.g. Figure 2 As shown in the midpoints 4 and 5.

[0098] According to one embodiment, the lamps are mounted on a moving system so that they are more or less close to the application system of Liquid B in order to better control its action and thus adjust its effect. For example, if a strong matte effect is to be obtained, prepolymerization / polymerization must be carried out immediately after the inkjet application, e.g. Figure 2 As shown in point 4.

[0099] At the end of the process objective of the present invention, there will be regions consisting of polymerized resin A and regions consisting of polymerized liquid B. Because of these regions of different hardness / toughness, the softer / brittle material can be selectively mechanically removed while the harder / tougher material remains ( Figure 2 -6).

[0100] In another form of the invention, Liquid B is applied to a wear layer (resin A) to which a finishing is subsequently applied, and the polymerized Liquid B is removed mechanically therefrom.

[0101] What is described above is very similar to what happens in certain natural materials such as wood, where during the roughening / brushing operation the softer parts of the wood are removed, leaving the harder parts intact.

[0102] The mechanical removal of the polymerized Liquid B can thus be carried out with the same machine used for roughening / brushing the wood. Such machines use brushes and / or pads made of more or less aggressive materials (steel, brass, nylon fibers, polyester fibers), depending on the hardness of the material to be removed and the desired degree of finish. Such equipment is produced, for example, by CEFLA (e.g. RSP4) and QUICKWOOD (e.g. CDI / 300+LEV).

[0103] The removal of polymerized Liquid B can also be performed by high-pressure air jets or high-pressure water jets.

[0104] In another embodiment of the invention, polymerized Liquid B is removed by using an adhesive roller or tape that, once applied to the surface of Resin A, removes polymerized Liquid B still attached to the adhesive itself while being removed. The adhesive roller or tape can then be cleaned from the polymerized Liquid B and reused.

[0105] In another embodiment of the present invention, the polymerized Liquid B can be removed by using a suitable solvent.

[0106] In a preferred embodiment of the present invention, after removing the polymerized liquid B, a finishing varnish is applied to the surface of the resin A to obtain the desired appearance in terms of brightness, feel and micro-scratch resistance ( Figure 2 -7).

[0107] In another embodiment of the invention, the application of Liquid B is performed in two separate steps and this allows, for example, to obtain a combined effect by using Liquids B with different properties, such as surface tension.

[0108] Typically, the method of the present invention aims to apply Liquid B by means of an inkjet print head.

[0109] Inkjet printing can be in either: multi-pass / scanning mode, where the image is generated by multiple passes through the print head while the material to be printed moves forward; or single-pass mode, where the material to be printed can only pass once under the print head installed at the same material width. Single-pass printing is used for long-distance printing (>1000m 2 / h), and for short and medium distances (10-600m 2 / h) multi-channel printing is definitely the most common printing method.

[0110] Typically, inkjet printing uses a print head to generate and eject droplets, which then form the image to be printed. For example, details of this type of printing can be found in the book "Fundamentals of inkjet printing: the science of inkjet and droplets" (Hoath, Stephen).

[0111] Depending on the inkjet print head used, the generated droplets can have different volumes and thus different diameters.

[0112] For example, in the table below the volumes of the droplets and the corresponding diameters are listed.

[0113] Volume (pl) Diameter(μ) VolumeLev.1(pl) VolumeLev.2(pl) VolumeLev.3(pl) 1.5 3 1.5 3 4.5 2.4 5 2.4 4.8 7.2 3 6 3 6 9 6 13 6 12 18 10 21 10 20 30 12 25 12 24 36 30 64 30 60 90 80 170 80 160 240

[0114] Table 1

[0115] In addition to the original drop size, an inherent characteristic of the print head, the print head itself can also produce larger droplets. For example, a print head capable of jetting 4 gray levels can have droplets smaller than 6 pl, while larger droplets are 18 pl.

[0116] Contrary to the digital embossing technologies currently on the market that only use 1-bit printing, the method of the present invention allows the droplets to be ejected in a grayscale mode. This way expands the effects that can be obtained and makes it possible to produce different depths and simultaneously create surface microstructures.

[0117] Typically, the method of the invention is advantageously intended for use in the manufacture of furniture and / or flooring. The preparation and finishing cycle depends on the material to be decorated and the desired properties.

[0118] For example, a typical cycle for decorative SPC (Stone Plastic Composite), a material currently gaining popularity in flooring production, provides the following operations:

[0119]

[0120]

[0121] Table 2

[0122] The method of the present invention can be carried out on both the wear layer and the facing, preferably on the first ( Figure 3 ).

[0123] In order to obtain different aesthetic effects, the wear layer and the facing can have different opacities. In fact, if the wear layer has a higher gloss than the facing, glossy holes will be obtained which will be highlighted.

[0124] Conversely, if the wear layer and the finish have the same gloss level, the holes will be less noticeable but the effect will be more natural.

[0125] In another application of the invention, the method can be used to manufacture molds and transfer films / embossed papers. The molds used to press melamine are usually made of metal sheets, which are then mechanically corroded and / or eroded to produce the desired structure. The method is quite laborious and takes several weeks. The molds are then chrome-plated, an environmentally harmful operation that should be banned in the near future.

[0126] On the other hand, melamine pressing requires high temperature (160-180°C) and pressure (15-70 bar) conditions, properties that cannot usually be adjusted by the chemical-physical properties of the polymerized inkjet formulation. By means of the method of the present invention, it is possible to alternatively select a suitable resin A, capable of withstanding the pressing conditions and producing the opposite of the structure we want to obtain after the pressing process. Similar to the molds used for melamine pressing, the method of the present invention can be used to manufacture molds for pressing ceramics, leather and plastics. In addition to the manufacture of flat molds, the method of the present invention can also be used to manufacture etching rollers, which have the same function as molds, but are mainly used on flexible materials.

[0127] Advantageously, the application of small droplets can be used to generate microgrooves and microwells with dimensions of a few micrometers, which are typical features of microfluidics, for the fabrication of sensors and functional devices.

[0128] Another application of small droplets is to create microstructures that matte the surface of the embossed varnish / resin / ink. With the latter application, simultaneously glossy and matte surfaces with interesting aesthetic effects can be obtained.

[0129] In another embodiment of the invention, resin A may contain a foaming agent to achieve a high embossing volume, but by limiting the weight and / or cost of the embossing layer. Typically, hollow polymer microspheres filled with a gas can be used, which increase in volume at a given temperature, such as EXPANCEL. The expansion stage preferably occurs before the application of Liquid B.

[0130] Besides reproducing natural materials such as wood and stone, the method object of the invention can also be used to produce three-dimensional structures typical of the graphic and / or decorative field.

[0131] Advantageously, the method object of the invention can be used to emboss surfaces printed in a conventional manner (rotogravure / flexographic / lithographic).

[0132] The following examples of embodiments are provided only to illustrate the present invention and should not be construed as limiting the scope of protection defined by the appended claims.

[0133] Example 1

[0134] Liquid B is poorly miscible with Resin A and once polymerized, Liquid B has a low Tg.

[0135] Onto a support made of melamine paper, 75 μ of a photocrosslinking varnish was applied using a hand tool to spread a film of TEKNOS UVILUX 143-001 for veneered floors (resin A).

[0136] Subsequently, on the stationary liquid varnish, Liquid B consisting of the following composition was applied by a single-pass type inkjet printer:

[0137] - Water: 47.5%

[0138] -Diacrylate monomer PEG600DA: 47.5%

[0139] -Photoinitiator, TPO-L 5%

[0140] Then immediately use 395nm and 8W / cm 2 The support was irradiated with a PHOSEON FIRELINE lamp and then with a Hg lamp (DR. ) to complete the polymerization of resin A and liquid B.

[0141] After application, the surface appeared uniform and the areas where Liquid B was printed were visible to the naked eye.

[0142] Although the area printed with Liquid B can be removed using a 2H pencil, the polymerized Resin A cannot be removed. Therefore, three-dimensionality is generated in the area printed with Liquid B.

[0143] Example 2

[0144] Liquid B is miscible with Resin A, and once polymerized, the mixture of Resin A and Liquid B has a low Tg.

[0145] Onto a support made of melamine paper, 75 μ of a photocrosslinking varnish was applied using a hand tool to spread a film of TEKNOS UVILUX 143-001 for veneered floors (resin A).

[0146] Subsequently, on the stationary liquid varnish, Liquid B consisting of the following composition was applied by a single-pass type inkjet printer:

[0147] -Monoacrylate monomer EOEOEA: 100%

[0148] Then immediately use 395nm and 8W / cm 2The support was irradiated with a PHOSEON FIRELINE lamp and then with a Hg lamp (DR. ) to complete the polymerization of resin A and liquid B.

[0149] After application, the surface appeared uniform and the areas where Liquid B was printed were visible to the naked eye.

[0150] Although the area printed with Liquid B can be removed using a 2H pencil, the polymerized Resin A cannot be removed. Therefore, three-dimensionality is generated in the area printed with Liquid B.

[0151] Example 3

[0152] Liquid B contains a UV polymerization inhibitor and is miscible with Resin A.

[0153] Onto a support made of melamine paper, 75 μ of a photocrosslinking varnish was applied using a hand tool to spread a film of TEKNOS UVILUX 143-001 for veneered floors (resin A).

[0154] Subsequently, on the stationary liquid varnish, Liquid B consisting of the following composition was applied by a single-pass type inkjet printer:

[0155] -Diacrylate monomer DPGDA: 90%

[0156] -Tinuvin 123: 10%

[0157] Then immediately use 395nm and 8W / cm 2 The support was irradiated with a PHOSEON FIRELINE lamp and then with a Hg lamp (DR. ) to complete the polymerization of resin A and liquid B.

[0158] After application, the surface appeared uniform and the areas where Liquid B was printed were visible to the naked eye.

[0159] Although the area printed with Liquid B can be removed using a 2H pencil, the polymerized Resin A cannot be removed. Therefore, three-dimensionality is generated in the area printed with Liquid B.

[0160] Example 4

[0161] Liquid B is immiscible with resin A.

[0162] Onto a support made of melamine paper, 75 μ of a photocrosslinking varnish was applied using a hand tool to spread a film of TEKNOS UVILUX 143-001 for veneered floors (resin A).

[0163] Subsequently, on the stationary liquid varnish, Liquid B composed of water was applied by a single-pass type inkjet printer.

[0164] Then immediately use 395nm and 8W / cm 2 The support was irradiated with a PHOSEON FIRELINE lamp and then with a Hg lamp (DR. ) to complete the polymerization of resin A.

[0165] After application, the surface appeared uniform and the areas where Liquid B was printed were visible to the naked eye.

[0166] Although the area printed with Liquid B can be removed using a 2H pencil, the polymerized Resin A cannot be removed. Therefore, three-dimensionality is generated in the area printed with Liquid B.

[0167] Example 5

[0168] The SPC panels have been subjected to the cycles described in Table 2.

[0169] The printer used (BARBERAN-JETMASTER) was equipped with a SEIKO print head, and the printed image was obtained by three-dimensionally scanning a natural Quercus sessile sheet using a scanner (METIS). The image was then uploaded to the printer via dedicated software (RIP).

[0170] The line speed is 18m / min.

[0171] After digital printing, 20 g / m 2 The wear-resistant layer is then gelled.

[0172] Subsequently, a 100 g / m2 wear-resistant layer (resin A) was applied while still in liquid form, and liquid B consisting of the following composition was applied thereto by a single-pass type inkjet printer:

[0173] -Diacrylate monomer DPGDA: 90%

[0174] -Tinuvin 123: 10%

[0175] The panels were then passed through a QUICKWOOD CDI / 300 brushing machine equipped with 3 sets of wire brushes having wires with a diameter of 0.3 mm.

[0176] Subsequently, 10 g / m 2 Clear varnish with matt finish (6 gloss levels).

[0177] The 3D structures are clearly defined and detailed, very similar to the scanned natural materials.

[0178] The structure was then analyzed by laser profilometer analysis (3D Profiler - USA), which provided a structure with a maximum depth of 95 μ.

[0179] Example 6

[0180] 100 g / m2 of a PLASTISOL formulation for LVT floor protection (resin A) was applied to the carrier material (SPC) by roller coating.

[0181] Subsequently, the support was passed under a single-pass inkjet printer, with which a liquid B consisting of the following composition was applied:

[0182] - Water: 47.5%

[0183] -Diacrylate monomer: PEG600DA: 47.5%

[0184] -Photoinitiator, TPO-L 5%

[0185] Subsequently, the panel was irradiated with UV light from a 160 w / cm Hg lamp at medium pressure to polymerize Liquid B.

[0186] The panel was then heated in an oven at 180°C for 3 minutes to polymerize the PLASTISOL.

[0187] The panels were then passed through a QUICKWOOD CDI / 300 brushing machine equipped with 3 sets of wire brushes having wires with a diameter of 0.3 mm.

[0188] Subsequently, 10 g / m 2 Clear varnish with matt finish (6 gloss levels).

[0189] The three-dimensional structure is clearly defined and detailed.

[0190] Example 7

[0191] 300 μ of a varnish (resin A) consisting of the following was applied to a C40 steel plate of 400×400×3 mm by a slot die (OSSILA):

[0192] -CN112C60: 90%

[0193] -OMNICURE 184: 5%

[0194] -OMNICURE TPO: 0.2%

[0195] The plate was then printed using a single-pass inkjet printer, the composition of Liquid B being as follows:

[0196] -Diacrylate monomer DPGDA: 90%

[0197] -Tinuvin 123: 10%

[0198] Subsequently, the plate was passed under a Hg lamp (160 w / cm) at a speed of 12 m / min, and the varnish (resin A) was difficult to touch.

[0199] The grain of the printed wood is clearly visible on the surface.

[0200] The panels were then passed through a QUICKWOOD CDI / 300 brushing machine equipped with 3 sets of wire brushes having wires with a diameter of 0.3 mm.

[0201] The three-dimensional structure is clearly defined and detailed.

[0202] The board with the structure described was used in a compression press, loaded with a 400×400×8 mm MDF panel, on which was placed a kraft paper impregnated with urea-formaldehyde resin, on which was placed a decorative paper impregnated with melamine-formaldehyde resin and on which was placed a melamine laminate. The whole was pressed for 30 seconds at a temperature of 180° C. and a pressure of 20 bar.

[0203] At the end of Example 7

[0204] 75 μ of a photocrosslinking varnish for floor finishing (TEKNOS UVILUX 143-001) was applied to a carrier made of melamine paper using a manual film applicator.

[0205] The panel was then passed under a single-pass inkjet printer, which applied Liquid B consisting of the following composition:

[0206] -Diacrylate monomer, EOEOEA: 95.5%

[0207] -HALS, TINUVIN 123: 5%

[0208] Then immediately use a medium pressure 160w / cm Hg lamp (DR. ) irradiates the carrier.

[0209] After application, the surface appeared uniform and the areas where Liquid B was printed were visible to the naked eye.

[0210] Although the area where the liquid B was printed can be removed using the HB pencil, the polymerized resin A cannot be removed. Therefore, three-dimensionality can be generated in the area where the liquid B was printed.

[0211] Figure 3A perspective view of a portion of a resin A layer to which water has been applied by an inkjet printer is shown in the central region. It is apparent that the central region, designated G, has a microporous or structure consisting of a plurality of small cavities which makes said region G less resistant to mechanical removal than the region to which no water has been applied and designated NG.

[0212] The size distribution of the microcavities or pores is shown in the figure on the left and the measured data are summarized in the table on the right.

[0213] After the polymerization step, the residual material in the embossed areas, ie the areas bombarded by the water droplets produced by the inkjet printing technique, is removed. The embossed areas are weaker and less resistant to removal than the untreated areas.

[0214] Figure 4 Shows Figure 3 1. Example of after the step of removing material from the projection area of ​​the embossed liquid particles. Obviously, the recesses formed have relatively sharp and precise, i.e. slightly jagged, side boundary walls.

Claims

1. A method for producing a three-dimensional surface on a substrate, comprising the following steps: A) applying a radiation curable resin A or a varnish or ink containing the same onto the surface of a substrate to form a coating; B) applying a liquid B capable of inhibiting radiation-curing polymerization to at least a portion of the resin A while the resin A is still liquid or partially cured to form a mixture of the resin A and the liquid B; C) a mixture of polymer resin A and liquid B; D) Mechanical removal of the polymerized mixture of Resin A and Liquid B.

2. The method according to claim 1, wherein the resin A is selected from the group consisting of cationic photocrosslinking resins, free radical photocrosslinking resins, epoxy resins, polyurethane resins, acrylic resins, polyester resins and mixtures thereof.

3. The method according to the preceding claim, wherein the inhibitor is selected from UV absorbers such as 2-hydroxyphenyl-benzophenone (BP), 2-(2-hydroxyphenyl)-benzotriazole (BTZ) and 2-hydroxyphenyl-s-triazine (HPT); hindered amines (HALS) such as 2,2,6,6-tetramethylpiperidine (TMP); antioxidants (AO) such as hindered phenols, secondary sulfides, phosphites; stabilizers (in-can stabilizers) such as quinone methides, free radical scavengers.

4. The method according to the preceding claim, wherein the substrate is a film made of paper and / or a polymer.

5. The method of claim 1, wherein the Liquid B is dispersible, emulsifiable or soluble in water.

6. The method according to claim 1, wherein the liquid B contains at least one substance selected from the group consisting of a surface tension modifier, an acrylic resin, a photo-crosslinking resin, a photoinitiator, a slip agent, a wetting agent, an oil, a light stabilizer, an antioxidant, a defoaming agent, a wetting agent, an antimicrobial agent, a colorant, a pigment, and a mixture thereof. The method according to claim 1 , wherein the surface tension of the liquid B is higher than that of the resin A. The method according to claim 1 , wherein the liquid B comprises a solvent.

9. The method according to claim 1, wherein the polymerized mixture of resin A and liquid B has one or both of the following characteristics: Tg<20°C, or Tg is lower than that of resin A.

10. The method of claim 1, wherein the polymerized mixture of Resin A and Liquid B is mechanically removed by a brush coater.

11. The method according to claim 1, wherein the polymerized mixture of Resin A and Liquid B is removed by compressed air jets and / or high pressure water jets.

12. The method of claim 1, wherein the Liquid B is applied by an inkjet print head.

13. The method of claim 1, wherein the Liquid B is applied in two or more separate steps by using different inkjet printing systems.

14. The method according to claim 1, wherein: After removing the polymerized mixture of Resin A and Liquid B, a coating is applied to the three-dimensional surface to provide further protection or to provide gloss to the three-dimensional surface.

15. A substrate or a finished product obtained by the method according to any one of claims 1 to 14, characterized in that: The substrates or finished products are used to make or coat flooring, furniture and more generally furnishing and architectural surfaces.

16. A substrate or a finished product manufactured according to any one of claims 1 to 14, characterized in that: The substrate or manufactured article is used as a mold or embossed paper for producing a three-dimensional surface.