Coating method of high-performance super-black paint

By adjusting the formula ratio and spraying process of the ultra-black paint, the problems of high environmental requirements and long curing time in ultra-black paint coating have been solved, achieving efficient production and cost reduction.

CN118976688APending Publication Date: 2024-11-19XIAMEN RUNNER IND CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411092745.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-09
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing ultra-black paint coating technology has high requirements for environmental conditions, long curing time, and fails to meet the requirements for diffuse reflectance and functional testing, resulting in increased production costs and reduced efficiency.

Method used

Using a mixture of 3-5 parts super black paint, 0.9-1.1 parts hardener, and 2-4 parts thinner, combined with fully automatic spraying equipment and a curing temperature of 70℃-100℃, the mixture was cured for 20-50 minutes, and then diffuse reflectance and functional tests were conducted.

Benefits of technology

It improves the functionality of ultra-black paint, shortens curing time, reduces production costs, and increases production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976688A_ABST
    Figure CN118976688A_ABST
Patent Text Reader

Abstract

The invention provides a coating method of high-performance super-black paint, and relates to the technical field of coating processes. Comprising the following steps: S1, removing stains on the surface of a to-be-sprayed product; s2, the proportion of the super-black paint is adjusted, 3-5 parts of super-black paint coating, 0.9-1.1 parts of a curing agent and 2-4 parts of banana oil are evenly mixed, and the prepared super-black paint is evenly sprayed to the surface of a product to be sprayed through a spraying device; and S3, curing is conducted for 20 min to 50 min at the temperature ranging from 70 DEG C to 100 DEG C. According to the scheme, the performance of a sprayed product can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of coating technology, and in particular to a coating method of high-performance ultra-black paint. Background Art

[0002] At present, for plastic substrates and metal substrate products coated with other ultra-black paints, there are high requirements for the environmental conditions of ultra-black paint coating, long curing time, diffuse reflectivity that cannot meet the required standards, and functional tests that cannot meet the requirements after coating. This not only increases production costs and reduces production efficiency, but also affects economic benefits and competitiveness among enterprises. Summary of the invention

[0003] The invention discloses a coating method of high-performance ultra-black paint, aiming to improve the above-mentioned problems.

[0004] The present invention adopts the following scheme:

[0005] The present application provides a method for coating a high-performance ultra-black paint, comprising the following steps:

[0006] S1. Remove stains on the surface of the product to be sprayed;

[0007] S2. Adjust the ratio of the ultra-black paint, mix 3-5 parts of the ultra-black paint, 0.9-1.1 parts of the curing agent and 2-4 parts of the thinner evenly, and spray the adjusted ultra-black paint evenly on the surface of the product to be sprayed through a spraying device;

[0008] S3. Curing at 70°C-100°C for 20min-50min.

[0009] Preferably, the ratio of the super black paint is 4 parts of super black paint, 1 part of curing agent and 3 parts of thinner.

[0010] Preferably, the curing temperature is 80°C.

[0011] Preferably, the curing time is set to 30 minutes.

[0012] Preferably, the method further comprises step S4: performing diffuse reflectance test and / or functional test; the functional test comprises at least one of heat resistance test, chemical resistance test and weather resistance test.

[0013] Preferably, the spraying device is a fully automatic spraying equipment.

[0014] Preferably, the ultra-black paint material coating is made of acrylic polyurethane material.

[0015] Beneficial effects:

[0016] The invention improves the functionality of the newly formulated ultra-black paint after spraying by adjusting the formula ratio of the ultra-black paint, reduces the time required for curing, thereby improving production efficiency and reducing production costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 It is a curve diagram of the diffuse reflectance of the product surface after being coated with high-performance ultra-black paint according to an embodiment of the present invention. DETAILED DESCRIPTION

[0018] Combination Figure 1 This embodiment provides a method for applying a high-performance ultra-black paint, comprising the following steps:

[0019] S1. Remove stains on the surface of the product to be sprayed;

[0020] S2. Adjust the ratio of the ultra-black paint, mix 3-5 parts of the ultra-black paint, 0.9-1.1 parts of the curing agent and 2-4 parts of the thinner evenly, and spray the adjusted ultra-black paint evenly on the surface of the product to be sprayed through a spraying device;

[0021] S3, curing at a temperature of 70°C-100°C for 20min-50min;

[0022] S4. Perform diffuse reflectance test and / or functional test.

[0023] In this embodiment, the ultra-black paint coating can be an existing black paint coating, such as water-based acrylic paint Musou Black, epoxy black paint, etc. The curing agent adopts existing vinyl triamine, amide amine, etc., which is used to accelerate the curing time. The ultra-black paint coating, curing agent, and thinner can reduce the environmental requirements for ultra-black paint coating through the ratio of (3-5): (0.9-1.1): (2-4), shorten the time required for curing, make the diffuse reflectivity meet the requirements, and improve its anti-oxidation and anti-corrosion capabilities. In this embodiment, the ultra-black paint coating can adopt acrylic polyurethane, and the curing agent can adopt isocyanate materials.

[0024] In a preferred embodiment, the ratio of the ultra-black paint is 4 parts of ultra-black paint, 1 part of curing agent and 3 parts of thinner; the curing temperature is 80°C; the curing time is set to 30 minutes. Under this ratio, the performance of the ultra-black paint after painting is the best.

[0025] In another embodiment, a functional test is further included, and the functional test includes at least one of a heat resistance test, a chemical resistance test, and a weather resistance test. The diffuse reflectance test, the heat resistance test, the chemical resistance test, and the weather resistance test are all tested using existing test methods, which will not be described in detail here.

[0026] In step S2, the spraying device uses fully automatic spraying equipment to improve spraying efficiency and ensure spraying uniformity. The fully automatic spraying equipment uses existing equipment.

[0027] The solution of the embodiment of the present invention makes the performance of the sprayed product better.

[0028] The product performance after spraying of existing coatings is shown in Table 1:

[0029] Table 1

[0030]

[0031] The test results of product performance and diffuse reflectivity after spraying with ultra-black paint are shown in Table 2:

[0032] Table 2

[0033]

[0034] Through Table 1, Table 2 and Figure 1 The test results show that by adjusting the formula ratio of the ultra-black paint, the functionality of the newly formulated ultra-black paint after spraying is improved, and the time required for curing is reduced, thereby improving production efficiency and reducing production costs.

[0035] It should be understood that the above are only preferred implementations of the present invention, and the protection scope of the present invention is not limited to the above embodiments. All technical solutions under the concept of the present invention belong to the protection scope of the present invention.

[0036] The above description of the drawings used in the implementation manner only illustrates certain embodiments of the present invention and should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

Claims

1. A method for applying high-performance ultra-black paint, characterized in that: The steps include: S1. Remove stains on the surface of the product to be sprayed; S2. Adjust the ratio of the ultra-black paint, mix 3-5 parts of the ultra-black paint, 0.9-1.1 parts of the curing agent and 2-4 parts of the thinner evenly, and spray the adjusted ultra-black paint evenly on the surface of the product to be sprayed through a spraying device; S3. Curing at 70°C-100°C for 20min-50min.

2. The coating method of high-performance ultra-black paint according to claim 1, characterized in that: The ratio of the super black paint is 4 parts of super black paint, 1 part of curing agent and 3 parts of thinner.

3. The coating method of high-performance ultra-black paint according to claim 1, characterized in that: The curing temperature is 80°C.

4. The coating method of high-performance ultra-black paint according to claim 1, characterized in that: The curing time was set to 30 min.

5. The coating method of high-performance ultra-black paint according to claim 1, characterized in that: The method further comprises step S4: performing diffuse reflectance test and / or functional test; the functional test comprises at least one of heat resistance test, chemical resistance test and weather resistance test.

6. The coating method of high-performance ultra-black paint according to claim 1, characterized in that: The spraying device adopts fully automatic spraying equipment.

7. The coating method of high-performance ultra-black paint according to claim 1, characterized in that: The ultra-black paint material coating is made of acrylic polyurethane material.