Preparation method of silver-based carbon nanoparticles

Through the adjustment of the complex precursor of pyridines and silver nitrate and polyvinylpyrrolidone, combined with high temperature calcination in nitrogen atmosphere, silver-based carbon nanoparticles with high carbonization and small particle size were prepared, and the preparation of silver-based carbon nanoparticles in the prior art was solved. Contamination and toxicity problems in the process achieve longer-lasting antibacterial effects and higher safety.

CN118976904APending Publication Date: 2024-11-19INNER MONGOLIA MEDICAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411065777.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The chemical reduction method used in the existing silver-based carbon nanoparticle preparation method has hidden dangers of pollution, toxic materials and process complexity, and the prepared carbon nanoparticles may have difficulty in controlling toxicity and morphology.

Method used

Pyridine divalent silver complex precursors were prepared by using pyridines and silver nitrate as raw materials, and highly carbonized, small and uniform silver-based carbon nanoparticles were prepared by adjusting the particle size through polyvinylpyrrolidone and combining with high-temperature calcining in nitrogen atmosphere. Avoid particle size increase and the presence of toxic groups.

Benefits of technology

The high enrichment of silver elements and dispersion of smaller particles are achieved, providing a more lasting antibacterial effect, avoiding the emergence of bacterial resistance, and improving the safety and stability of the preparation process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976904A_ABST
    Figure CN118976904A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of silver-based carbon nano-particles, which comprises the following steps: preparing nano-particles of a pyridine divalent silver complex precursor by using pyridines and silver nitrate as raw materials, and adjusting the particle size of the complex nano-particles by using polyvinylpyrrolidone. And finally, preparing highly carbonized silver-based carbon nanoparticles which are relatively small and uniform in particle size through a nitrogen atmosphere high-temperature calcination method. According to the preparation method, raw materials are low in cost, the process is simple and controllable, according to the prepared silver-based nano-particles, under the condition that the size of the main body particles is not obviously increased, the silver element in the particles is highly enriched and dispersed in all positions of the main body particles in a smaller particle mode, the silver element can bring a more continuous antibacterial effect, generation of bacterial drug resistance can be avoided, and the antibacterial effect is better. The silver-based carbon nanoparticles are good in safety and stability. The method is suitable for preparing the silver-based carbon nanoparticles, and the silver-based carbon nanoparticles are further applied to skin antibacterial dressings.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of nano-drugs, and in particular relates to a method for preparing silver-based carbon nano-particles. Background Art

[0002] Silver nanoparticles have excellent antimicrobial properties and can effectively kill bacteria, fungi and viruses, while the addition of carbon nanoparticles can further enhance this antimicrobial effect. This material is widely used in topical medications and dressings to help prevent and treat various skin infections and bacterial diseases.

[0003] Among topical medications, antibacterial ointments and creams containing silver-carbon nanoparticles can effectively treat skin infections, accelerate wound healing, and reduce the risk of infection. This drug not only has a strong antibacterial effect, but also provides lasting protection, helping to relieve patients' pain and speed up the recovery process. It can also be added to dressings. Antibacterial dressings containing silver-carbon nanoparticles can effectively prevent wound infection and promote wound healing. This dressing has good breathability and comfort, can provide lasting antibacterial protection, help keep wounds clean and dry, and reduce the risk of infection.

[0004] The application of silver-based carbon nanoparticles in topical medications and dressings provides new options for treating skin infections and wound healing. The antibacterial properties and durability of this material can effectively protect patients' skin health, improve treatment outcomes, and provide safer and more effective solutions for healthcare.

[0005] At present, the preparation of silver-based carbon nanoparticles is mainly through chemical reduction, which is to reduce the solution containing silver ions into silver nanoparticles by adding a reducing agent to the solution, and at the same time, add carbon-based materials to the solution to make it interact with the silver nanoparticles to form silver-based carbon nanoparticles. However, this method has some disadvantages. The chemical reducing agent required for the chemical reduction method has the hidden danger of polluting the environment, and the prepared carbon nanoparticles may have toxicity, difficulty in morphology control and process complexity. In the prior art, Qin Liping et al. reported that a graphite phase carbon nitride-loaded silver-based nanoparticle composite material was prepared by chemical reduction. The silver-based carbon nanoparticles prepared by this method have excellent antibacterial properties, but a large amount of toxic dicyandiamide, melamine and thiourea are used in the process, which has certain safety issues.

[0006] Based on this, a method for preparing silver nanoparticles is urgently needed to solve the problems existing in the prior art. Summary of the invention

[0007] In view of the above technical problems, the present invention aims to provide a method for preparing silver-based carbon nanoparticles, using pyridine and silver nitrate as raw materials to prepare nanoparticles of pyridine divalent silver complex precursor, and using polyvinyl pyrrolidone to adjust the particle size of the complex nanoparticles, and finally preparing highly carbonized, small and uniform silver-based carbon nanoparticles by high-temperature calcination in a nitrogen atmosphere; the preparation method of the present invention has low raw materials, simple process and controllable, and the prepared silver-based nanoparticles, when the volume of the main particles is not significantly increased, make the silver element in the particles highly enriched, and dispersed in the form of smaller particles throughout the main particles, the silver element can bring a more sustained antibacterial effect, and can also avoid the generation of bacterial resistance. The silver-based carbon nanoparticles after calcination have removed the aminomethyl group and broken the pyridine ring structure, and the highly carbonized structure with the toxic group removed may bring higher safety and stability.

[0008] To achieve the above object, the technical solution adopted by the present invention is:

[0009] A method for preparing silver-based carbon nanoparticles is carried out in the following order:

[0010] (1) Dissolve silver nitrate and pyridine in water and mix well to obtain a bright white suspension, denoted as A;

[0011] (2) adding 35% ammonia water to A and mixing well to obtain B;

[0012] (3) Dissolve ammonium persulfate in water until it is completely dissolved without bubbles to obtain C;

[0013] (4) Add polyvinyl pyrrolidone to B and dissolve it uniformly by ultrasonication to obtain D;

[0014] (5) D and C were mixed by rapid stirring, and placed in a sealed, light-proof place at 20°C for 9 h to obtain E;

[0015] (6) E was centrifuged and washed three times with water and acetone respectively, and then dried naturally to obtain a reddish brown solid, which was recorded as F;

[0016] (7) F is placed in an iron crucible and calcined under a nitrogen atmosphere to obtain silver-based carbon nanoparticles.

[0017] As a limitation of the present invention, in step (1), the pyridine material is a pyridine compound containing a pyridine ring and exposing the nitrogen atom on the pyridine ring, and the molar ratio of the silver nitrate to the pyridine material is 1:(1-3).

[0018] As a second limitation of the present invention, in step (2), the volume ratio of the ammonia water to the water in step (1) is 1:10.

[0019] As a third limitation of the present invention, in step (3), the molar ratio of silver nitrate to ammonium persulfate is 1:(2-8).

[0020] As a fourth limitation of the present invention, in step (4), the mass ratio of polyvinyl pyrrolidone to ammonium persulfate is 0.25:1.82.

[0021] The roles of ammonium persulfate and polyvinyl pyrrolidone in the present invention are to provide oxidation to make the compound precipitate spontaneously and to control particle agglomeration to reduce particle size. The content of the two affects whether the complex can be precipitated and the particle size of the formed nanoparticles.

[0022] As a fifth limitation of the present invention, in step (6), the centrifugal speed is 16000 r / min and the centrifugal time is 10 min.

[0023] As a sixth limitation of the present invention, in step (7), the calcination process is carried out in sequence according to the following steps:

[0024] a. The first stage of heating: from room temperature to 87°C, keep warm for 30 minutes;

[0025] b. The second stage of heating: from 87℃ to 326℃, keep warm for 30min;

[0026] c. The third stage of heating: from 326℃ to 400℃, keep warm for 60min;

[0027] d. Cooling: Cool to room temperature along with the furnace.

[0028] As a further limitation of the present invention, the heating rate of the first heating stage is 3°C / min; the heating rate of the second heating stage is 3°C / min; and the heating rate of the third heating stage is 3°C / min.

[0029] The present invention adopts a three-stage heating method to prepare the final silver-based carbon nanoparticles. In the first stage of heating and heat preservation, crystal water evaporates, in the second stage of heating and heat preservation, dimethylamino on the pyridine ring falls off, and in the third stage of heating and heat preservation, the pyridine ring is partially decomposed and the silver elements in some molecules are released and enriched to form highly carbonized carbon nanoparticles containing high-purity silver crystals to form carbonized particles. These three stages are critical for the final formation of a structure in which the silver elements in the particles are highly enriched and dispersed in various parts of the main particles in the form of smaller particles without significantly increasing the volume of the main particles.

[0030] As a further limitation of the present invention, in step (1), the pyridine material is 4-dimethylaminopyridine.

[0031] As a seventh limitation of the present invention, the particle size of the silver-based carbon nanoparticles is about 100 nm, and the silver-based carbon nanoparticles are applied to antibacterial skin dressings.

[0032] As we all know, the particle size affects properties such as dispersibility, stability and biological activity. If the particle size of nanoparticles is too large, the surface area will be reduced, the contact area between the particles and bacteria and the number of exposed groups will be reduced, and the performance will be greatly reduced; if the particle size of nanoparticles is too small, aggregation and precipitation will easily occur, resulting in poor dispersion of the particles, making it difficult to play a role, and they may even pass through the cell membrane and affect normal cells.

[0033] The above technical solution of the present invention is taken as a whole, and each step is closely related and influences each other, which jointly determine the morphological characteristics and performance of the product.

[0034] The above technical solution has the following advantages or beneficial effects:

[0035] 1. The preparation method of the present invention is simple and the process is easy to control. The divalent silver pyridine complex is prepared into silver-based carbon nanoparticles by a method of calcination in a low vacuum-nitrogen atmosphere. The particle size of the silver-based carbon nanoparticles is about 100 nm, which is close to the particle size of the complex nanoparticles, and no obvious increase or fusion occurs. The silver-based nanoparticles prepared by this method have a high concentration of silver elements in the particles without significantly increasing the volume of the main particles, and are dispersed in the form of smaller particles throughout the main particles.

[0036] 2. The proportion of silver element in the silver-based carbon nanoparticles prepared by the present invention is nearly doubled, and the carbon element and nitrogen element are nearly halved. The silver-based carbon nanoparticles after calcination have removed the aminomethyl group and broken the pyridine ring structure. The highly carbonized structure with no toxic groups may bring higher safety and stability.

[0037] 3. The minimum inhibitory concentration of the silver-based carbon nanoparticles prepared by the present invention for inhibiting drug-resistant Staphylococcus aureus (MRSA) is 0.125 mg / mL, and the minimum inhibitory concentration for inhibiting Staphylococcus epidermidis is 0.25 mg / mL. The silver-based carbon nanoparticles have good antibacterial effect.

[0038] The invention is suitable for preparing silver-based carbon nanoparticles, and is further applied to skin antibacterial dressings. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 The SEM and TEM images of the divalent silver pyridine complex nanoparticles prepared in Example 1, wherein: Figures a, b, and c are SEM images of the divalent silver pyridine complex nanoparticles, and Figures d, e, and f are TEM images of the divalent silver pyridine complex nanoparticles;

[0040] Figure 2 The infrared spectra of 4-dimethylaminopyridine and the divalent silver complex of pyridine in Example 1 are compared, wherein: Figure a is the infrared spectrum of 4-dimethylaminopyridine, and Figure b is the infrared spectrum of the divalent silver complex of pyridine;

[0041] Figure 3 This is the energy spectrum of the divalent silver pyridine complex prepared in Example 1;

[0042] Figure 4 This is a differential scanning calorimetry curve of the divalent silver pyridine complex prepared in Example 1;

[0043] Figure 5 It is a comparison diagram of the products of Examples 1, 2, and 3;

[0044] Figure 6 The SEM and TEM images of the silver-based carbon nanoparticles prepared in Example 1, wherein: a and b are SEM images of the silver-based carbon nanoparticles, and ch is a TEM image of the silver-based carbon nanoparticles;

[0045] Figure 7 This is an infrared spectrum of the silver-based carbon nanoparticles prepared in Example 1;

[0046] Figure 8 This is the energy spectrum of the silver-based carbon nanoparticles prepared in Example 1;

[0047] Fig. 9 The bar graphs are the OD600 value changes of the minimum inhibitory concentration of the silver-based nanoparticles prepared in Example 1, wherein: Figure a is the OD600 value change graph of Staphylococcus aureus, and Figure b is the OD600 value change graph of Staphylococcus epidermidis;

[0048] Fig.10 This is a structural diagram of the divalent silver pyridine complex prepared in Example 1. DETAILED DESCRIPTION

[0049] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0050] In the present invention, unless otherwise specified, all equipment and raw materials can be purchased from the market or are commonly used in the industry. The methods in the following embodiments are all conventional methods in the art unless otherwise specified.

[0051] Example 1 A method for preparing silver-based carbon nanoparticles

[0052] This embodiment prepares a silver-based carbon nanoparticle, and the specific preparation method is carried out in the following order:

[0053] (1) Accurately weigh 0.1690 g of 1.0 mmol of silver nitrate and put it into a beaker, add 50 mL of distilled water to completely dissolve the silver nitrate, accurately weigh 0.3660 g of 3.0 mmol of 4-dimethylaminopyridine and add it to the above silver nitrate solution, and stir thoroughly to completely dissolve the 4-dimethylaminopyridine to form solution A;

[0054] (2) Add 5 mL of 25% ammonia water to solution A to change the solution from a turbid liquid to a transparent liquid to obtain solution B;

[0055] (3) Accurately weigh 1.8200 g of 4.0 mmol of ammonium persulfate and place it in a 100 mL beaker. Add 50 mL of distilled water to dissolve all the ammonium persulfate to obtain C.

[0056] (4) Add 0.2500 g of polyvinyl pyrrolidone to B and dissolve the polyvinyl pyrrolidone in the solution by ultrasonication to obtain D;

[0057] (5) Rapidly stir and mix solutions D and C, place in a sealed, light-proof place at 20°C for 9 hours to obtain E;

[0058] (6) E was centrifuged at 16000 r / min for 10 min, washed three times with distilled water and acetone respectively, and dried naturally to obtain a pyridine divalent silver complex precursor as a reddish brown solid, denoted as F;

[0059] (7) F is placed in an iron crucible and calcined in stages under a nitrogen atmosphere to obtain the final silver-based carbon nanoparticles. The specific calcination procedure is as follows:

[0060] a. The first stage of heating: heating from room temperature to 87°C at a heating rate of 3°C / min, and keeping warm for 30 minutes;

[0061] b. Second stage of heating: heating from 87°C to 326°C at a heating rate of 3°C / min, and keeping warm for 30 minutes;

[0062] c. The third stage of heating: heating from 326°C to 400°C at a heating rate of 3°C / min, and keeping the temperature for 60 minutes;

[0063] d. Cooling: Cool to room temperature along with the furnace.

[0064] The morphology and structure of F prepared in step (6) of this embodiment were measured, as shown in Figure 1 , Figure 2 and Figure 3As shown in the figure, the pyridine divalent silver complex nanoparticles are spherical, with uniform particle size distribution and small silver particles evenly distributed on the surface. Figure 6 The infrared spectrum and Figure 7 From the energy spectrum analysis diagram, we can infer that the specific structure of F is as follows Fig.10 shown.

[0065] The thermal calcination process of the divalent silver pyridine complex precursor prepared in step (7) of this embodiment was subjected to a thermogravimetric test. The divalent silver pyridine complex precursor was placed in a differential scanning calorimeter and subjected to thermal analysis at a heating rate of 3°C per minute. The results showed that under a nitrogen atmosphere, there was obvious heat release at 87°C, 326°C, and 400°C and a large amount of material decomposed. At 87°C, the main cause was evaporation of crystal water to form anhydrous dry particles; at 326°C, the main cause was the shedding of the dimethylamino group on the pyridine ring to form a new complex structure with a higher proportion of silver; at 400°C, the main cause was partial decomposition of the pyridine ring and the release and enrichment of the silver element in some molecules to form highly carbonized carbon nanoparticles containing high-purity silver crystals; as shown in FIG. Figure 4 According to the thermal analysis results, highly carbonized, small and uniform silver-based carbon nanoparticles can be prepared under the calcination conditions of 87°C and 326°C for 30 min respectively and 400°C for 60 min in a nitrogen atmosphere, as shown in FIG. Figure 5 The particle size of the final product particles prepared is about 100 nm, and the morphology is spherical with an uneven surface.

[0066] Example 2-3 Preparation method of silver-based carbon nanoparticles

[0067] Examples 2-3 respectively prepare silver-based carbon nanoparticles. The specific preparation method is similar to that of Example 1, except that the technical parameters in the preparation process are different, as follows. The results are shown in FIG. Figure 5 .

[0068]

[0069] Comparative Example

[0070] In order to explore the effect of the calcination process on the morphological characteristics of the final silver-based carbon nanoparticles, different silver-based carbon particles were prepared respectively. The specific preparation process was similar to that in Example 1, except that the calcination process was different during the preparation process, as follows.

[0071] Comparative Example 1

[0072] Calcination temperature and dwelling stage: keep warm at 87℃ for 30min, keep warm at 326℃ for 60min, the prepared product is brown and easily agglomerates and settles, such as Figure 5 shown.

[0073] Comparative Example 2

[0074] Calcination temperature and dwelling stage: keep at 87℃ for 30min, keep at 326℃ for 30min, and keep at 400℃ and 500℃ for 60min respectively. The product is black and has a lot of obvious large particles. See Figure 5 shown.

[0075] Antibacterial performance test

[0076] The antibacterial properties of the silver-based carbon nanoparticles prepared in Example 1 were tested, and the antibacterial experimental test steps were carried out according to the existing test steps, as follows:

[0077] 1.LB broth liquid culture medium

[0078] Take 12.5 g of LB broth, add distilled water to make up to 500 mL, place in an autoclave, sterilize at 121°C for 20 min, and cool to room temperature for use.

[0079] 2. Preparation of antibacterial drugs at different concentration gradients

[0080] The test tube two-fold dilution method was used. Twelve sterile EP tubes were taken, and 1 ml of the above LB broth was added to each tube as a liquid culture medium for bacteria. 1.0 ml of 4 mg / ml of the drug to be tested (the drug to be tested is the silver-based carbon nanoparticles prepared in Example 1) was added to the first tube, and 1.0 ml was drawn into the second tube after mixing. The same method was used to dilute the solution to the twelfth tube, and 1.0 ml was taken from the twelfth tube and placed in a sterile empty EP tube as a blank control.

[0081] 3. Antimicrobial testing

[0082] Add bacterial solution to each tube to make up to 10 -7 CFU / mL, mix well, culture MRSA bacteria and Staphylococcus epidermidis at 37°C, and after 48 hours, aspirate 200uL of the liquid in the tube into a 96-well plate, and measure the OD600 value using a microplate reader. The lowest drug concentration when there is no difference between the OD600 value of the sample and the OD600 value of the negative control (NC) is the minimum inhibitory concentration (MIC) of the drug.

[0083] Note: Negative control (NC) is the drug-free control without bacterial solution. Positive control is the drug-free control with bacterial solution. Blank control (C) is the drug-free control without bacterial solution.

[0084] Depend on Figure 8 and Fig. 9It can be known that the silver-based carbon nanoparticles prepared by the present invention have good antibacterial properties; the antibacterial experimental results show that the minimum inhibitory concentration of the silver-based carbon nanoparticles for inhibiting drug-resistant Staphylococcus aureus (MRSA) is 0.125 mg / mL, and the minimum inhibitory concentration for inhibiting Staphylococcus epidermidis is 0.25 mg / mL.

[0085] The excellent antibacterial performance of the silver-based carbon nanoparticles prepared by the present invention is mainly due to the fact that the silver element is highly enriched and distributed on the surface of the particles, and the particles are small enough and have a large surface area, so that they have good antibacterial performance.

[0086] Finally, it should be noted that the above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein with equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the scope of protection of the claims of the present invention.

Claims

1. A method for preparing silver-based carbon nanoparticles, characterized in that: Follow the steps below in order: (1) Dissolve silver nitrate and pyridine in water and mix well to obtain a bright white suspension, denoted as A; (2) adding 25% ammonia water to A and mixing well to obtain B; (3) Dissolve ammonium persulfate in water until it is completely dissolved without bubbles to obtain C; (4) Add polyvinyl pyrrolidone to B and dissolve it uniformly by ultrasonication to obtain D; (5) D and C were mixed by rapid stirring, and placed in a sealed, light-proof place at 20°C for 9 h to obtain E; (6) E was centrifuged and washed three times with water and acetone respectively, and then dried naturally to obtain a reddish brown solid, which was recorded as F; (7) F is placed in an iron crucible and calcined under a nitrogen atmosphere to obtain silver-based carbon nanoparticles.

2. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: In step (1), the pyridine material is a pyridine compound containing a pyridine ring and exposing the nitrogen atom on the pyridine ring, and the molar ratio of the silver nitrate to the pyridine material is 1:(1-3).

3. The method for preparing silver-based carbon nanoparticles according to claim 2, characterized in that: In step (1), the pyridine material is 4-dimethylaminopyridine.

4. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: In step (2), the volume ratio of the ammonia water to the water in step (1) is 1:

10.

5. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: In step (3), the molar ratio of silver nitrate to ammonium persulfate is 1:(2-8).

6. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: In step (4), the mass ratio of polyvinyl pyrrolidone to ammonium persulfate is 0.25:1.

82.

7. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: In step (6), the centrifugal speed is 16000 r / min and the centrifugal time is 10 min.

8. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: In step (7), the calcination process is carried out in sequence according to the following steps: a. The first stage of heating: from room temperature to 87°C, keep warm for 30 minutes; b. The second stage of heating: from 87℃ to 326℃, keep warm for 30min; c. The third stage of heating: from 326℃ to 400℃, keep warm for 60min; d. Cooling: Cool to room temperature along with the furnace.

9. The method for preparing silver-based carbon nanoparticles according to claim 8, characterized in that: In step (7), the heating rate of the first stage of heating is 3°C / min; the heating rate of the second stage of heating is 3°C / min; and the heating rate of the third stage of heating is 3°C / min.

10. The method for preparing silver-based carbon nanoparticles according to claim 1, characterized in that: The particle size of the silver-based carbon nanoparticles is about 100 nm; the silver-based carbon nanoparticles are applied to antibacterial skin dressings.