Method for improving performance of galvanized high-strength steel spot-welded joint
By generating high melting point compounds on the surface of galvanized high-strength steel and adopting two-stage spot welding process, the LME crack problem of galvanized high-strength steel spot welding joints is solved, which significantly improves the mechanical properties of the spot welding joints and is suitable for lightweight industries in the automobile manufacturing industry Quantitative technology.
Patent Information
- Application Number
- CN202411362936.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-27
- Publication Date
- 2024-11-19
AI Technical Summary
Galvanized high-strength steel is prone to liquid metal brittle (LME) cracks during resistance spot welding, which affects the mechanical properties of the spot welding joints and the safety of the vehicle. The existing technology methods have high requirements for equipment or are costly, and cannot be effectively solved. Crack problem.
The surface of galvanized high-strength steel is used to generate high-melting compound with Al plate and zinc layer. Combined with the two-stage spot welding process, the aluminum alloy plate overlaps with galvanized high-strength steel to inhibit the diffusion and penetration of liquid zinc and improve the spot welding joints shear performance.
It effectively reduces the number and depth of LME cracks, improves the mechanical properties of spot welded joints, and significantly improves the performance of galvanized high-strength steel spot welded joints, which is suitable for the development of automotive lightweight technology.
Smart Images

Figure CN118976972A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of high-strength steel welding technology, and in particular relates to a method for improving the performance of galvanized high-strength steel spot welding joints. Background Art
[0002] As people's awareness of energy conservation, environmental protection and vehicle safety continues to increase, lightweight technology has developed rapidly in the automotive industry. Against this background, the use of high-strength steel in the automotive industry is increasing, especially galvanized high-strength steel, which has excellent corrosion resistance and is highly favored in the automotive manufacturing industry. Resistance spot welding has the advantages of high production efficiency and low cost, and is the most widely used connection method in body assembly. However, the resistance spot welding joints of galvanized high-strength steel will produce liquid metal embrittlement (Liquid Metal Embrittlement, LME) cracks, which have a negative impact on the mechanical properties of the spot welding joints and the safety of the whole vehicle, and seriously restrict the application of galvanized high-strength steel.
[0003] There are still many defects in the research of galvanized high-strength steel welding in the prior art. For example, the patent "Resistance spot welding method of galvanized high-strength steel with good joint performance" with publication number CN108015401A uses three welding pulses to suppress the formation of liquid metal embrittlement (LME) cracks. This method has high requirements for spot welding equipment. The patent "Zinc-coated steel with reduced liquid metal embrittlement (LME) sensitivity" with publication number CN114686651A forms an oxide-containing layer on the surface of the steel substrate by annealing the steel substrate in an oxygen-containing atmosphere, thereby achieving the effect of reducing the LME sensitivity of the spot welding joint. This method has high requirements for steel production equipment. The patent "High-strength steel composite galvanized sheet resistant to spot welding LME cracks and its preparation method" with publication number CN116657033A compositely rolls a low-carbon steel composite layer on the surface of the high-strength steel body, preventing liquid metal from penetrating into the parent material along the grain boundary during spot welding, reducing the spot welding LME sensitivity of the high-strength steel composite galvanized sheet, and alleviating the spot welding LME crack problem; this method has high requirements for steel production equipment and is costly. When galvanized high-strength steel is resistance spot welded, as the heat input increases, the core diameter and the shear performance of the spot welding joint show an increasing trend. When the welding current is too large, LME cracks will appear in the spot welding joint. The LME crack density is usually 3-6 / cm, and the crack depth is usually 5-10μm. The presence of LME cracks causes the shear performance of the spot welding joint to be unable to exceed 20kN. Summary of the invention
[0004] In order to overcome the defects of the above-mentioned prior art, the purpose of the present invention is to provide a resistance spot welding method for GPa-grade galvanized high-strength steel, by which high-melting-point compounds are generated on the surface of the galvanized high-strength steel through the action of the Al plate and the zinc layer, and combined with the spot welding tooling and process, the purpose of improving the LME cracks of the galvanized high-strength steel spot welding joint is achieved, which is of great significance to the development of automobile lightweight technology.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides a method for improving the performance of galvanized high-strength steel spot welding joints, the method comprising the following steps:
[0006] Step 1: Select a GPa-grade galvanized high-strength steel plate with a predetermined composition, and use acetone or alcohol to clean the surface to be welded to remove impurities such as oil stains. The galvanized high-strength steel is GPa-grade galvanized high-strength steel, the thickness of the GPa-grade galvanized high-strength steel is 1.0-2.0 mm, and its chemical composition is C: 0.09%-0.14%, Si: 0.25%-0.38%, Mn: 2.35%-2.75%, P: 0.002%-0.020%, S: 0.003%-0.020%, Cr: 0.43%-0.76%, Nb: 0.010%-0.030%, Ti: 0.020%-0.045%, and the balance is Fe and other inevitable impurities; the microstructure of the galvanized high-strength steel is martensite and bainite, and the mechanical properties are yield strength ≥930MPa, tensile strength ≥1180MPa, and elongation after fracture ≥14%. The high-strength steel substrate slab is heated, rough rolled, finished rolled, cooled, coiled, cold rolled and continuously annealed to obtain an annealed substrate, and the annealed substrate is hot-dip galvanized, heat treated and skin-passed to obtain the galvanized high-strength steel sheet. The zinc liquid composition in the galvanizing process is Al: 6%-10%, Si: 4%-8%, Mg: 2%-5%, and the balance is Zn and unavoidable impurities. The zinc layer thickness is 80-100g / m 3 .
[0007] Step 2: Select an aluminum alloy plate with a predetermined composition, mechanically grind off the dense oxide layer on the surface to be welded, and use acetone or alcohol to clean the surface to be welded to remove impurities such as oil stains. The thickness of the aluminum alloy plate is 0.1-0.3 mm, and its chemical composition is as follows by weight percentage: Cu: 3.5%-6.5%, Mg: 1.0%-2.3%, Mn: 0.2%-1.0%, Cr: 0.05%-0.18%, Si: 0.35%-0.85%, Ni: 0.05%-0.35%, and the remainder is Al and other inevitable impurities.
[0008] Step 3: Overlap two GPa-grade galvanized high-strength steel plates, overlap two aluminum alloy plates on the upper and lower surfaces of the overlap area, and then place them between spot welding electrodes, which are chromium-zirconium-copper spherical electrodes with a radius of 30 mm.
[0009] Step 4: Set the spot welding parameters and perform welding; cooling water flow: 20-30L / min, slow rise 1 current 4.5-6.8kA, welding 1 time 72-120ms, welding 1 current 5.0-8.0kA, slow fall 1 time 0-10ms, slow fall 1 current 4.0-7.0kA, cooling 1 time 60-80ms; slow fall 2 time 0-12ms, slow rise 2 current 4.0-6.0kA, welding 2 time 150-220ms, welding 2 current 7.5-10.5kA, slow fall 2 time 0-10ms, slow fall 2 current 4.5-6.5kA, cooling 2 time 0-20ms. Among them, slow rise 1, welding 1, slow fall 1, cooling 1 refer to the technical parameters in the first stage spot welding process; slow rise 2, welding 2, slow fall 2, cooling 2 refer to the technical parameters in the second stage spot welding process.
[0010] Step 5: Shear performance test and LME crack density and maximum crack depth test. A single tensile test was conducted at a tensile speed of 30 mm / min to test the shear performance of the spot welded joints. The LME crack density and maximum crack depth were tested after the spot welded joints were inlaid, ground and polished.
[0011] The present invention adds a layer of aluminum alloy plate between the upper and lower electrodes and the galvanized high-strength steel. Figure 1 As shown, a certain amount of copper element is added to the aluminum alloy plate, and Al and Cu elements are easily combined with Zn element to form compounds. The compound has a high melting point and can inhibit the diffusion of liquid zinc into the high-strength steel, thereby reducing the number and depth of LME cracks in the spot welding joint. At the same time, with the two-stage spot welding process, the first stage mainly preheats the galvanized high-strength steel plate to initially form a molten core, and at the same time forms a high-melting point compound on the surface of the aluminum alloy and the galvanized steel to inhibit the penetration of liquid zinc into the high-strength steel side. The second stage mainly grows the galvanized high-strength steel molten core and expands the cross-sectional area of the molten core, thereby improving the shear performance of the spot welding joint and improving the performance of the galvanized high-strength steel spot welding joint.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] The invention discloses a resistance spot welding method for GPa-level galvanized high-strength steel, which generates a high melting point compound on the surface of the galvanized high-strength steel through the action of an Al plate and a zinc layer, and combines spot welding tooling and a process to achieve the purpose of improving LME cracks in spot welding joints of the galvanized high-strength steel; by reducing the number and depth of LME cracks and improving the shear performance of the spot welding joint, the problem of LME cracks in spot welding of galvanized high-strength steel can be effectively alleviated, and the obtained spot welding joint has excellent mechanical properties, and has great promotion and application value in the automobile manufacturing industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1It is a schematic diagram of the overlapping method of galvanized high-strength steel and aluminum alloy plate of the present invention. DETAILED DESCRIPTION
[0015] The present invention is further described below in conjunction with specific examples, but the present invention is not limited in any way. To avoid redundant description, the raw materials in the following examples are all commercially available products unless otherwise specified, and the methods used are all conventional methods unless otherwise specified.
[0016] A method for improving the performance of galvanized high-strength steel spot welded joints (such as Figure 1 The schematic diagram of the overlapping method of the galvanized high-strength steel and the aluminum alloy plate of the present invention shown in the figure comprises the following steps:
[0017] Step 1: Select GPa grade galvanized high-strength steel plate, clean the surface to be welded, and remove impurities;
[0018] Step 2: Select an aluminum alloy plate, grind off the dense oxide layer on the surface to be welded, clean the surface to be welded, and remove impurities;
[0019] Step 3: overlap two GPa-grade galvanized high-strength steel plates, overlap two aluminum alloy plates on the upper and lower surfaces of the overlap area, and then place them between spot welding electrodes, which are chromium-zirconium-copper spherical electrodes with a radius of 30 mm;
[0020] Step 4: Set spot welding parameters and perform welding;
[0021] Step 5: Shear performance test and LME crack density and maximum crack depth test.
[0022] The matters not described in the following embodiments are the same as the description of the above specific implementation methods.
[0023] Example 1
[0024] A method for improving the performance of galvanized high-strength steel spot welding joints, the specific steps are as follows:
[0025] Step 1: Select GPa grade galvanized high-strength steel with a thickness of 1.2mm. Its chemical composition by weight percentage is C: 0.098%, Si: 0.28%, Mn: 2.55%, P: 0.008%, S: 0.008%, Cr: 0.52%, Nb: 0.015%, Ti: 0.028%, and the balance is Fe and other inevitable impurities; its microstructure is martensite and bainite, and its mechanical properties are yield strength 950MPa, tensile strength 1195MPa, and elongation after fracture ≥14%. The high-strength steel substrate slab is subjected to heating, rough rolling, finish rolling, cooling, coiling, cold rolling and continuous annealing to obtain an annealed substrate, and the annealed substrate is subjected to hot-dip galvanizing, heat treatment and skin-passing to obtain the galvanized high-strength steel sheet; the zinc liquid composition in the galvanizing process is Al: 7.1%, Si: 5.2%, Mg: 2.8%, and the remainder is Zn and unavoidable impurities, and the zinc layer thickness is 90g / m 3 .
[0026] Step 2: Select an aluminum alloy plate with a predetermined composition, mechanically grind off the dense oxide layer on the surface to be welded, and use acetone or alcohol to clean the surface to be welded to remove impurities such as oil. The thickness of the aluminum alloy plate is 0.15 mm, and its chemical composition is Cu: 5.53%, Mg: 1.84%, Mn: 0.62%, Cr: 0.13%, Si: 0.55%, Ni: 0.25% by weight, and the remainder is Al and other inevitable impurities.
[0027] Step 3: Overlap two GPa-grade galvanized high-strength steel plates, overlap two aluminum alloy plates on the upper and lower surfaces of the overlap area, and then place them between spot welding electrodes, which are chromium-zirconium-copper spherical electrodes with a radius of 30 mm.
[0028] Step 4: Set the spot welding parameters and perform welding, the spot welding parameters are: cooling water flow: 25L / min, slow rise 1 current 4.8kA, welding 1 time 80ms, welding 1 current 7.0kA, slow drop 1 time 5ms, slow drop 1 current 5.5kA, cooling 1 time 70ms, slow drop 2 time 8ms, slow rise 2 current 4.8kA, welding 2 time 180ms, welding 2 current 9.0kA, slow drop 2 time 6ms, slow drop 2 current 5.2kA, cooling 2 time 0ms.
[0029] Step 5: Shear performance test: The maximum shear force of the spot welding joint is 22.43kN. LME crack detection: The crack density is 2.5 / cm and the maximum crack depth is 2.8μm.
[0030] Example 2
[0031] A method for improving the performance of galvanized high-strength steel spot welding joints, the specific steps are as follows:
[0032] Step 1: Select GPa-grade galvanized high-strength steel with a thickness of 1.6mm, and its chemical composition is C: 0.11%, Si: 0.28%, Mn: 2.45%, P: 0.009%, S: 0.009%, Cr: 0.61%, Nb: 0.021%, Ti: 0.028% by weight, and the balance is Fe and other inevitable impurities; its microstructure is martensite and bainite, and its mechanical properties are yield strength 988MPa, tensile strength 1238MPa, and elongation after fracture 16%. The high-strength steel substrate slab is heated, rough rolled, finished rolled, cooled, coiled, cold rolled and continuously annealed to obtain an annealed substrate, and the annealed substrate is hot-dip galvanized, heat treated and skin-passed to obtain the galvanized high-strength steel sheet. The zinc liquid composition in the galvanizing process is Al: 6.9%, Si: 6.5%, Mg: 3.2%, and the balance is Zn and unavoidable impurities. The zinc layer thickness is 95g / m 3 .
[0033] Step 2: Select an aluminum alloy plate with a predetermined composition, mechanically grind off the dense oxide layer on the surface to be welded, and use acetone or alcohol to clean the surface to be welded to remove impurities such as oil. The thickness of the aluminum alloy plate is 0.25 mm, and its chemical composition is Cu: 5.8%, Mg: 2.1%, Mn: 0.7%, Cr: 0.12%, Si: 0.63%, Ni: 0.24% by weight, and the remainder is Al and other inevitable impurities.
[0034] Step 3: Overlap two GPa-grade galvanized high-strength steel plates, overlap two aluminum alloy plates on the upper and lower surfaces of the overlap area, and then place them between spot welding electrodes, which are chromium-zirconium-copper spherical electrodes with a radius of 30 mm.
[0035] Step 4: Set the spot welding parameters and perform welding; the cooling water flow rate of the spot welding parameters is: 27L / min, slow rise 1 current 6.0kA, welding 1 time 100ms, welding 1 current 7.5kA, slow drop 1 time 0ms, slow drop 1 current 5.8kA, cooling 1 time 70ms, slow drop 2 time 0ms, slow rise 2 current 5.8kA, welding 2 time 200ms, welding 2 current 10.0kA, slow drop 2 time 8ms, slow drop 2 current 6.2kA, cooling 2 time 10ms.
[0036] Step 5: Shear performance test: The maximum shear force of the spot welding joint is 23.58kN. LME crack detection: The crack density is 1.8 / cm and the maximum crack depth is 1.68μm.
[0037] Comparative Example 1
[0038] A method for improving the performance of galvanized high-strength steel spot welding joints, the specific steps are as follows:
[0039] Step 1: Select GPa-grade galvanized high-strength steel with a thickness of 1.6mm, and its chemical composition is C: 0.14%, Si: 0.23%, Mn: 2.35%, P: 0.009%, S: 0.009%, Cr: 0.61%, Nb: 0.021%, Ti: 0.028% by weight, and the balance is Fe and other inevitable impurities; its microstructure is martensite and bainite, and its mechanical properties are yield strength 988MPa, tensile strength 1238MPa, and elongation after fracture 15%. The high-strength steel substrate slab is heated, rough rolled, finished rolled, cooled, coiled, cold rolled and continuously annealed to obtain an annealed substrate, and the annealed substrate is hot-dip galvanized, heat treated and skin-passed to obtain the galvanized high-strength steel sheet. The zinc liquid composition in the galvanizing process is Al: 6.3%, Si: 2.5%, Mg: 6.0%, and the balance is Zn and unavoidable impurities. The zinc layer thickness is 92g / m 3 .
[0040] Step 2: Select an aluminum alloy plate with a predetermined composition, mechanically grind off the dense oxide layer on the surface to be welded, and use acetone or alcohol to clean the surface to be welded to remove impurities such as oil. The thickness of the aluminum alloy plate is 0.25 mm, and its chemical composition is Cu: 5.8%, Mg: 2.1%, Mn: 0.7%, Cr: 0.12%, Si: 0.63%, Ni: 0.24% by weight, and the remainder is Al and other inevitable impurities.
[0041] Step 3: Overlap two GPa-grade galvanized high-strength steel plates, overlap two aluminum alloy plates on the upper and lower surfaces of the overlap area, and then place them between spot welding electrodes, which are chromium-zirconium-copper spherical electrodes with a radius of 30 mm.
[0042] Step 4: Set the spot welding parameters and perform welding; the cooling water flow rate of the spot welding parameters is: 26L / min, slow rise 1 current 3.8kA, welding 1 time 50ms, welding 1 current 4.2kA, slow drop 1 time 12ms, slow drop 1 current 3.8kA, cooling 1 time 100ms, slow drop 2 time 20ms, slow rise 2 current 7.2kA, welding 2 time 130ms, welding 2 current 6.5kA, slow drop 2 time 5ms, slow drop 2 current 7.0kA, cooling 2 time 10ms.
[0043] Step 5: Shear performance test: The maximum shear force of the spot welding joint is 17.58 kN. LME crack detection: The crack density is 5.8 lines / cm and the maximum crack depth is 12.3 μm.
[0044] For any technician familiar with the art, without departing from the scope of the technical solution of the present invention, the technical content disclosed above can be used to make many possible changes and modifications to the technical solution of the present invention, or modified into equivalent embodiments with equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should still fall within the scope of protection of the technical solution of the present invention.
Claims
1. A method for improving the performance of galvanized high-strength steel spot welding joints, characterized in that: The method comprises the following steps: Step 1: Select GPa grade galvanized high-strength steel plate, clean the surface to be welded, and remove impurities; Step 2: Select an aluminum alloy plate, grind off the dense oxide layer on the surface to be welded, clean the surface to be welded, and remove impurities; Step 3: overlap two GPa-grade galvanized high-strength steel plates, overlap two aluminum alloy plates on the upper and lower surfaces of the overlap area, and then place them between spot welding electrodes, which are chromium-zirconium-copper spherical electrodes with a radius of 30 mm; Step 4: Set spot welding parameters and perform welding; Step 5: Shear performance test and LME crack density and maximum crack depth test.
2. The method according to claim 1, characterized in that Step 1: The thickness of the GPa-grade galvanized high-strength steel is 1.0-2.0 mm, and its chemical composition by weight percentage is C: 0.09%-0.14%, Si: 0.25%-0.38%, Mn: 2.35%-2.75%, P: 0.002%-0.020%, S: 0.003%-0.020%, Cr: 0.43%-0.76%, Nb: 0.010%-0.030%, Ti: 0.020%-0.045%, and the remainder is Fe and other inevitable impurities.
3. The method according to claim 1, characterized in that: The microstructure of the GPa-grade galvanized high-strength steel in step 1 is martensite and bainite, and the mechanical properties are yield strength ≥930MPa, tensile strength ≥1180MPa, and elongation after fracture ≥14%.
4. The method according to claim 1, characterized in that: Step 1: The high-strength steel substrate slab is heated, rough rolled, finished rolled, cooled, coiled, cold rolled and continuously annealed to obtain an annealed substrate; the annealed substrate is hot-dip galvanized, heat treated and skin-passed to obtain a galvanized high-strength steel sheet; the zinc liquid composition in the hot-dip galvanizing process is Al: 6%-10%, Si: 4%-8%, Mg: 2%-5%, and the remainder is Zn and unavoidable impurities, and the zinc layer thickness is 80-100g / m 3 .
5. The method according to claim 1, characterized in that The aluminum alloy plate in step 2 has a thickness of 0.1-0.3 mm, and its chemical composition by weight percentage is Cu: 3.5%-6.5%, Mg: 1.0%-2.3%, Mn: 0.2%-1.0%, Cr: 0.05%-0.18%, Si: 0.35%-0.85%, Ni: 0.05%-0.35%, and the remainder is Al and other inevitable impurities.
6. The method according to claim 1, characterized in that The spot welding parameters described in step 4 are: cooling water flow rate: 20-30L / min, slow rise 1 current 4.5-6.8kA, welding 1 time 72-120ms, welding 1 current 5.0-8.0kA, slow drop 1 time 0-10ms, slow drop 1 current 4.0-7.0kA, cooling 1 time 60-80ms, slow drop 2 time 0-12ms, slow rise 2 current 4.0-6.0kA, welding 2 time 150-220ms, welding 2 current 7.5-10.5kA, slow drop 2 time 0-10ms, slow drop 2 current 4.5-6.5kA, cooling 2 time 0-20ms.