Basalt nanosheet and preparation method thereof

By amidation modification of basalt scales and coordination bonding with perovskites, the problem of unstable performance of basalt sheets is solved, the strength and stability of the material are improved, and the performance improvement in composite materials is achieved and 环境适应性。

CN118978165AActive Publication Date: 2024-11-19四川文理学院 +2

Patent Information

Application Number
CN202411211372.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-19
Estimated Expiration
2044-08-30

Smart Images

  • Figure BDA0005020394370000131
    Figure BDA0005020394370000131
Patent Text Reader

Abstract

The invention relates to the technical field of basalt nanomaterials, and discloses a basalt nanosheet and a preparation method thereof in order to solve the problems that an existing modified basalt sheet is uneven in product performance, unstable and not long-acting, and the basalt nanosheet comprises modified basalt flakes and perovskite, the modified basalt flakes are connected with the perovskite through coordination bonding; the use amount ratio of the modified basalt flakes to the perovskite is (1.2 to 1.5): (0.5 to 0.85) according to the mass. According to the preparation method, basalt scales are subjected to amidation modification treatment and then compounded with perovskite, coordination ions in perovskite are subjected to coordination combination with acylamino, the coordination effect of the acylamino and lead ions is obviously enhanced under the action of dipoles, the defect state density caused by modification and compounding of basalt and other materials is reduced, and the performance of the composite material is improved. And the performance of the basalt material is more stable, controllable and long-acting.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of basalt nanomaterials, and in particular to a basalt nanosheet and a preparation method thereof. Background Art

[0002] Basalt fiber is an inorganic, environmentally friendly, green, high-performance fiber material. It is mainly composed of oxides such as silicon dioxide, aluminum oxide, calcium oxide, magnesium oxide, iron oxide and titanium dioxide. It is made by melting basalt ore at high temperature and drawing it into wire. It has silicates similar to natural ore and can be biodegraded in the environment after being discarded. As one of the four major fibers in my country, basalt fiber has been industrialized and applied. It is commonly used in fiber-reinforced composite materials, friction materials, shipbuilding materials, thermal insulation materials, the automotive industry, high-temperature filter fabrics, and protective materials.

[0003] With the rapid development of electronics and other technologies, the application of basalt fiber materials is becoming more and more extensive, and with it comes higher demands for material morphology and other aspects. For example, the patent with publication number CN114477199A provides a basalt nanosheet and a preparation method thereof. By sequentially etching the surface, etching the depth, dispersing and crushing, etc., basalt flakes can be made into basalt nanosheets with higher precision. Further, the patent with publication number CN115044079A provides an aramid nanofiber doped basalt nanosheet composite insulating film and a preparation method thereof, which combines the aramid nanofiber with the basalt nanosheet by doping, thereby giving the basalt nanosheet higher strength, temperature resistance, etc. However, in the above-mentioned insulating film, when the aramid nanofiber is doped with the basalt nanosheet, the pore combination controllability of the aramid nanofiber and the basalt nanosheet is low, which is manifested as uneven or insufficient doping, resulting in the problem of uneven product performance.

[0004] Based on the above situation, a high-performance basalt nanosheet material with stable product performance is needed. Summary of the invention

[0005] The technical problems to be solved by the present invention are:

[0006] In order to improve the material properties of basalt sheets or give them the characteristics required in special application scenarios, other materials with modification functions are usually added to basalt sheets for compounding, thereby improving the overall use effect of basalt sheets according to needs. However, in the modification treatment for improving the hardness or tolerance of basalt sheets, there are basalt sheet products with uneven performance, instability and lack of long-term effect.

[0007] The technical solution adopted by the present invention is:

[0008] The present invention provides a basalt nanosheet, comprising modified basalt flakes and perovskite, wherein the modified basalt flakes and the perovskite are connected by coordination bonding; in terms of mass, the usage ratio of the modified basalt flakes to the perovskite is 1.2-1.5:0.5-0.85.

[0009] Preferably, the basalt flakes have a thickness of 3-20 μm.

[0010] Preferably, its thickness is 20-45 nm.

[0011] The present invention also provides a method for preparing the above-mentioned basalt nanosheets, comprising the following steps:

[0012] (1) Preparation of modified basalt flakes;

[0013] (2) preparing a perovskite precursor solution;

[0014] (3) adding the modified basalt flakes to the perovskite precursor solution, heating to 50-65° C. for reaction, then cooling to 25-35° C. for reaction, crushing, and drying to obtain the basalt nanosheets.

[0015] Preferably, in step (1), the method for preparing modified basalt flakes comprises the following steps: taking cleaned basalt fiber flakes, adding to 1.5-2.8% volume fraction of an amide-containing silane coupling agent-ethanol solution, adding a catalyst, stirring the reaction, filtering and drying, to obtain the modified basalt flakes.

[0016] Preferably, the preparation method of the amide-containing silane coupling agent comprises the following steps: taking an aminosilane coupling agent and xylene, mixing them evenly, reacting them at 5-10°C, and adding glacial acetic acid dropwise during the reaction; after the reaction is completed, distilling and removing impurities to obtain the amide-containing silane coupling agent.

[0017] Preferably, the mass ratio of the aminosilane coupling agent to xylene is 1:2.5-3.

[0018] Preferably, at the beginning of the reaction, glacial acetic acid is added dropwise at a uniform rate of 0.5-1.5 mL / min, and the total amount of glacial acetic acid added is equal to the mass of the aminosilane coupling agent.

[0019] Preferably, in step (2), the method for preparing the perovskite precursor solution comprises the following steps: taking perovskite, adding it to 1.5-3 times the volume of an organic solvent, and ultrasonically dispersing it to obtain the perovskite precursor solution.

[0020] Preferably, in step (3), the reaction time at a temperature of 50-65°C is 1-2.5 h, and the reaction time at a temperature of 25-35°C is 0.5-1.25 h.

[0021] The beneficial effects of the present invention are as follows:

[0022] The basalt nanosheets of the present invention first perform an amidation modification treatment on the basalt flakes, and then compound them with perovskite. The coordination ions in the perovskite are coordinated with the amide groups. Under the action of dipoles, the coordination effect of the amide groups and lead ions is significantly enhanced, thereby reducing the defect state density caused by the modification and compounding of basalt with other materials, making the performance of the basalt material more stable, controllable and long-lasting. Furthermore, during the coordination and combination, through appropriate heating reaction, the calcium ions in the perovskite and the basalt flakes realize silicon-oxygen-calcium covalent bonding to form a crystal connection, thereby improving the strength of the basalt material and maintaining long-term stability in harsh environments. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0024] The present invention provides a method for preparing basalt nanosheets, comprising the following steps:

[0025] (1) Taking an appropriate amount of basalt flakes, placing them in ethanol so that the ethanol completely immerses the basalt flakes, stirring, filtering and drying, and obtaining a basalt flake to be treated with a layer thickness of about 3-20 μm; taking another amide-containing silane coupling agent, adding ethanol, and preparing an amide-containing silane coupling agent solution with a volume fraction of 1.5-2.8%, adding the basalt flakes to be treated and a catalyst, stirring for reaction, filtering and drying, and obtaining amide-containing basalt flakes for use as modified basalt flakes.

[0026] (2) Take an appropriate amount of perovskite, add it to 1.5-3 times the volume of an organic solvent, and ultrasonically disperse it for 0.5-1.2 hours to obtain a perovskite precursor solution.

[0027] (3) Take amide basalt flakes and add them to the perovskite precursor solution, control the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution to be 1.2-1.5:0.5-0.85, first apply an electric field to heat to 50-65°C, react for 1-2.5 hours, then remove the electric field and cool to 25-35°C, react for 0.5-1.25 hours; after the reaction is completed, ultrasonically crush, let stand to separate, remove the clarified layer, place in a 0.05-0.1MPa vacuum drying oven, and dry for 20-35 hours to obtain basalt nanosheets with a thickness of about 20-45nm.

[0028] In the present invention, amide-based basalt flakes are combined with over-coordinated lead ions in perovskite. Under an external electric field, the coordination effect between the amide group and the lead ions is significantly enhanced through the dipole effect, thereby reducing the defect state density caused by the modified composite of basalt and other materials, making the performance of the basalt nanosheet product more stable, controllable and long-lasting.

[0029] In the present invention, the preparation method of the amide silane coupling agent comprises the following steps:

[0030] Take an aminosilane coupling agent, add 2.5-3 times the mass of xylene, mix well, and place in a low temperature environment of 5-10°C to react. After the reaction starts, add glacial acetic acid of the same mass as the aminosilane coupling agent at a uniform rate of 0.5-1.5 mL / min. After the addition is completed, continue stirring to react for 8-10 hours, distill and remove impurities to obtain an amide-containing silane coupling agent.

[0031] The aminosilane coupling agent can be selected from common and universal amino-containing silane coupling agents such as dimethyldimethoxysilane, isopropyltrimethoxysilane, dimethylaminosilane, and butylaminosilane.

[0032] Example 1

[0033] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0034] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated and the amide silane coupling agent is equivalent, then add 0.3 times the volume of 1M hydrochloric acid solution, stir to react for 3.5 hours, filter and dry, obtain amide basalt flake, and store it for later use.

[0035] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0036] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.7, amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2℃ with an external electric field for 1.75h, then cooled to 30±2℃ without the electric field for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt nanosheets with a thickness of about 30nm.

[0037] Example 2

[0038] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0039] Take another basalt flake, place it in ethanol so that the ethanol completely covers the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, and prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated is 2 times the mass of the amide silane coupling agent, and then add 0.3 times the volume of 1M hydrochloric acid solution, stir the reaction for 3.5 hours, filter and dry, obtain amide basalt flakes, and store them for later use.

[0040] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0041] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.7, amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2℃ with an external electric field for 1.75h, then cooled to 30±2℃ without the electric field for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt nanosheets with a thickness of about 30nm.

[0042] Example 3

[0043] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0044] Take another basalt flake, place it in ethanol so that the ethanol completely covers the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, and prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the amide silane coupling agent is 2 times the mass of the basalt flake to be treated, and then add 0.3 times the volume of 1M hydrochloric acid solution, stir the reaction for 3.5 hours, filter and dry, obtain amide basalt flakes, and store them for later use.

[0045] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0046] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.7, amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2℃ with an external electric field for 1.75h, then cooled to 30±2℃ without the electric field for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt nanosheets with a thickness of about 30nm.

[0047] Example 4

[0048] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0049] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated and the amide silane coupling agent is equivalent, then add 0.3 times the volume of 1M hydrochloric acid solution, stir to react for 3.5 hours, filter and dry, obtain amide basalt flake, and store it for later use.

[0050] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0051] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.5:0.55, amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2℃ with an external electric field for 1.75h, then cooled to 30±2℃ without the electric field for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt nanosheets with a thickness of about 30nm.

[0052] Example 5

[0053] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0054] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated and the amide silane coupling agent is equivalent, then add 0.3 times the volume of 1M hydrochloric acid solution, stir to react for 3.5 hours, filter and dry, obtain amide basalt flake, and store it for later use.

[0055] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0056] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.83, amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2℃ with an external electric field for 1.75h, then cooled to 30±2℃ without the electric field for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt nanosheets with a thickness of about 30nm.

[0057] Example 6

[0058] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0059] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated and the amide silane coupling agent is equivalent, then add 0.3 times the volume of 1M hydrochloric acid solution, stir to react for 3.5 hours, filter and dry, obtain amide basalt flake, and store it for later use.

[0060] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0061] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.7, amide basalt flakes were added to the perovskite precursor solution, first heated to 50°C with an external electric field for 1 hour, and then cooled to 33°C without the electric field for 1.2 hours. After the reaction, ultrasonic treatment was performed for 30 hours to obtain basalt nanosheets with a thickness of about 30 nm.

[0062] Example 7

[0063] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0064] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated and the amide silane coupling agent is equivalent, then add 0.3 times the volume of 1M hydrochloric acid solution, stir to react for 3.5 hours, filter and dry, obtain amide basalt flake, and store it for later use.

[0065] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0066] According to the mass ratio of amide basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.7, amide basalt flakes were added to the perovskite precursor solution, first heated to 65°C with an external electric field for 2.3 hours, and then cooled to 30°C without the electric field for 0.85 hours. After the reaction, ultrasonic treatment was performed for 30 hours to obtain basalt nanosheets with a thickness of about 30 nm.

[0067] Comparative Example 1

[0068] Take basalt flakes, place them in ethanol so that the ethanol completely covers the basalt flakes, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flakes and form a large number of pore structures, and obtain basalt flakes with a thickness of about 15 μm to be treated, which are stored for later use.

[0069] Take perovskite, add 2.5 times the volume of dimethylformamide, and disperse it ultrasonically for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0070] According to the mass ratio of the basalt flakes to be treated and the perovskite in the perovskite precursor solution of 1.2:0.7, the amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2°C for reaction for 1.75h, and then cooled to 30±2°C for reaction for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt sheets.

[0071] Comparative Example 2

[0072] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0073] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt scale, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt scale to be treated with a thickness of about 15 μm; take another dimethyldimethoxysilane, add it to ethanol, prepare a dimethyldimethoxysilane-ethanol solution with a volume concentration of 2.2%, add the basalt scale to be treated, and the mass of the basalt scale to be treated is equivalent to that of dimethyldimethoxysilane, then add 0.3 times the volume of 1M hydrochloric acid solution, stir the reaction for 3.5 hours, filter and dry, obtain aminobasalt flakes, and store them for later use.

[0074] Take another perovskite, add 2.5 times the volume of dimethylformamide, and disperse it by ultrasonic for 1 hour to obtain a perovskite precursor solution, which is stored for later use.

[0075] According to the mass ratio of amino basalt flakes to perovskite in the perovskite precursor solution of 1.2:0.7, the amide basalt flakes were added to the perovskite precursor solution, first heated to 60±2℃ for reaction for 1.75h, and then cooled to 30±2℃ for reaction for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt sheets.

[0076] Comparative Example 3

[0077] Take 1 part by mass of dimethyldimethoxysilane, add 2.5 parts by mass of xylene, stir and mix, place in a 7±2°C low temperature box to react, at the beginning of the reaction, add 1 part by mass of glacial acetic acid at a uniform rate, and the total addition time is controlled to be about 2h. After the addition is completed, continue stirring to react for 8h, and finally distill off excess anhydride and xylene to obtain an amide silane coupling agent, which is stored for later use.

[0078] Take another basalt flake, place it in ethanol, make the ethanol completely cover the basalt flake, stir for 15 minutes, filter and dry, remove impurities on the surface of the basalt flake and form a large number of pore structures, and obtain a basalt flake to be treated with a thickness of about 15 μm; take another amide silane coupling agent, add it to ethanol, prepare an amide silane coupling agent-ethanol solution with a volume concentration of 2.2%, add the basalt flake to be treated, and the mass of the basalt flake to be treated and the amide silane coupling agent is equivalent, then add 0.3 times the volume of 1M hydrochloric acid solution, stir to react for 3.5 hours, filter and dry, obtain amide basalt flake, and store it for later use.

[0079] Amido basalt flakes were added to dimethylformamide, first heated to 60±2°C for reaction for 1.75h, then cooled to 30±2°C for reaction for 0.85h; after the reaction, ultrasonic treatment was performed for 30h to obtain basalt flakes.

[0080] Test example

[0081] Take the basalt materials prepared in Examples 1 to 7 and Comparative Examples 1 to 3, randomly cut 5mm*5mm sheet material samples, and measure the tensile strength of the samples according to the test method in GB / T 38111-2019 Classification and grading of basalt fibers and codes, and measure the breakdown strength of the samples according to the test method in GB / T 6461-2002 Rating of samples and test pieces of metal and other inorganic coatings on metal substrates after corrosion tests; then place the samples in an alkaline salt solution or a high temperature environment of 500°C, stand for 2 hours, and take them out and repeat the above performance tests. The results are summarized in Table 1:

[0082] The alkali salt solution is a 1L aqueous solution containing 1 mol of equimolar masses of sodium hydroxide, potassium hydroxide, sodium chloride and sodium sulfate. After alkali salt corrosion, it is rinsed with deionized water and then measured; after high-temperature treatment, it is cooled to room temperature and then measured.

[0083] Table 1 Performance test results of different basalt material samples

[0084]

[0085] It can be seen from Table 1 above that before alkali salt or high temperature treatment, the strength properties of the basalt material samples in Examples 1 to 7 are higher than those of the basalt material samples in Comparative Examples 1 to 3, indicating that the basalt nanosheets in the present invention can improve the strength properties of the basalt material by coordination bonding with perovskite; and after alkali salt or high temperature treatment, the reduction in the strength properties of the basalt material samples in Examples 1 to 7 is significantly smaller than the reduction in the strength properties of the basalt material samples in Comparative Examples 1 to 3, indicating that the basalt nanosheets of the present invention can maintain their strength properties more stably in a strong corrosion environment or an extreme temperature environment, that is, the effect of the modification treatment of the basalt flake performance of the present invention is significant and stable.

[0086] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A basalt nanosheet, It is characterized in that It comprises modified basalt flakes and perovskite, wherein the modified basalt flakes and the perovskite are connected by coordination bonding; By mass, the usage ratio of the modified basalt flakes to the perovskite is 1.2-1.5:0.5-0.

85.

2. The basalt nanosheet according to claim 1, It is characterized in that The basalt flakes have a thickness of 3-20 μm.

3. The basalt nanosheet according to claim 1, It is characterized in that Its thickness is 20-45nm.

4. A method for preparing the basalt nanosheets according to any one of claims 1 to 3, It is characterized in that The steps include: (1) Preparation of modified basalt flakes; (2) preparing a perovskite precursor solution; (3) adding the modified basalt flakes to the perovskite precursor solution, heating to 50-65° C. for reaction, then cooling to 25-35° C. for reaction, crushing, and drying to obtain the basalt nanosheets.

5. The method for preparing basalt nanosheets according to claim 4, It is characterized in that In step (1), the method for preparing modified basalt flakes comprises the following steps: The cleaned basalt fiber flakes are added to an amide-containing silane coupling agent-ethanol solution with a volume fraction of 1.5-2.8%, a catalyst is added, the mixture is stirred for reaction, and the mixture is filtered and dried to obtain the modified basalt flakes.

6. The method for preparing basalt nanosheets according to claim 5, It is characterized in that The preparation method of the amide-containing silane coupling agent comprises the following steps: The aminosilane coupling agent and xylene are mixed evenly, placed at 5-10° C. for reaction, and glacial acetic acid is added dropwise during the reaction; after the reaction is completed, impurities are removed by distillation to obtain the amide-containing silane coupling agent.

7. The method for preparing basalt nanosheets according to claim 6, It is characterized in that The mass ratio of aminosilane coupling agent to xylene is 1:2.5-3.

8. The method for preparing basalt nanosheets according to claim 6, It is characterized in that At the beginning of the reaction, glacial acetic acid is added dropwise at a uniform rate of 0.5-1.5 mL / min, and the total amount of glacial acetic acid added is equal to the mass of the aminosilane coupling agent.

9. The method for preparing basalt nanosheets according to claim 4, It is characterized in that In step (2), the method for preparing the perovskite precursor solution comprises the following steps: Take perovskite, add it into 1.5-3 times volume of organic solvent, and disperse it by ultrasonic to obtain the perovskite precursor solution.

10. The method for preparing basalt nanosheets according to any one of claims 4 to 9, It is characterized in that In step (3), the reaction time at a temperature of 50-65°C is 1-2.5 h, and the reaction time at a temperature of 25-35°C is 0.5-1.25 h.

Citation Information

Patent Citations

  • Basalt nanosheet and preparation method thereof

    CN114477199A

  • Aramid nanofiber doped basalt nanosheet composite insulating film and preparation method thereof

    CN115044079A

  • Basalt fiber-based photoelectric material and preparation method thereof

    CN111117613A

  • Surface coordination modified all-inorganic perovskite and preparation method and application thereof

    CN118540970A

  • Basalt fiber sheet for repairing and reinforcing concrete structure and repairing and reinforcing method for concrete structure using same

    KR102265343B1

Cited By