Integral electroactive ceramic membrane as well as preparation method and application thereof

By forming a uniformly loaded TiO2 layer on the ceramic membrane, the porous structure of the ceramic membrane improves the electrocatalytic capacity and anti-pollution ability, solving the problem of insufficient loading of the conductive layer in the prior art, and achieving efficient pollutant removal and membrane large-scale production.

CN118978230AInactive Publication Date: 2024-11-19江苏环保产业技术研究院股份公司 +1
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411260545.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-09
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing electroactive ceramic membranes do not fully utilize the porous structure of the ceramic membrane when loading the conductive layer, and it is difficult to achieve large-scale production, resulting in insufficient electrocatalytic and anti-pollution ability.

Method used

By mixing tetrabutyl titanate with an alcohol solvent, solution a is formed, diethanolamine and water is mixed to form solution b, the ceramic film is flowed through respectively to form the first and second ceramic films, and the process is repeated, followed by sintering and The hydrogen gas is reduced to form an overall electroactive ceramic film loaded with TiO2, and the uniformly loaded conductive layer is on the surface of the ceramic film and the pores.

Benefits of technology

It significantly improves the efficiency of electrocatalytic treatment and pollutant removal rate, reduces membrane pollution, is suitable for different organic industrial wastewater application scenarios, and controls the thickness and morphology of the load layer.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the technical field of wastewater treatment, and provides an integral electroactive ceramic membrane as well as a preparation method and application thereof. The preparation method comprises the following steps: mixing tetrabutyl titanate with an alcohol solvent to obtain a solution a; mixing diethanol amine with water to obtain a solution b; enabling the solution a to flow through a ceramic membrane to obtain a first ceramic membrane; enabling the solution b to flow through a first ceramic membrane to obtain a second ceramic membrane; repeating the process to obtain a ceramic membrane containing active components; sintering the TiO2-loaded ceramic membrane to obtain a TiO2-loaded ceramic membrane; and reducing the TiO2-loaded ceramic membrane in a hydrogen atmosphere to obtain the integral electroactive ceramic membrane. A conductive layer is uniformly loaded on the surface and in a pore channel of the prepared integral electroactive ceramic membrane, more electrochemical active sites can be provided, gradient degradation is realized when organic pollutants penetrate through the membrane by utilizing a confinement space in the membrane, the removal efficiency of the pollutants can be remarkably improved, and meanwhile, the membrane pollution can be reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wastewater treatment, and in particular to an integral electroactive ceramic membrane and a preparation method and application thereof. Background Art

[0002] Electroactive ceramic membrane is an emerging membrane material with broad application prospects in the field of deep treatment of industrial wastewater. It combines electrochemical oxidation with membrane separation, effectively solving the problems of high energy consumption and low current efficiency in the electrochemical oxidation process. It also solves the membrane pollution problem in the membrane separation process, achieving synergistic efficiency.

[0003] Chinese patent CN202210717325.6 discloses a double-sided electrocatalytic active ceramic membrane and its preparation method and water treatment application. It uses a ceramic membrane as a base membrane, sputters Ti4O7 on both sides of the membrane as an electrocatalytic membrane anode, and deposits CuFe2O4 as an electrocatalytic membrane cathode, which can achieve rapid removal and mineralization of organic pollutants in water. It is suitable for the treatment of coexistence of multiple pollutants, micropollutants, etc., and can reduce environmental risks. The ceramic membrane has a porous structure with abundant micro-nanopores inside. Studies have shown that in a confined space, mass transfer between active free radicals and pollutants can be achieved, thereby improving the efficiency of electrocatalytic treatment. However, the double-sided electrocatalytic membrane prepared above only loads a conductive layer on both sides of the membrane, and does not fully utilize the porous structure advantages of the ceramic membrane. At the same time, the conductive layer is loaded by sputtering, which makes it difficult to achieve large-scale production. Chinese patent CN202111120600.8 discloses a method for preparing a ceramic-based carbon nanotube composite membrane, which uses ceramic as a substrate and adopts a series of operations such as solvent dispersion, filtration coating, solvent cleaning, and high-temperature treatment to obtain a ceramic-based carbon nanotube composite membrane. The membrane combines the catalytic and conductive properties of carbon nanotubes with the pressure resistance and permeability of ceramic membranes, and can be used as an electrocatalytic oxidation electrode in a variety of water treatment processes. However, the composite membrane only has single-sided conductivity.

[0004] In summary, it is of great significance to provide an electroactive ceramic membrane with many active sites to significantly improve the membrane's electrocatalytic ability and anti-pollution ability. Summary of the invention

[0005] The purpose of the present invention is to overcome the problems existing in the prior art and to provide an integral electroactive ceramic membrane and a preparation method and application thereof.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing an integral electroactive ceramic membrane, comprising the following steps:

[0008] (1) mixing tetrabutyl titanate with an alcohol solvent to obtain a solution a; mixing diethanolamine with water to obtain a solution b;

[0009] (2) passing solution a through the ceramic membrane to obtain a first ceramic membrane; passing solution b through the first ceramic membrane to obtain a second ceramic membrane;

[0010] (3) Repeating step (2) to obtain a ceramic membrane containing an active ingredient; the number of repetitions is ≥ 0 times; sintering the ceramic membrane containing the active ingredient to obtain a ceramic membrane loaded with TiO2;

[0011] (4) Under a hydrogen atmosphere, the ceramic membrane loaded with TiO2 is reduced to obtain the integral electroactive ceramic membrane.

[0012] Preferably, the alcohol solvent in step (1) is ethanol, and the volume ratio of tetrabutyl titanate to the alcohol solvent is 0.5-1.5:4.5-5.5;

[0013] The volume ratio of the diethanolamine to water is 9.5-10.5:0.5-1.5.

[0014] Preferably, the pore size of the ceramic membrane in step (2) is 50 to 500 nm.

[0015] Preferably, in step (2), the pressure of solution a flowing through the ceramic membrane is 0.2 to 0.5 bar, the flow rate of solution a flowing through the ceramic membrane is 0.4 to 0.8 m / s, and the duration of solution a flowing through the ceramic membrane is 10 to 20 min.

[0016] Preferably, in step (2), the pressure of solution b flowing through the first ceramic membrane is 0.5-1.0 bar, the flow rate of solution b flowing through the first ceramic membrane is 1-3 m / s, and the duration of solution b flowing through the ceramic membrane is 5-10 min.

[0017] Preferably, the number of repetitions in step (3) is 1 to 5 times.

[0018] Preferably, the sintering temperature in step (3) is 400-800° C., and the sintering time is 4-6 hours.

[0019] Preferably, the reduction temperature in step (4) is 900-1350° C., the reduction time is 4-8 h, and the reduction hydrogen flow rate is 100-120 mL / min.

[0020] The present invention also provides an integral electroactive ceramic membrane prepared by the method for preparing the integral electroactive ceramic membrane.

[0021] The invention also provides application of the integral electroactive ceramic membrane in wastewater treatment.

[0022] The beneficial effects of the present invention are:

[0023] The present invention provides a method for preparing an integral electroactive ceramic membrane, comprising the following steps: mixing tetrabutyl titanate with an alcohol solvent to obtain a solution a; mixing diethanolamine with water to obtain a solution b; circulating solution a through a ceramic membrane to obtain a first ceramic membrane; circulating solution b through the first ceramic membrane to obtain a second ceramic membrane; repeating the above process to obtain a ceramic membrane containing active ingredients; sintering the ceramic membrane containing active ingredients to obtain a ceramic membrane loaded with TiO2; reducing the ceramic membrane loaded with TiO2 under a hydrogen atmosphere to obtain an integral electroactive ceramic membrane. The present invention utilizes the porous structure of the ceramic membrane, takes the ceramic membrane as a base membrane, synthesizes a TiO2 loading layer in situ on the surface of the ceramic membrane and in the membrane pores by a sol-sol method, and then prepares a Ti4O7 loading layer by high-temperature hydrogen reduction. The integral electroactive ceramic membrane prepared by the present invention has a conductive layer uniformly loaded on the surface and in the pores, which can provide more electrochemically active sites, utilize the confined space inside the membrane, and achieve gradient degradation of organic pollutants when passing through the membrane, which can significantly improve the removal efficiency of pollutants and reduce membrane pollution. In addition, the present invention can also control the thickness and morphology of the loading layer through reasonable regulation of conditions, so that the overall electroactive ceramic membrane is suitable for different organic industrial wastewater application scenarios. DETAILED DESCRIPTION

[0024] The present invention provides a method for preparing an integral electroactive ceramic membrane, comprising the following steps:

[0025] (1) mixing tetrabutyl titanate with an alcohol solvent to obtain a solution a; mixing diethanolamine with water to obtain a solution b;

[0026] (2) passing solution a through the ceramic membrane to obtain a first ceramic membrane; passing solution b through the first ceramic membrane to obtain a second ceramic membrane;

[0027] (3) Repeating step (2) to obtain a ceramic membrane containing an active ingredient; the number of repetitions is ≥ 0 times; sintering the ceramic membrane containing the active ingredient to obtain a ceramic membrane loaded with TiO2;

[0028] (4) Under a hydrogen atmosphere, the ceramic membrane loaded with TiO2 is reduced to obtain the integral electroactive ceramic membrane.

[0029] In the present invention, the alcohol solvent in step (1) is preferably ethanol, and the volume ratio of tetrabutyl titanate to the alcohol solvent is preferably 0.5-1.5:4.5-5.5, more preferably 0.7-1.3:4.7-5.3, and more preferably 1:5.

[0030] In the present invention, the volume ratio of diethanolamine to water is preferably 9.5-10.5:0.5-1.5, more preferably 9.7-10.3:0.7-1.3, and more preferably 10:1.

[0031] In the present invention, the ceramic membrane in step (2) is purchased, and the material of the ceramic membrane is preferably Al2O3, ZrO2, TiO2 or SiC. The type of the ceramic membrane is preferably a plate membrane, a single-channel tubular membrane or a multi-channel tubular membrane. The pore size of the ceramic membrane is preferably 50 to 500 nm, more preferably 100 to 400 nm, and more preferably 200 to 300 nm.

[0032] In the present invention, in step (2), the pressure of solution a flowing through the ceramic membrane is preferably 0.2 to 0.5 bar, more preferably 0.25 to 0.45 bar, and more preferably 0.3 to 0.4 bar; the flow rate of solution a flowing through the ceramic membrane is preferably 0.4 to 0.8 m / s, more preferably 0.5 to 0.7 m / s, and more preferably 0.6 m / s; the duration of solution a flowing through the ceramic membrane is preferably 10 to 20 min, more preferably 12 to 18 min, and more preferably 15 to 16 min.

[0033] In the present invention, in step (2), the pressure of solution b flowing through the first ceramic membrane is preferably 0.5-1.0 bar, more preferably 0.6-0.9 bar, more preferably 0.7-0.8 bar; the flow rate of solution b flowing through the first ceramic membrane is preferably 1-3 m / s, more preferably 1.5-2.5 m / s, more preferably 2 m / s; the duration of solution b flowing through the ceramic membrane is preferably 5-10 min, more preferably 6-9 min, more preferably 7-8 min.

[0034] In the present invention, after step (2), the obtained second ceramic membrane is dried, and then step (3) is performed; the drying temperature is preferably 25 to 35°C, more preferably 27 to 33°C, and more preferably 30°C; the drying time is preferably 20 to 30h, more preferably 24 to 28h, and more preferably 26h.

[0035] In the present invention, the number of repetitions in step (3) is preferably 1 to 5 times, more preferably 2 to 4 times, and even more preferably 3 times.

[0036] In the present invention, in step (3), each time step (2) is repeated, the obtained membrane needs to be dried once, that is, the process of "step (2)-drying" is repeated. After the repetition, a ceramic membrane containing active ingredients is obtained; the drying temperature is preferably 25-35°C, more preferably 27-33°C, and more preferably 30°C; the drying time is preferably 20-30h, more preferably 24-28h, and more preferably 26h.

[0037] In the present invention, the sintering temperature in step (3) is preferably 400-800°C, more preferably 500-700°C, and more preferably 600-650°C; the sintering time is preferably 4-6h, more preferably 4.5-5.5h, and more preferably 4.7-5h.

[0038] In the present invention, the reduction temperature in step (4) is preferably 900-1350°C, more preferably 950-1300°C, and more preferably 1100-1150°C; the reduction time is preferably 4-8h, more preferably 5-7h, and more preferably 6-6.5h; the reduction hydrogen flow rate is preferably 100-120mL / min, more preferably 105-115mL / min, and more preferably 110mL / min.

[0039] The present invention also provides an integral electroactive ceramic membrane prepared by the method for preparing the integral electroactive ceramic membrane.

[0040] The invention also provides application of the integral electroactive ceramic membrane in wastewater treatment.

[0041] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0042] Example 1

[0043] Tetrabutyl titanate was mixed with ethanol (the volume ratio of tetrabutyl titanate to ethanol was 1:5) to obtain solution a; diethanolamine was mixed with water (the volume ratio of diethanolamine to water was 10:1) to obtain solution b; a ZrO2 single-channel tubular membrane with a pore size of 200 nm was selected as a ceramic membrane, and solution a was passed through the ceramic membrane at a pressure of 0.3 bar and a flow rate of 0.5 m / s for 15 minutes to obtain a first ceramic membrane; then, solution b was passed through the first ceramic membrane at a pressure of 0.8 bar and a flow rate of 2 m / s for 15 minutes. 8min to obtain a second ceramic membrane; the second ceramic membrane obtained is dried at 30°C for 24h; the above process (flowing solution a through the ceramic membrane, flowing solution b through the first ceramic membrane and drying) is repeated 3 times to obtain a ceramic membrane containing active ingredients; the ceramic membrane containing active ingredients is sintered at 400°C in an air atmosphere for 5h to obtain a ceramic membrane loaded with TiO2; finally, the ceramic membrane loaded with TiO2 is reduced at 950°C in a hydrogen atmosphere for 6h, and the hydrogen flow rate is set to 100mL / min to obtain the integral electroactive ceramic membrane.

[0044] The integral electroactive ceramic membrane prepared in this embodiment is used to remove aniline from printing and dyeing wastewater. The initial wastewater COD is 48 mg / L, and the aniline concentration is 5 mg / L. The integral electroactive ceramic membrane is used as the anode and the titanium mesh is used as the cathode. Under the conditions of an operating pressure of 1 bar, a cross-flow filtration mode, and a voltage of 3 V, the test shows that the stable COD removal rate reaches 84.3%, and the aniline removal rate reaches 100%.

[0045] Example 2

[0046] Tetrabutyl titanate was mixed with ethanol (the volume ratio of tetrabutyl titanate to ethanol was 1:5) to obtain solution a; diethanolamine was mixed with water (the volume ratio of diethanolamine to water was 10:1) to obtain solution b; an Al2O3 plate membrane with a pore size of 50 nm was selected as a ceramic membrane, and solution a was passed through the ceramic membrane at a pressure of 0.5 bar and a flow rate of 0.8 m / s for 20 min to obtain a first ceramic membrane; then, solution b was passed through the first ceramic membrane at a pressure of 1.0 bar and a flow rate of 3 m / s for 10 min to obtain a second ceramic membrane; drying the obtained second ceramic membrane at 30°C for 26h; repeating the above process (flowing solution a through the ceramic membrane, flowing solution b through the first ceramic membrane and drying) twice, drying the obtained membrane at 30°C for 48h to obtain a ceramic membrane containing active ingredients; sintering the ceramic membrane containing active ingredients at 800°C in an air atmosphere for 6h to obtain a ceramic membrane loaded with TiO2; finally, reducing the ceramic membrane loaded with TiO2 at 1300°C in a hydrogen atmosphere for 8h, setting the hydrogen flow rate to 120mL / min, to obtain the integral electroactive ceramic membrane.

[0047] The integral electroactive ceramic membrane prepared in this embodiment is used to treat biochemical tail water in a comprehensive sewage treatment plant in a chemical park. The initial wastewater COD is 98 mg / L. The integral electroactive ceramic membrane is used as the anode and the titanium mesh is used as the cathode. Under the conditions of an operating pressure of 2 bar, a cross-flow filtration mode, and a voltage of 5 V, the test shows that the stable COD removal rate reaches 68.4%.

[0048] Example 3

[0049] Tetrabutyl titanate was mixed with ethanol (the volume ratio of tetrabutyl titanate to ethanol was 1:5) to obtain solution a; diethanolamine was mixed with water (the volume ratio of diethanolamine to water was 10:1) to obtain solution b; a SiC multi-channel tubular membrane with a membrane pore size of 500 nm was selected as a ceramic membrane, and solution a was passed through the ceramic membrane at a pressure of 0.2 bar and a flow rate of 0.4 m / s for 10 minutes to obtain a first ceramic membrane; then, solution b was passed through the first ceramic membrane at a pressure of 0.5 bar and a flow rate of 1 m / s for 5 minutes to obtain a second ceramic membrane; drying the obtained second ceramic membrane at 30°C for 30h; repeating the above process (flowing solution a through the ceramic membrane, flowing solution b through the first ceramic membrane and drying) for 5 times, drying the obtained membrane at 30°C for 48h to obtain a ceramic membrane containing active ingredients; sintering the ceramic membrane containing active ingredients at 500°C in an air atmosphere for 4h to obtain a ceramic membrane loaded with TiO2; finally, reducing the ceramic membrane loaded with TiO2 at 1150°C in a hydrogen atmosphere for 4h, setting the hydrogen flow rate to 110mL / min, to obtain the integral electroactive ceramic membrane.

[0050] The integral electroactive ceramic membrane prepared in this embodiment was used for the deep treatment of biochemical tail water of printing and dyeing wastewater from a sewage treatment plant. The initial wastewater COD was 102 mg / L. The integral electroactive ceramic membrane was used as the anode and the titanium mesh was used as the cathode. Under the conditions of an operating pressure of 1 bar, a cross-flow filtration mode, and a voltage of 4 V, the test showed that the stable COD removal rate reached 72.5%.

[0051] It can be seen from the above embodiments that the present invention provides a method for preparing an integral electroactive ceramic membrane, comprising the following steps: mixing tetrabutyl titanate with an alcohol solvent to obtain a solution a; mixing diethanolamine with water to obtain a solution b; circulating solution a through a ceramic membrane to obtain a first ceramic membrane; circulating solution b through the first ceramic membrane to obtain a second ceramic membrane; repeating the above process to obtain a ceramic membrane containing active ingredients; sintering the ceramic membrane containing active ingredients to obtain a ceramic membrane loaded with TiO2; reducing the ceramic membrane loaded with TiO2 in a hydrogen atmosphere to obtain an integral electroactive ceramic membrane. The present invention utilizes the porous structure of the ceramic membrane, takes the ceramic membrane as the base membrane, synthesizes a TiO2 loading layer in situ on the surface of the ceramic membrane and in the membrane pores by a sol-sol method, and then prepares a Ti4O7 loading layer by high-temperature hydrogen reduction. The surface and pores of the overall electroactive ceramic membrane prepared by the present invention are uniformly loaded with a conductive layer, which can provide more electrochemical active sites, and utilize the confined space inside the membrane to achieve gradient degradation of organic pollutants when passing through the membrane, which can significantly improve the removal efficiency of pollutants and reduce membrane pollution. In addition, the present invention can also control the thickness and morphology of the load layer through reasonable regulation of conditions, so that the overall electroactive ceramic membrane is suitable for different organic industrial wastewater application scenarios.

[0052] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing an integral electroactive ceramic membrane, characterized in that: It includes the following steps: (1) mixing tetrabutyl titanate with an alcohol solvent to obtain a solution a; mixing diethanolamine with water to obtain a solution b; (2) passing solution a through the ceramic membrane to obtain a first ceramic membrane; passing solution b through the first ceramic membrane to obtain a second ceramic membrane; (3) Repeating step (2) to obtain a ceramic membrane containing an active ingredient; the number of repetitions is ≥ 0 times; sintering the ceramic membrane containing the active ingredient to obtain a ceramic membrane loaded with TiO2; (4) In a hydrogen atmosphere, the ceramic membrane loaded with TiO2 is reduced to obtain the integral electroactive ceramic membrane.

2. The method for preparing the integral electroactive ceramic membrane according to claim 1, characterized in that: In step (1), the alcohol solvent is ethanol, and the volume ratio of tetrabutyl titanate to the alcohol solvent is 0.5-1.5:4.5-5.5; The volume ratio of the diethanolamine to water is 9.5-10.5:0.5-1.

5.

3. The method for preparing the integral electroactive ceramic membrane according to claim 1 or 2, characterized in that: The pore size of the ceramic membrane in step (2) is 50 to 500 nm.

4. The method for preparing the integral electroactive ceramic membrane according to claim 3, characterized in that: In step (2), the pressure of solution a flowing through the ceramic membrane is 0.2 to 0.5 bar, the flow rate of solution a flowing through the ceramic membrane is 0.4 to 0.8 m / s, and the duration of solution a flowing through the ceramic membrane is 10 to 20 min.

5. The method for preparing the integral electroactive ceramic membrane according to claim 4, characterized in that: In step (2), the pressure of solution b flowing through the first ceramic membrane is 0.5-1.0 bar, the flow rate of solution b flowing through the first ceramic membrane is 1-3 m / s, and the duration of solution b flowing through the ceramic membrane is 5-10 min.

6. The method for preparing the integral electroactive ceramic membrane according to claim 5, characterized in that: The number of repetitions in step (3) is 1 to 5 times.

7. The method for preparing the integral electroactive ceramic membrane according to claim 6, characterized in that: The sintering temperature in step (3) is 400-800° C. and the sintering time is 4-6 hours.

8. The method for preparing the integral electroactive ceramic membrane according to claim 7, characterized in that: The reduction temperature of step (4) is 900-1350° C., the reduction time is 4-8 h, and the reduction hydrogen flow rate is 100-120 mL / min.

9. An integral electroactive ceramic membrane prepared by the method for preparing an integral electroactive ceramic membrane according to any one of claims 1 to 8.

10. Use of the integral electroactive ceramic membrane according to claim 9 in wastewater treatment.

Citation Information

Patent Citations

  • Dye-sensitized Zn2TiO4 nano-crystalline film for solar cell and preparation method of film

    CN106024398A

  • Preparation method of Ti4O7 ceramic electrode

    CN113416070A

  • Preparation method of p-nitrophenol hydrogenation Co (at) CM multichannel ceramic catalytic membrane

    CN117181003A

  • Preparation method of titanium black ceramic membrane electrode and water purification membrane electrode reactor thereof

    CN117550686A

  • Titanium Sub-oxide / Ruthenium Oxide Composite Electrode And Preparation Method And Application Thereof

    US20200208282A1