Silica-aluminum cementing material, preparation method and application thereof, and raw material processing system
By designing a raw material treatment system for silicon-aluminum gelling materials, treating coal gangue and red mud, and combining alkaline excitants, the problems of industrial solid waste resource utilization and environmental impact are solved, and the preparation and low production of high-strength building materials are achieved. Carbon and environmentally friendly effect.
Patent Information
- Application Number
- CN202411155159.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-19
AI Technical Summary
The environmental impact of industrial solid waste such as coal gangue and red mud is increasingly serious, and it is difficult for existing technologies to achieve their large-scale resource utilization, especially when preparing efficient building materials.
A raw material treatment system for silicon-aluminum gelling materials is designed, including homogenization, drying and calcining and grinding systems. Coal gangue and red mud are treated through crushing, homogenization, drying, calcining, cooling and crushing. Combined with alkaline exciters, high-strength silicon-aluminum gelling material is prepared.
It has achieved resource utilization of large amounts of industrial solid waste, significantly reduced carbon emissions, provided high-strength building materials, with wide applicability and economic and environmental benefits.
Smart Images

Figure CN118978351A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building materials, and in particular relates to a silicon-aluminum gelling material, a preparation method and application thereof, and a raw material processing system. Background Art
[0002] With the continuous development of the economy and the continuous expansion of industrialization, the adverse effects of large solid wastes such as coal gangue and red mud on the environment cannot be ignored. Realizing the large-scale resource utilization of these industrial solid wastes is the key to the metallurgical industry's transformation to a green circular economy. The consumption of building materials is huge, and industrial solid wastes such as red mud and coal gangue with silicon, aluminum, oxygen and other main elements can be used to prepare silicon-aluminum low-carbon cementitious materials, which is a good way to utilize them. Summary of the invention
[0003] Therefore, the object of the present invention is to provide a silica-alumina gelling material, a preparation method and application thereof, and a raw material processing system. The silica-alumina gelling material can consume a large amount of coal gangue and red mud and has excellent compressive strength.
[0004] To this end, the present invention provides the following technical solutions.
[0005] The present invention provides a raw material processing system for silicon-aluminum gelling material, comprising a homogenizing system, a feeding system, a drying and calcining system, and a grinding system which are arranged in sequence; the homogenizing system comprises a crushing device and a homogenizing device which are connected in sequence; the feeding system comprises a fuel feeding system and a raw material feeding system; the fuel feeding system comprises a screening device, a metering device, and a storage device, wherein the screening device is located at the starting end of the fuel feeding system; the raw material feeding system comprises a metering device and a storage device; the drying and calcining system comprises a drying device, a calcining device, and a cooling device which are connected in sequence; the grinding system comprises a crushing device and a powder selection device which are connected in sequence; the drying device comprises 1 to 9 drying devices connected in parallel; the cooling device comprises 1 to 9 cooling devices connected in series; when the number of cooling devices is greater than 1, the temperature of each cooling device decreases in sequence along the raw material transportation direction.
[0006] Optionally, the drying device includes a drying room; a drying series reamer may be provided in the drying room.
[0007] Optionally, the calcining device includes a rotary kiln calcining furnace.
[0008] Optionally, a burner is used to provide heat for the rotary kiln calcining furnace.
[0009] Optionally, the calcining device is provided with a smoke chamber, which is located at the end of the calcining device and is used to collect hot air generated in the raw material processing system and use it to heat the calcining device; the hot air generated in the raw material processing system can be hot air from a drying room.
[0010] Optionally, the cooling device includes a water-cooled jacketed reamer conveyor.
[0011] Optionally, a raw material storage device is further provided between the drying device and the calcining device for storing the dried raw materials.
[0012] Optionally, a metering device is provided at the discharge port of the raw material storage device.
[0013] Optionally, a hot gas outlet is provided on the raw material storage device, and the hot gas outlet is connected to the calcining device to provide heat for the calcining device, thereby achieving full utilization of thermal energy in the system.
[0014] Optionally, a calcined product storage device is further provided between the cooling device and the crushing device for storing the calcined raw materials.
[0015] Optionally, a metering device is provided at the discharge port of the calcined product storage device.
[0016] Optionally, the pulverizing device includes a tube mill, which is filled with grinding bodies, which are common grinding bodies, such as steel ball grinding bodies. As the tube mill runs, the grinding media and materials form a multi-dimensional orderly circulation activity under the action of friction, gravity and centrifugal force, and the media, the media and materials, and the media and the inner wall of the mill grind each other, which can effectively crush the materials. The tube mill is provided with an air inlet, an air outlet, and a manhole; the air inlet is provided with a cooling valve for controlling the air volume entering the tube mill; the air outlet of the tube mill is connected to the powder selection equipment to guide the hot air into the powder selection equipment; at the same time, the air inlet and air outlet of the tube mill are also used for unloading the material after grinding and ventilation in the mill; the manhole facilitates the replacement of the grinding body.
[0017] Optionally, a metering device is provided at the discharge port of the pulverizing device.
[0018] Optionally, the pulverizing device is provided with an air supply device to help supply the required air volume to the powder selection device.
[0019] In the raw material processing system of the silicon-alumina gelling material provided by the present invention, the qualification degree of the material can be adjusted according to the engineering requirements when selecting the powder, and specifically, the particle size of the selected material can be adjusted by controlling the air volume of the fan.
[0020] Optionally, a collecting device is included after the powder selection device.
[0021] Optionally, the collecting device includes a dust collector.
[0022] Optionally, a final product storage device is included after the powder selection device.
[0023] Optionally, the final product storage device includes 1 to 9 final product storage devices connected in parallel.
[0024] Optionally, the final product storage device includes a final product storage bin.
[0025] Optionally, the powder selection device is connected to the feed port of the pulverizing device, and unqualified materials are returned to the pulverizing device for re-pulverization.
[0026] Optionally, the grinding system includes a pneumatic conveying system connected thereto.
[0027] Optionally, the pneumatic conveying system includes a conveying pump, a fan, and a material distribution valve connected in sequence.
[0028] Optionally, the blower includes a Roots blower.
[0029] Optionally, the starting end of the raw material feeding system includes a feeding device for lifting the raw material from the homogenizing device.
[0030] Optionally, the feeding device includes a feeding grab bucket.
[0031] Optionally, the raw materials are transferred between the devices via a conveying device.
[0032] Optionally, the transmission device includes at least one of a belt conveyor, a reamer conveyor, an elevator, a chute conveyor, and a pipe conveyor; a suitable transmission device or a combination of transmission devices can be adaptively selected according to the positional relationship of each device in the entire system and the state of the material being transmitted.
[0033] Optionally, the metering device includes at least one of a metering scale, a punch plate flow meter, and a metering bin; a suitable metering device can be selected according to the adaptability of the setting of the lines in the entire system.
[0034] Optionally, a dust collecting device and / or a fan is provided on the transmission device; optionally, a dust collecting device and / or a fan is provided on the drying device; these are used to reduce the escape of dust into the outside air during the working process.
[0035] Optionally, a dust collecting device and / or a fan is provided on the final product storage device, which can not only reduce the escape of dust into the outside air during the working process, but also help unloading, aeration and homogenization of the product.
[0036] The present invention provides a silica-alumina gelling material, comprising a base material and an alkaline activator. The base material comprises the following raw materials in percentage by weight: 30-70% of calcined coal gangue, 0-30% of red mud, 0-30% of steel slag, 0-40% of cement clinker, 0-40% of gypsum, and 0-10% of carbide slag; wherein the red mud is calcined red mud or uncalcined red mud.
[0037] Optionally, when added externally, the mass of the alkaline activator is less than 11% of the mass of the base material, calculated as Na2O.
[0038] Optionally, the alkaline activator includes at least one of sodium carbonate, sodium silicate and sodium hydroxide.
[0039] Preferably, the alkaline activator is sodium carbonate and sodium silicate in a mass ratio of 1-8:2-9; this alkaline activator combination can better promote the reaction between the cementitious components and further improve the flexural strength and compressive strength of the cement.
[0040] Preferably, the base material comprises the following raw materials in percentage by weight: 40-70% of calcined coal gangue, 10-30% of red mud, 5-20% of steel slag, 0-30% of cement clinker, 5-30% of gypsum and 1-2% of carbide slag.
[0041] Optionally, the calcined coal gangue includes, by mass percentage: Al2O3>20%, CaO<5%, SO3<5%, Al / Si>0.5; Optionally, the calcined coal gangue includes, by mass percentage, Al2O3>25%, and the 28-day compressive strength activity index of the calcined coal gangue is>85%; Further optionally, the calcined coal gangue includes, by mass percentage: Al2O3: 30%~40%, SiO2: 40%~65%, K2O+Na2O≤3%, CaO+ MgO ≤5%, SO3<3%, and the 28-day compressive strength activity index is>95%.
[0042] Optionally, in the red mud, calculated by mass percentage: Al2O3≥6.0%, SiO2≥10.0%, and the 28-day compressive strength activity index of the red mud is>60%; Optionally, the red mud includes, by mass percentage, Al2O3: 8.0%~25%, SiO2: 15.0%~30%, Fe2O3: 5%~15%, CaO: 5%~50%, MgO: 0.1%~2%, K2O: 0.001%~1%, Na2O: 2%~8%, SO3≤5%; the red mud is selected from sintered red mud and / or Bayer red mud.
[0043] Optionally, the steel slag includes, by mass percentage, the following components: CaO: 30%~60%, SiO2: 10%~30%, MgO: 2%~20%, Fe2O3: 10%~40%; Optionally, the steel slag includes, by mass percentage, the following components: CaO: 38%~50%, Fe2O3: 25%~35%, SiO2: 14%~20%, MgO: 4.5%~12%, Al2O3: 1%~10%, MnO≤5%, CaF2≤2%, SO3≤5%.
[0044] Optionally, the cement clinker includes Portland cement clinker, which complies with the requirements of GB / T 21372 "Portland cement clinker".
[0045] Optionally, the gypsum includes at least one of desulfurized gypsum, mirabilite gypsum, phosphogypsum and titanium gypsum.
[0046] Optionally, the carbide slag includes, by mass percentage, the following components: CaO: 65%~98%, SiO2: 1%~10%, Al2O3: 0%~5%, Fe2O3: 0%~10%; Optionally, the carbide slag includes, by mass percentage, the following components: CaO: 90%~98%, Fe2O3: 0%~3%, SiO2: 1%~5%, Al2O3: 0%~3%, MgO≤1%, MnO≤1%, CaF2≤1%, SO3≤1%.
[0047] The present invention also provides a method for preparing the above-mentioned silica-alumina gelling material, comprising the following steps: mixing the raw materials according to weight percentage to obtain the base material, adding the alkaline activator to obtain the silica-alumina gelling material; or, mixing the raw materials and the alkaline activator according to weight percentage to obtain the silica-alumina gelling material.
[0048] Optionally, the step of drying the raw materials is also included before the preparation.
[0049] Optionally, after obtaining the base material and adding the alkaline activator or mixing the raw materials and the alkaline activator, a grinding step is further included; optionally, after grinding, a step of screening out particles with a particle size of ≤45 μm for standby use is also included; during grinding, the residue on the 45 μm negative pressure sieve does not exceed 10%.
[0050] Optionally, the calcined coal gangue and the calcined red mud are obtained by processing the raw material processing system of the above-mentioned silica-alumina gelling material; optionally, the fuel used in the preparation includes biofuel.
[0051] Optionally, the heating rate of the calcined coal gangue during calcination is 1-50°C / min, the calcination temperature is 600-1000°C, and the insulation time is 0-60min.
[0052] Optionally, the heating rate of the calcined red mud during calcination is 1-50°C / min, the calcination temperature is 600-1000°C, and the insulation time is 0-60min.
[0053] The present invention also provides the use of the above-mentioned silicon-aluminum gelling material, or the silicon-aluminum gelling material prepared by the above-mentioned preparation method in building materials.
[0054] The beneficial effects of the present invention are: The raw material processing system of silicon-aluminum gelling material provided by the present invention comprises a homogenizing system, a feeding system, a drying and calcining system, and a grinding system which are arranged in sequence; the homogenizing system comprises a crushing device and a homogenizing device which are connected in sequence; the feeding system comprises a fuel feeding system and a raw material feeding system; the fuel feeding system comprises a screening device, a metering device, and a storage device, wherein the screening device is located at the starting end of the fuel feeding system; the raw material feeding system comprises a metering device and a storage device; the drying and calcining system comprises a drying device, a calcining device, and a cooling device which are connected in sequence; the grinding system comprises a crushing device and a powder selection device which are connected in sequence; the drying device comprises 1 to 9 parallel drying devices; the cooling device comprises 1 to 9 series cooling devices; when the number of cooling devices is greater than 1, the temperature of each cooling device decreases in sequence along the raw material transportation direction. Through the raw material processing system, raw materials which can be directly applied to the preparation of silicon-aluminum gelling material can be obtained, which is convenient for the large-scale industrial preparation of silicon-aluminum gelling material.
[0055] The silicon-alumina gelling material provided by the present invention comprises a base material and an alkaline activator. The base material comprises the following raw materials in terms of weight percentage: 30-70% of calcined coal gangue, 0-30% of red mud, 0-30% of steel slag, 0-40% of cement clinker, 0-40% of gypsum, and 0-10% of carbide slag; wherein the red mud is calcined red mud or uncalcined red mud. The silicon-alumina gelling material has fast strength formation, high final strength, and a wide range of applications; at the same time, it can consume a large amount of solid waste coal gangue and red mud to realize their resource utilization, and can significantly reduce carbon emissions while ensuring that the quality of the gelling material product remains unchanged; it can bring economic and environmental benefits, has strong practicality, and is suitable for popularization and use.
[0056] The method for preparing the above-mentioned silicon-aluminum gelling material provided by the present invention comprises mixing raw materials by weight percentage to obtain the base material, adding the alkaline activator to obtain the silicon-aluminum gelling material; or mixing the raw materials of the base material and the alkaline activator by weight percentage to obtain the silicon-aluminum gelling material. The preparation method is simple, low in cost, energy-saving, low-carbon and environmentally friendly. BRIEF DESCRIPTION OF THE DRAWINGS
[0057] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0058] Figure 1 It is a schematic diagram of a raw material processing system of the silicon-alumina gelling material of the present invention; Figure 2 It is a schematic diagram of a homogenizing system in a raw material processing system of a silicon-alumina gelling material of the present invention; Figure 3 It is a schematic diagram of a feeding system in a raw material processing system of a silicon-alumina gelling material of the present invention; Figure 4 It is a schematic diagram of a drying and calcining system in a raw material processing system of a silicon-alumina gelled material of the present invention; Figure 5 It is a schematic diagram of a grinding system in a raw material processing system of a silicon-alumina gelled material of the present invention.
[0059] Description of reference numerals: 1-crusher; 2-belt conveyor; 3-raw material homogenizing warehouse; 4-feeding grab bucket; 5-fuel powder screen; 6-pipe belt conveyor; 7-raw material metering warehouse; 8-drying room; 9-raw material storage warehouse; 10-reamer conveyor; 11-elevator; 12-burner; 13-rotary kiln calcining furnace; 14-water-cooled jacketed reamer conveyor; 15-calcined finished product storage warehouse; 16-tube mill; 17-powder selector; 18-dust collector; 19-chute conveyor; 20-weighing scale; 21-punch flowmeter; 22-Roots blower; 23-conveyor pump; 24-first final product storage warehouse; 25-fuel metering warehouse; 26-second final product storage warehouse; 27-third final product storage warehouse. DETAILED DESCRIPTION
[0060] The technical solution of the present invention will be described clearly and completely below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0061] In the description of the present invention, it should be noted that the terms "center", "upper", "lower", "left", "right", "vertical", "horizontal", "inner", "outer", etc., indicating the orientation or positional relationship, are based on the orientation or positional relationship shown in the drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the present invention. In addition, the terms "first", "second", and "third" are used for descriptive purposes only, and cannot be understood as indicating or implying relative importance.
[0062] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be indirectly connected through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0063] Example 1 Reference below Figure 1 , 2 , 3, 4, and 5 describe the raw material processing system of the silica-alumina gelling material according to an embodiment of the present invention.
[0064] The raw material processing system of silicon-alumina gelling material provided by the embodiment of the present invention comprises: a homogenizing system, a feeding system, a drying and calcining system, and a grinding system which are arranged in sequence; the homogenizing system comprises a crushing device and a homogenizing device which are connected in sequence; the feeding system comprises a fuel feeding system and a raw material feeding system; the fuel feeding system comprises a screening device, a metering device, and a storage device, wherein the screening device is located at the starting end of the fuel feeding system; the raw material feeding system comprises a metering device and a storage device; the drying and calcining system comprises a drying device, a calcining device, and a cooling device which are connected in sequence; the grinding system comprises a crushing device and a powder selection device which are connected in sequence; the drying device comprises 1 to 9 drying devices connected in parallel; the cooling device comprises 1 to 9 cooling devices connected in series; when the number of cooling devices is greater than 1, the temperature of each cooling device decreases in sequence along the raw material transportation direction; the raw materials are transferred between the devices through a transmission device. When processing the raw materials of silicon-alumina gelling material, the raw materials are first passed into a homogenizing device for homogenization. The homogenized raw materials pass through a metering device and a storage device in turn. After being weighed, they are delivered to a drying device for drying. Finally, they are passed into a calcining device for calcination. After being cooled by a cooling device, they are passed into a pulverizing device for pulverization. The powder with a qualified particle size is selected by a powder selection device.
[0065] In some embodiments, the drying device is a drying room 8; a drying series reamer may be provided in the drying room 8.
[0066] In some embodiments, the calcining device is a rotary kiln calcining furnace 13 , and a matching burner 12 can be used to provide heat for the rotary kiln calcining furnace 13 .
[0067] In some embodiments, a smoke chamber is provided on the calcining device. The smoke chamber is located at the end of the calcining device and is used to collect hot air generated in the raw material processing system and use it to provide heat for the calcining device.
[0068] In some embodiments, the cooling device is a water-cooled jacketed reamer conveyor 14 .
[0069] In some embodiments, a raw material storage device is further included between the drying device and the calcining device for storing the dried raw materials.
[0070] In some embodiments, a metering device is provided at the discharge port of the raw material storage device to weigh the mass of the raw materials passing through.
[0071] In some embodiments, a hot gas outlet is provided on the raw material storage device, and the hot gas outlet is connected to the calcining device to provide heat for the calcining device, thereby achieving full utilization of thermal energy in the system.
[0072] In some embodiments, a calcined product storage device is further provided between the cooling device and the crushing device for storing the calcined raw materials.
[0073] In some embodiments, a metering device is provided at the discharge port of the calcined product storage device to weigh the mass of the calcined product passing through.
[0074] In some embodiments, the crushing device is a tube mill 16, and the tube mill 16 is filled with grinding bodies. In a non-limiting manner, the grinding bodies are common grinding bodies, such as steel ball grinding bodies. As the tube mill 16 operates, the grinding media and the materials form a multi-dimensional orderly circulation activity under the action of friction, gravity and centrifugal force, and the media, the media and the materials, and the media and the inner wall of the mill grind each other, which can effectively crush the materials. The tube mill 16 is provided with an air inlet, an air outlet, and a manhole; the air inlet is provided with a cooling valve for controlling the air volume entering the tube mill 16; the air outlet of the tube mill 16 is connected to the powder selection equipment to guide the hot air into the powder selection equipment; at the same time, the air inlet and air outlet of the tube mill 16 are also used for unloading the material after grinding and ventilation in the mill; the manhole facilitates the replacement of the grinding body.
[0075] In some embodiments, a metering device is provided at the discharge port of the pulverizing device for weighing the mass of the pulverized product passing through.
[0076] In some embodiments, the pulverizing device is provided with an air supply device to help supply the required air volume to the powder selection device.
[0077] In some embodiments, a collecting device is included after the powder selecting device; the collecting device includes a dust collector 18.
[0078] In some embodiments, a final product storage device is included after the powder selection device; the final product storage device includes 1 to 9 final product storage devices connected in parallel; the final product storage device includes a final product storage bin.
[0079] In some embodiments, the powder selection device is connected to the feed port of the pulverizing device, and unqualified materials are returned to the pulverizing device for re-pulverization.
[0080] In some embodiments, the grinding system includes a pneumatic conveying system connected thereto; the pneumatic conveying system includes a conveying pump 23, a fan, and a material distribution valve connected in sequence.
[0081] In some embodiments, the blower includes a Roots blower 22 .
[0082] In some embodiments, the starting end of the raw material feeding system includes a feeding device for lifting the raw material from the homogenizing device; the feeding device includes a feeding grab 4.
[0083] In some embodiments, a dust collecting device and / or a fan is provided on the transmission device to reduce the escape of dust into the outside air during operation.
[0084] In some embodiments, a dust collecting device and / or a fan is provided on the drying device to reduce the escape of dust into the outside air during operation.
[0085] In some embodiments, a dust collecting device and / or a fan is provided on the final product storage device, which can not only reduce the escape of dust into the outside air during the working process, but also help unloading, aeration and homogenization of the product.
[0086] The transmission device mentioned above includes at least one of a belt conveyor 2, a reamer conveyor 10, an elevator 11, a chute conveyor 19, and a pipe conveyor 6; in different embodiments, a suitable transmission device or a combination of transmission devices can be adaptively selected according to the positional relationship of each device in the entire system and the state of the material being transmitted.
[0087] The metering device mentioned above includes at least one of a metering scale 20, a punch plate flow meter 21, and a metering bin; in different embodiments, a suitable metering device can be selected according to the adaptability of the setting of the lines in the entire system.
[0088] Embodiments 2 to 27 This embodiment provides a silica-alumina gelling material and a preparation method thereof. The processing system in Embodiment 1 is used to calcine the raw materials to be calcined. Biofuel is used during calcination. The processing system includes: A homogenization system, a feeding system, a drying and calcining system, and a grinding system are arranged and connected in sequence; wherein the homogenization system includes a crusher 1 and a raw material homogenization warehouse 3 connected in sequence; the feeding system includes a parallel fuel feeding system and a raw material feeding system, and the raw material feeding system includes a feeding grab 4, a raw material metering warehouse 7 and a pipe conveyor 6 connected in sequence; the drying and calcining system includes a drying room 8, a raw material storage warehouse 9, a rotary kiln calcining furnace 13, and a water-cooled jacketed auger conveyor 14 connected in sequence; the grinding system includes a calcined finished product storage warehouse 15, a tube mill 16, a powder selector 17, a dust collector 18, and a final product storage warehouse connected in sequence. The particle size of the raw material passing through the crusher 1 is ≤45mm. The drying room 8 includes three parallel drying rooms, each of which is provided with a drying series auger. The rotary kiln calcining furnace 13 also includes a matching burner 12 for supplying heat to the rotary kiln calcining furnace 13. The water-cooled jacketed auger conveyor 14 includes three sets of water-cooled jacketed auger conveyors whose temperatures decrease in sequence along the material transport direction; the temperature range is 30° C. to -30° C. The final product storage warehouse includes a first final product storage warehouse 24, a second final product storage warehouse 26, and a third final product storage warehouse 27 connected in parallel.
[0089] The feeding system further includes a fuel powder screen 5 , a pipe conveyor 6 , and a fuel metering bin 25 which are connected in sequence; the discharge port of the fuel metering bin 25 is connected to the fuel feed port of the rotary kiln calcining furnace 13 .
[0090] The raw material feeding port and the crusher 1, the crusher 1 and the raw material homogenizing silo 3, the feeding grab 4 and the raw material metering bin 7, and the fuel feeding port and the fuel powder screen 5 are connected by belt conveyors 2. The raw materials are transported to the raw material feeding port and the fuel is transported to the fuel feeding port by a feeding vehicle.
[0091] The discharge port of the drying room 8 is connected to the feed port of the raw material storage bin 9 through a reamer conveyor 10 and an elevator 11 which are arranged in sequence.
[0092] The discharge port of the raw material storage bin 9 is connected to the feed port of the rotary kiln calcining furnace 13 through a reamer conveyor 10 and an elevator 11 which are arranged in sequence.
[0093] A weighing scale 20 is also provided behind the discharge port of the raw material storage bin 9 for weighing the discharge amount. The material passes through the discharge port of the raw material storage bin 9 and then passes through the weighing scale 20 and enters the feed port of the rotary kiln calcining furnace 13 .
[0094] The raw material storage bin 9 is provided with a hot gas outlet, which is communicated with the burner 12 to provide part of the heat for the burner 12 .
[0095] The rotary kiln calcining furnace 13 is provided with a kiln tail smoke chamber, and the hot air in the processing system enters the rotary kiln calcining furnace 13 through the kiln tail smoke chamber, runs in the kiln together with the calcined material and performs heat exchange; the hot air in the processing system is mainly the hot air generated in the drying room 8.
[0096] A weighing scale 20 is provided behind the discharge port of the calcined product storage bin 15 for weighing the discharge amount. The material passes through the weighing scale 20 from the discharge port of the calcined product storage bin 15 and then enters the feed port of the tube mill 16 .
[0097] The tube mill 16 is filled with steel ball grinding bodies. As the tube mill 16 runs, the grinding media and the materials form a multi-dimensional orderly circulation activity under the action of friction, gravity and centrifugal force. The media, the media and the materials, and the media and the inner wall of the mill grind each other, which can effectively crush the materials. The tube mill 16 is provided with an air inlet, an air outlet, a supplementary air valve, and a manhole; the air inlet of the tube mill 16 is provided with a cooling valve, which is used to control the air volume entering the tube mill 16 by the size of the valve opening; the air outlet of the tube mill 16 is connected to the powder selector 17 to guide the hot air into the powder selector 17; at the same time, the air inlet and air outlet of the tube mill 16 are also used for unloading the ground materials and ventilating the mill; the manhole is convenient for the replacement of the grinding body; the supplementary air valve can be used to supplement the air volume required by the powder selector 17.
[0098] The qualified material discharge port of the powder selector 17 is connected with the feed port of the dust collector 18, and the qualified material (particle size ≤ 45μm) is transported to the dust collector 18 along with the airflow; the unqualified material discharge port of the powder selector 17 is connected with the feed port of the tube mill 16 through the chute conveyor 19 and the punch plate flowmeter 21 which are arranged in sequence, and the unqualified material (particle size > 45μm) is returned to the tube mill 16 for re-grinding.
[0099] The grinding system includes a pneumatic conveying system connected thereto, and the pneumatic conveying system is used for material conveying. The pneumatic conveying system includes a conveying pump 23, a Roots blower 22, and a material dividing valve connected in sequence; the material dividing valve is used to control the final product to enter the first final product storage warehouse 24, the second final product storage warehouse 26, or the third final product storage warehouse 27.
[0100] The second final product storage warehouse 26 and the third final product storage warehouse 27 are respectively connected to the Roots blower 22 and the dust collector 18, and the first final product storage warehouse 24 is connected to the Roots blower 22 for unloading, aeration of the product warehouse and homogenization of the product.
[0101] The drying room 8 and the elevator 11 in the drying and calcining system and the elevator 11 in the grinding system are respectively connected with a Roots blower 22 and a dust collector 18 to reduce the escape of dust into the outside air.
[0102] The specific preparation method comprises the following steps: The gangue is processed by using the above-mentioned processing system. First, the gangue is passed into the raw material homogenization bin 3 for homogenization; the homogenized gangue is taken out through the loading grab 4, and passes through the raw material metering bin 7 and the pipe conveyor 6 in turn to the drying room 8 for drying, and then passed into the raw material storage bin 9 for standby; the standby gangue in the raw material storage bin 9 is transported to the rotary kiln calcining furnace 13, and the heating rate is 30°C / min. After the heating rate reaches 750°C, the gangue is kept warm for 10 minutes for calcination. After the calcination is completed, the calcined gangue is passed through a water-cooled jacket reamer The conveyor 14 is cooled and then passed into the calcined finished product storage bin 15 for standby; the calcined coal gangue for standby in the calcined finished product storage bin 15 is passed into the tube mill 16 for grinding and then transported to the powder classifier 17, and the qualified calcined coal gangue powder is transported to the dust collector 18 along with the airflow, and the unqualified calcined coal gangue powder is returned to the tube mill 16 for further grinding. The calcined coal gangue powder after passing through the dust collector 18 is passed into the first final product storage bin 24, or the second final product storage bin 26, or the third final product storage bin 27 for standby.
[0103] The raw materials are mixed according to the ratio given in Table 1 to obtain a base material, and an alkaline activator is prepared. The base material and the alkaline activator are mixed and ground into a powder with a 45μm negative pressure sieve residue of no more than 10%, thereby obtaining a silica-alumina cementitious material. The chemical composition (%) and 28-day compressive strength activity index of the calcined coal gangue used are shown in Table 2, the chemical composition (%) of the sintered red mud used is shown in Table 3, the chemical composition (%) of the steel slag used is shown in Table 4, the cement clinker used is a silicate cement clinker that meets the requirements of GB / T 21372 "Silicate Cement Clinker", and its chemical composition (%) is shown in Table 5, the chemical composition (%) of the desulfurized gypsum used is shown in Table 6, and the chemical composition (%) of the calcium carbide slag used is shown in Table 7.
[0104] Table 1
[0105] Table 2
[0106] Table 3
[0107] Table 4
[0108] Table 5
[0109] Table 6
[0110] Table 7
[0111] Comparative Examples 1 to 6 This comparative example provides a silica-alumina gelling material, which differs from Example 2 in the raw material ratio and the amount of alkaline activator used. The specific amount is shown in Table 1.
[0112] Test Example 1 The silicon-alumina cementitious materials obtained in the embodiments and comparative examples were mixed and molded according to the provisions of GB / T17671-1999 "Test method for strength of cement mortar (ISO method)", and cured in water: the mortar specimens were demoulded after being cured in a curing box at 20℃±2℃ and a relative humidity of not less than 90% for 1 day. The demoulded specimens were placed in water at 20℃±1℃ for curing for 28 days, and the compressive strength was tested. See Table 8.
[0113] Table 8
[0114] It can be seen from Table 8 that compared with the comparative examples in which the amounts of each raw material are not within the range specified in the present application, the silicon-alumina cementitious material obtained in the embodiments in which the amounts of each raw material are within the range specified in the present application has a fast strength formation, a high final strength and a better application effect.
[0115] Test Example 2 The silica-alumina cementitious material obtained in the example was tested for its setting time and stability according to the "Test Method for Water Consistency, Setting Time and Stability of Cement Standard Consistency" (GB / T1346-2011). The data are shown in Table 9. The results all meet the requirements of the national standard GB175-2020 for cement. Table 9
[0116] It can be seen from Table 9 that the silica-alumina cementitious materials obtained in the examples of the present application have good stability. Although the setting time in some examples is relatively long, they can still meet the standards for use in actual engineering.
[0117] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. A raw material processing system for silicon-alumina gelling material, characterized in that: It includes a homogenizing system, a feeding system, a drying and calcining system, and a grinding system which are arranged in sequence; The homogenization system comprises a crushing device and a homogenization device which are connected in sequence; The feeding system includes a fuel feeding system and a raw material feeding system; the fuel feeding system includes a screening device, a metering device, and a storage device, wherein the screening device is located at the starting end of the fuel feeding system; the raw material feeding system includes a metering device and a storage device; The drying and calcining system comprises a drying device, a calcining device and a cooling device which are connected in sequence; The grinding system comprises a pulverizing device and a powder selecting device which are connected in sequence; The drying device comprises 1 to 9 drying devices connected in parallel; The cooling device comprises 1 to 9 cooling devices connected in series; when the number of cooling devices is greater than 1, the temperature of each cooling device decreases in sequence along the raw material transportation direction.
2. The material processing system according to claim 1, characterized in that: The drying device comprises a drying room; And / or, the calcining device comprises a rotary kiln calcining furnace; optionally, a burner is used to supply heat to the rotary kiln calcining furnace; And / or, the calcining device is provided with a smoke chamber, which is located at the end of the calcining device and is used to collect hot air generated in the raw material processing system and use it to heat the calcining device; and / or, the cooling device comprises a water-cooled jacketed reamer conveyor; And / or, a raw material storage device is further included between the drying device and the calcining device, for storing the dried raw materials; optionally, a metering device is provided at the discharge port of the raw material storage device; optionally, a hot air outlet is provided on the raw material storage device, and the hot air outlet is connected to the calcining device; And / or, a calcined product storage device is further included between the cooling device and the pulverizing device, for storing the calcined raw materials; Optionally, a metering device is provided at the discharge port of the calcined product storage device; and / or, the comminution device comprises a tube mill; And / or, a metering device is provided at the discharge port of the pulverizing device; And / or, the pulverizing device is provided with an air supply device; And / or, a collecting device is included after the powder selection device; optionally, the collecting device includes a dust collector; And / or, a final product storage device is included after the powder selection device; optionally, the final product storage device includes 1 to 9 final product storage devices connected in parallel; optionally, the final product storage device includes a final product storage bin; And / or, the powder selection device is connected to the feed port of the pulverizing device, and unqualified materials are returned to the pulverizing device for re-pulverization; And / or, the grinding system includes a pneumatic conveying system connected thereto; optionally, the pneumatic conveying system includes a conveying pump, a blower, and a material distribution valve connected in sequence; optionally, the blower includes a Roots blower; And / or, the starting end of the raw material feeding system includes a feeding device for lifting the raw material from the homogenizing device; optionally, the feeding device includes a feeding grab; And / or, the raw materials are transferred between the various devices through a transmission device; optionally, the transmission device includes at least one of a belt conveyor, a reamer conveyor, an elevator, a chute conveyor, and a pipe belt conveyor.
3. The material processing system according to claim 2, characterized in that: The metering device includes at least one of a metering scale, a punch plate flow meter, and a metering bin; and / or, a dust collecting device and / or a fan is provided on the transmission device; and / or, a dust collecting device and / or a fan is provided on the drying device; And / or, a dust collecting device and / or a fan is provided on the final product storage device.
4. A silicon-alumina gelling material, characterized in that: It includes a base material and an alkaline activator. The base material includes the following raw materials in percentage by weight: 30-70% of calcined coal gangue, 0-30% of red mud, 0-30% of steel slag, 0-40% of cement clinker, 0-40% of gypsum, and 0-10% of carbide slag; wherein the red mud is calcined red mud or uncalcined red mud.
5. The silicon-alumina gelling material according to claim 4, characterized in that: The alkaline activator includes at least one of sodium carbonate, sodium silicate and sodium hydroxide; optionally, the alkaline activator is sodium carbonate and sodium silicate in a mass ratio of 1-8:2-9; and / or, when added externally, the mass of the alkaline activator is less than 11% of the mass of the base material, calculated as Na2O; And / or, in terms of weight percentage, the base material comprises the following raw materials: 40-70% calcined coal gangue, 10-30% red mud, 5-20% steel slag, 0-30% cement clinker, 5-30% gypsum and 1-2% carbide slag.
6. The silicon-alumina gelling material according to claim 4 or 5, characterized in that: The calcined coal gangue includes, by mass percentage: Al2O3>20%, CaO<5%, SO3<5%, Al / Si>0.5; Optionally, the calcined coal gangue includes, by mass percentage, Al2O3>25%, and the 28-day compressive strength activity index of the calcined coal gangue is>85%; Further optionally, the calcined coal gangue includes, by mass percentage: Al2O3: 30%~40%, SiO2: 40%~65%, K2O+Na2O≤3%, CaO+MgO≤5%, SO3<3%, and the 28-day compressive strength activity index is>95%; And / or, in the red mud, by mass percentage: Al2O3≥6.0%, SiO2≥10.0%, and the red mud 28-day compressive strength activity index>60%; Optionally, the red mud includes, by mass percentage, Al2O3: 8.0%~25%, SiO2: 15.0%~30%, Fe2O3: 5%~15%, CaO: 5%~50%, MgO: 0.1%~2%, K2O: 0.001%~1%, Na2O: 2%~8%, SO3≤5%; And / or, the steel slag comprises, by mass percentage: CaO: 30%-60%, SiO2: 10%-30%, MgO: 2%-20%, Fe2O3: 10%-40%; Optionally, the steel slag comprises, by mass percentage: CaO: 38%-50%, Fe2O3: 25%-35%, SiO2: 14%-20%, MgO: 4.5%-12%, Al2O3: 1%-10%, MnO≤5%, CaF2≤2%, SO3≤5%; And / or, the cement clinker comprises Portland cement clinker; And / or, the gypsum includes at least one of desulfurized gypsum, mirabilite gypsum, phosphogypsum and titanium gypsum; And / or, the carbide slag includes, by mass percentage, the following: CaO: 65%~98%, SiO2: 1%~10%, Al2O3: 0%~5%, Fe2O3: 0%~10%; Optionally, the carbide slag includes, by mass percentage, the following: CaO: 90%~98%, Fe2O3: 0%~3%, SiO2: 1%~5%, Al2O3: 0%~3%, MgO≤1%, MnO≤1%, CaF2≤1%, SO3≤1%.
7. A method for preparing the silicon-alumina gelling material according to any one of claims 4 to 6, characterized in that: The method comprises the following steps: mixing the raw materials according to weight percentage to obtain the base material, adding the alkaline activator to obtain the silica-alumina gelling material; or mixing the raw materials and the alkaline activator according to weight percentage to obtain the silica-alumina gelling material.
8. The preparation method according to claim 7, characterized in that: The method also includes the step of drying the raw materials before the preparation; And / or, after obtaining the base material, adding the alkaline activator or mixing the raw materials and the alkaline activator, a grinding step is further included; optionally, after grinding, a step of screening out particles with a particle size of ≤45 μm for standby use is also included.
9. The preparation method according to claim 7 or 8, characterized in that: The calcined coal gangue and the calcined red mud are obtained by processing the raw material processing system of the silica-alumina gelling material according to any one of claims 1 to 3; optionally, the fuel used in the preparation includes biofuel; And / or, the calcined coal gangue has a heating rate of 1-50°C / min, a calcination temperature of 600-1000°C, and a holding time of 0-60min during calcination; And / or, the calcined red mud has a heating rate of 1-50°C / min, a calcination temperature of 600-1000°C, and a holding time of 0-60min during calcination.
10. Use of the silica-alumina cementitious material according to any one of claims 4 to 6, or the silica-alumina cementitious material prepared by the preparation method according to any one of claims 7 to 9 in building materials.