Alkali-activated soil stabilizer and preparation method thereof

By using alkali-exciting combination materials in soil curing agents, the curing effect and durability of the slag are improved, the environmental pollution problem of large cement consumption is solved, and efficient and environmentally friendly soil curing is achieved.

CN118978373AActive Publication Date: 2024-11-19CHANGCHUN URBAN CONSTR & MAINTENANCE GRP CO LTD

Patent Information

Application Number
CN202411041627.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

When treating engineering slag, a large amount of cement is required to cause high alkalinity and environmental pollution. The cured slag is insufficient durability, which cannot effectively reduce the amount of cement and reduce the greenhouse effect.

Method used

Using alkali-excited soil curing agents, including cement, mineral blends, alkaline exciters, wollastonite powder, fiber and modified chitosan, improve material activity through calcination, grinding, ultrasonic treatment and other means to increase the alkali-excited effect and gel network polymerization degree, combined with modified chitosan and curing additives, form a dense structure to improve compressive strength.

Benefits of technology

Soil has achieved good curing effect, reduced cement usage, improved soil hardness and compressive strength after curing, and was environmentally friendly and reduced greenhouse effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004972532750000081
    Figure BDA0004972532750000081
Patent Text Reader

Abstract

The invention belongs to the field of building materials, and particularly relates to an alkali-activated soil stabilizer and a preparation method thereof, the alkali-activated soil stabilizer comprises the following raw materials by weight: 20-25 parts of cement, 70-80 parts of a mineral admixture, 13-16 parts of an alkali activator, 4-8 parts of wollastonite powder, 0.3-0.8 part of fiber, and 3-7 parts of modified chitosan. The alkali-activated soil stabilizer obtained by the invention is suitable for engineering residue soil, has a good curing effect, is environment-friendly and has good ecological benefits, and the use amount of cement is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of building materials, and particularly relates to an alkali-activated soil solidifying agent and a preparation method thereof. Background Art

[0002] There are a large number of underground projects in the process of urban construction, which will generate a large amount of construction waste. Most of the abandoned construction waste is piled up beside urban rivers, depressions, vacant land, etc., or even on planned land. This treatment method occupies a large amount of land resources. In addition, the random stacking of waste is prone to cause landslides, collapses, mudslides and other hazards. In the stacking process, a large amount of construction waste that cannot be used for engineering backfill is mixed with soil that can be used for engineering backfill without any treatment, resulting in the failure to reasonably utilize the construction waste that can be utilized as a resource, increasing social costs. The traditional method of treating construction waste is to solidify it with cement. This treatment method requires a large amount of cement. Due to the strong alkalinity of cement, the solidified engineering waste mud and waste have high alkalinity. At the same time, the production of cement is a high-energy-consuming process. The firing of cement clinker requires a large amount of fossil energy. These fossil energy sources will emit a large amount of polluting gases and CO into the atmosphere during the combustion process. 2 , which aggravates the greenhouse effect. Therefore, environmentally friendly soil solidifiers that can reduce cement consumption have become the research focus in this field.

[0003] Patent CN115806417B discloses a construction slag solidifying agent, which uses construction slag, desulfurization ash, industrial by-product gypsum, slag powder and other solid wastes as components of the solidifying agent, and rationally utilizes waste resources. The aluminum oxide in the slag powder accelerates the conversion of calcium sulfate in the desulfurization ash to ettringite. 2 O 3 、SiO 2 The curing agent can improve the mechanical properties of construction waste by using components such as iron tailings, slag, desulfurized gypsum powder, lime powder, and polycarboxylic acid high-efficiency water reducing agent. Although the curing agent can realize the reuse of waste, it still needs to use a large amount of cement, which aggravates the greenhouse effect. Patent CN113620655B discloses a curing agent for the base material of the water-stabilized layer of tailings-based construction waste, which is composed of iron tailings slurry, slag powder, desulfurized gypsum powder, lime powder, and polycarboxylic acid high-efficiency water reducing agent. The curing agent has good consolidation performance for construction waste with high mud content, and realizes the comprehensive utilization of resources and reduces construction costs. In order to reduce the amount of water used, the invention needs to add a water reducing agent, which may cause the durability of the solidified waste to decrease.

[0004] Therefore, there is an urgent need to prepare a soil solidifying agent that reduces cement usage, is environmentally friendly, and has good durability of solidified slag. Summary of the invention

[0005] In order to overcome the above-mentioned deficiencies of the prior art, the present invention provides an environmentally friendly alkali-activated soil solidifier which is applicable to a variety of soils, has good solidification effect, and reduces cement usage.

[0006] In order to achieve the above object, the technical solution adopted by the present invention is:

[0007] The first aspect of the present invention provides an alkali-activated soil solidifier, which comprises the following raw materials by weight: 20-25 parts of cement, 70-80 parts of mineral admixtures, 13-16 parts of alkaline activator, 4-8 parts of wollastonite powder, 0.3-0.8 parts of fiber, and 3-7 parts of modified chitosan.

[0008] In some embodiments, the cement includes one or more of ordinary Portland cement, aluminate cement, and sulphoaluminate cement.

[0009] Preferably, the cement is 42.5 ordinary Portland cement.

[0010] In some embodiments, the mineral admixture includes one or more of coal gangue powder, slag, silica fume, and steel slag powder.

[0011] Preferably, the mineral admixtures are coal gangue powder and slag, with a mass ratio of 1:(0.8-1.1).

[0012] Further preferably, the coal gangue powder is activated coal gangue powder, and the preparation method of activated coal gangue powder comprises the following steps: placing coal gangue with a particle size less than 5 mm in a rapid heating box-type electric furnace, calcining at a temperature of 450-550°C for 2-3 hours, cooling to room temperature, and then grinding the calcined coal gangue with a ball mill, passing through an 8-8.5μm sieve, to obtain activated coal gangue powder.

[0013] The invention activates the coal gangue by means of calcination and grinding, thereby improving the volcanic ash activity of the material and enhancing the alkali excitation effect.

[0014] In some embodiments, the alkaline activator is CaO, Ca(OH) 2 , NaOH, Na 2 SO 4 、Na 2 CO 3 , water glass or more.

[0015] Preferably, the alkaline activator is NaOH and Na 2 CO 3 , the mass ratio is 1:(0.9-1.2).

[0016] In some embodiments, the wollastonite powder has a particle size of 500-900 mesh.

[0017] Preferably, the particle size of the wollastonite powder is 800 mesh.

[0018] Further preferably, the wollastonite powder is purified wollastonite powder, and the preparation method of purified wollastonite powder comprises the following steps: subjecting the wollastonite powder to ultrasonic treatment, the ultrasonic time is 4-6 minutes, the ultrasonic power is 100-250W, and then the ultrasonicated wollastonite powder is calcined at 600-800°C for 2-3 hours, and purified wollastonite powder is obtained after filtration, washing and drying.

[0019] The present invention uses ultrasound and calcination to treat wollastonite powder, providing sufficient silicon source and calcium source for the reaction system, increasing the amount of active silicon in the system, and effectively increasing the initial silicon-aluminum ratio and the number of Si-O-Si bonds. Under alkaline conditions, the active calcium content in the system increases, and calcium ions react with Si(OH) 4 、Al(OH) 4 - The monomers combine to form CSH and CASH gels, which promote gel formation, increase the degree of polymerization of the gel network, make the structure denser, and help enhance the compressive strength.

[0020] In some embodiments, the fiber is one or more of corn straw fiber, polypropylene fiber and basalt fiber.

[0021] Preferably, the fiber is corn stover fiber.

[0022] Further preferably, the corn straw fiber is pretreated corn straw fiber, and the pretreatment steps are: soaking the corn straw fiber in 2-3wt% NaOH solution for 30-40min, then washing the straw fiber with water until neutral, and drying at 75-85°C to obtain pretreated corn straw fiber.

[0023] The invention adopts alkali activation to pretreat the straw fiber, solves the shortcomings of traditional soil solidifiers such as high brittleness and low toughness, and improves the bending strength and tensile strength of the solidified soil.

[0024] In some embodiments, the preparation method of the modified chitosan comprises the following steps: stirring acrylic acid and 2,4-hexadien-1-ol at a constant temperature of 70-80°C for 1-2 hours, then adding chitosan, toluene and concentrated sulfuric acid and stirring at a constant temperature of 60-70°C for 5-6 hours, and drying to obtain the modified chitosan.

[0025] In some embodiments, the mass ratio of acrylic acid, 2,4-hexadien-1-ol, and chitosan is (2.8-3):1:(0.8-1.2).

[0026] The present invention adds polymers to the soil, utilizes the steric shielding effect of organic polymer materials, reduces the adsorbed water in the soil, improves the soil's anti-permeability, forms a dense structure when the soil is compacted and formed to ensure good compressive strength, and improves the engineering properties of the soil. The applicant polymerizes acrylic acid and 2,4-hexadiene-1-ol, and then grafts it with chitosan. On the one hand, the gel property of chitosan is utilized to accelerate the solidification of sludge, and on the other hand, the dispersibility of chitosan in water is improved, the internal hardness unevenness after soil solidification is reduced, and the compressive resistance is enhanced. The possible reason is that by limiting the mass ratio of acrylic acid, 2,4-hexadiene-1-ol, and chitosan, the modified chitosan is still a hydrophobic structure, which is conducive to water loss during compaction, is not easy to enter the soil, reduces the pores in the soil, makes the solidified soil more resistant to compression and is not easy to crack, and the double bonds and hydroxyl groups on the chain segments can be complexed with metal ions in the soil, enhance the curing agent and the soil to form a whole to form a cementation, and make the soil more solidified.

[0027] In some embodiments, the alkali-activated soil solidifier further comprises 0.8-1.2 parts by weight of a solidification aid.

[0028] In some embodiments, the method for preparing the curing aid comprises the following steps: adding pentaerythritol and triphenylmethane triisocyanate into DMF, reacting at 60-70° C. for 5-6 hours, rotary evaporating, and drying to obtain the curing aid.

[0029] The present invention prepares a curing aid, which contains multiple isocyanate groups and benzene rings in one molecular structure. On the one hand, it increases the hardness of the cured soil, and on the other hand, it can cross-link with modified chitosan to form a dense network structure to accelerate soil curing. At the same time, the isocyanate group reacts with water to produce carbon dioxide, which makes Ca(OH) 2 Converted to CaCO 3 , while CaCO 3 The solid phase volume is larger than Ca(OH) 2 , thereby reducing the pores in the soil and further improving the density of the soil after solidification.

[0030] In some embodiments, the mass ratio of pentaerythritol to triphenylmethane triisocyanate is 1:(11-14).

[0031] The invention limits the mass ratio of pentaerythritol to triphenylmethane triisocyanate, so that the hydroxyl groups of pentaerythritol can react completely on the one hand, and on the other hand, a large amount of free triphenylmethane triisocyanate is provided so that each hydroxyl group of pentaerythritol reacts with a single triphenylmethane triisocyanate.

[0032] The second aspect of the present invention provides a method for preparing an alkali-activated soil solidifier, comprising the following steps: mixing cement, mineral admixtures, wollastonite powder, fiber and modified chitosan for 10-15 minutes, then adding an alkaline activator and continuing to stir for 20-30 minutes to obtain the soil solidifier.

[0033] Compared with the prior art, the present invention has the following beneficial effects:

[0034] 1. The present invention obtains an alkali-activated soil solidifier by adding modified chitosan and a solidifying aid, which has a good solidifying effect. The solidified soil has a higher hardness and compressive strength, while reducing the amount of cement used and being environmentally friendly.

[0035] 2. The present invention polymerizes acrylic acid and 2,4-hexadiene-1-ol and then grafts them with chitosan. On the one hand, the gel property of chitosan is used to accelerate the solidification of sludge. On the other hand, the dispersibility of chitosan in water is improved, the uneven hardness of the soil after solidification is reduced, and the compression resistance is enhanced.

[0036] 3. The curing aid prepared by the present invention contains multiple isocyanate groups in one molecular structure, which cross-link with modified chitosan to form a dense network structure to accelerate soil curing. At the same time, the isocyanate groups react with water to produce carbon dioxide, making Ca(OH) 2 Converted to CaCO 3 , while CaCO 3 The solid phase volume is larger than Ca(OH) 2 , thereby reducing the pores in the soil and further improving the density of the soil after solidification. DETAILED DESCRIPTION

[0037] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following examples and comparative examples are examples of the present invention and are only used to illustrate the present invention, but not to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.

[0038] In order to facilitate those skilled in the art to implement the present invention, some raw materials and manufacturers of the embodiments and comparative examples are described as follows: the compounds and related reagents used in the present invention can be purchased from the market.

[0039] Preparation Example 1

[0040] The preparation method of activated coal gangue powder comprises the following steps: placing 10 g of coal gangue with a particle size of less than 5 mm in a fast heating box-type electric furnace, calcining at a temperature of 500° C. for 2.5 hours, cooling to room temperature, and then grinding the calcined coal gangue with a ball mill, passing through an 8.5 μm square hole sieve to obtain activated coal gangue powder.

[0041] Preparation Example 2

[0042] The preparation method of purified wollastonite powder comprises the following steps: subjecting the wollastonite powder to ultrasonic treatment, wherein the ultrasonic time is 5 minutes and the ultrasonic power is 200W, then calcining the ultrasonicated wollastonite powder at 700°C for 2.5 hours, and obtaining the purified wollastonite powder after filtration, washing and drying.

[0043] Preparation Example 3

[0044] The pretreated corn straw fiber comprises the following steps: soaking 5 g corn straw fiber in 100 ml 2 wt % NaOH solution for 35 min, then washing the straw fiber with water until the pH value of the solution is 7, and drying at 80° C. to obtain the pretreated corn straw fiber.

[0045] Preparation Example 4

[0046] The preparation method of modified chitosan-1 comprises the following steps: 2.9g acrylic acid and 1g 2,4-hexadiene-1-ol are stirred at 75°C for 1.5h, 1g chitosan, 50ml toluene and 0.5ml concentrated sulfuric acid are added, stirred at 65°C for 5.5h, and dried to obtain modified chitosan-1.

[0047] Preparation Example 5

[0048] The preparation method of modified chitosan-2 comprises the following steps: 3.5g acrylic acid and 1g 2,4-hexadiene-1-ol are stirred at 75°C for 1.5h, 1g chitosan, 50ml toluene and 0.5ml concentrated sulfuric acid are added, stirred at 65°C for 5.5h, and dried to obtain modified chitosan-2.

[0049] Preparation Example 6

[0050] The preparation method of modified chitosan-3 comprises the following steps: 2.9g acrylic acid and 1g 2,4-hexadiene-1-ol are stirred at 75°C for 1.5h, 2g chitosan, 50ml toluene and 0.5ml concentrated sulfuric acid are added, stirred at 65°C for 5.5h, and dried to obtain modified chitosan-3.

[0051] Preparation Example 7

[0052] The preparation method of curing aid-1 comprises the following steps: adding 1g of pentaerythritol and 12g of triphenylmethane triisocyanate into 20ml of DMF, reacting at 65°C for 5.5h, rotary evaporating, and drying to obtain curing aid-1.

[0053] Preparation Example 8

[0054] The preparation method of curing aid-2 comprises the following steps: adding 1g of pentaerythritol and 8g of triphenylmethane triisocyanate into 20ml of DMF, reacting at 65°C for 5.5h, rotary evaporating, and drying to obtain curing aid-2.

[0055] Example 1

[0056] An alkali-activated soil solidifier comprises the following raw materials, measured by weight: 23 parts of 42.5 ordinary Portland cement, 75 parts of mineral admixtures, 15 parts of alkaline activator, 6 parts of purified wollastonite powder, 0.5 parts of pretreated corn straw fiber, and 5 parts of modified chitosan-1.

[0057] The mineral admixture is activated coal gangue powder and slag, with a mass ratio of 1:1; the alkaline activator is NaOH and Na 2 CO 3 , the mass ratio is 1:1.

[0058] The preparation method of the alkali-activated soil solidifier of this embodiment comprises the following steps: 42.5 ordinary Portland cement, mineral admixture, purified wollastonite powder, pretreated corn straw fiber and modified chitosan-1 are mixed and stirred for 13 minutes, and then an alkaline activator is added and stirred for 25 minutes to obtain the soil solidifier.

[0059] Example 2

[0060] An alkali-activated soil solidifier comprises the following raw materials, measured by weight: 20 parts of 42.5 ordinary Portland cement, 70 parts of mineral admixtures, 13 parts of alkaline activator, 4 parts of purified wollastonite powder, 0.3 parts of pretreated corn straw fiber, and 3 parts of modified chitosan-1.

[0061] The mineral admixture is activated coal gangue powder and slag, with a mass ratio of 1:0.8; the alkaline activator is NaOH and Na 2 CO 3 , the mass ratio is 1:0.9.

[0062] The preparation method of the alkali-activated soil solidifier of this embodiment comprises the following steps: 42.5 ordinary Portland cement, mineral admixture, purified wollastonite powder, pretreated corn straw fiber and modified chitosan-1 are mixed and stirred for 10 minutes, and then an alkaline activator is added and stirred for 30 minutes to obtain the soil solidifier.

[0063] Example 3

[0064] An alkali-activated soil solidifier comprises the following raw materials, measured by weight: 25 parts of 42.5 ordinary Portland cement, 80 parts of mineral admixtures, 16 parts of alkaline activator, 8 parts of purified wollastonite powder, 0.8 parts of pretreated corn straw fiber, and 7 parts of modified chitosan-1.

[0065] The mineral admixture is activated coal gangue powder and slag, with a mass ratio of 1:1.1; the alkaline activator is NaOH and Na 2 CO 3 , the mass ratio is 1:1.2.

[0066] The preparation method of the alkali-activated soil solidifier of this embodiment comprises the following steps: 42.5 ordinary Portland cement, mineral admixture, purified wollastonite powder, pretreated corn straw fiber and modified chitosan-1 are mixed and stirred for 15 minutes, and then an alkaline activator is added and stirred for 20 minutes to obtain the soil solidifier.

[0067] Example 4

[0068] An alkali-activated soil solidifier comprises the following raw materials, measured by weight: 23 parts of 42.5 ordinary Portland cement, 75 parts of mineral admixtures, 15 parts of alkaline activator, 6 parts of purified wollastonite powder, 0.5 parts of pretreated straw fiber, 5 parts of modified chitosan-1, and 1 part of curing aid-1.

[0069] The mineral admixture is activated coal gangue powder and slag, with a mass ratio of 1:1; the alkaline activator is NaOH and Na 2 CO 3 , the mass ratio is 1:1.

[0070] The preparation method of the alkali-activated soil solidifier of this embodiment comprises the following steps: 42.5 ordinary Portland cement, mineral admixture, purified wollastonite powder, pretreated corn straw fiber and modified chitosan-1 are mixed and stirred for 13 minutes, and then an alkaline activator and curing aid-1 are added and stirred for 25 minutes to obtain the soil solidifier.

[0071] Example 5

[0072] An alkali-activated soil solidifier and a preparation method thereof. The specific implementation manner is the same as that of Example 4, except that an equal amount of modified chitosan-1 is replaced by modified chitosan-2.

[0073] Example 6

[0074] An alkali-activated soil solidifier and a preparation method thereof. The specific implementation manner is the same as that of Example 4, except that an equal amount of modified chitosan-1 is replaced by modified chitosan-3.

[0075] Example 7

[0076] An alkali-activated soil solidifier and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 4, except that an equal amount of solidifying aid-1 is replaced by a solidifying aid-2.

[0077] Comparative Example 1

[0078] An alkali-activated soil solidifier and a preparation method thereof, wherein the specific implementation manner is the same as that of Example 4, except that an equal amount of modified chitosan-1 is replaced by chitosan.

[0079] Performance Testing

[0080] The soil sample used in the test is silty clay. The basic physical properties of the soil sample are shown in Table 1.

[0081] Table 1

[0082]

[0083] Take silty clay, add the soil solidifier in the above embodiments and comparative examples, the addition amount is 5wt% of the soil sample, make a Φ50cm×50cm cylindrical specimen, and compact it by static compaction at the optimal moisture content, the compaction degree is 95%, and according to JTG E51-2009 "Test Procedure for Stabilized Materials of Inorganic Binders for Highway Engineering" standard, cure for 7 days and 28 days, and test the unconfined compressive strength for 7 days and 28 days.

[0084] The test results are shown in Table 2.

[0085] Table 2

[0086] serial number 7d unconfined compressive strength / MPa 28d unconfined compressive strength / MPa Example 1 3.32 3.84 Example 2 3.08 3.31 Example 3 3.12 3.57 Example 4 3.81 3.98 Example 5 2.63 2.69 Example 6 2.35 2.86 Example 7 2.71 2.73 Comparative Example 1 1.53 1.81

[0087] From the data comparison of Examples 1-3 in Table 1, it can be seen that the base-activated soil solidifier has a good curing effect when the ratio of each material is changed; the addition of curing aid-1 in Example 4 accelerates soil curing and increases the compactness of the soil after curing; compared with Example 4, it can be seen that the amount of acrylic acid in the modified chitosan-2 increases, which may lead to an increase in water absorption during the curing process, the generation of pores, and a decrease in compressive performance; compared with Example 4, it can be seen that the amount of chitosan in the modified chitosan-3 increases, which may lead to a decrease in the dispersibility of the modified chitosan-3, resulting in uneven distribution during the curing process and a decrease in compressive strength; compared with Example 4, it can be seen that the triphenylmethane triisocyanate in the curing aid-2 decreases, resulting in a decrease in the degree of crosslinking and slowing down the Ca(OH) 2 Converted to CaCO 3 , the compressive strength decreases; comparison between Example 4 and Comparative Example 1 shows that the dispersibility of chitosan decreases and the compressive strength decreases.

[0088] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes using the technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. An alkali-activated soil solidifier, characterized in that: The raw materials include the following by weight: 20-25 parts of cement, 70-80 parts of mineral admixture, 13-16 parts of alkaline activator, 4-8 parts of wollastonite powder, 0.3-0.8 parts of fiber, and 3-7 parts of modified chitosan.

2. An alkali-activated soil solidifier according to claim 1, characterized in that: The cement includes one or more of ordinary Portland cement, aluminate cement, and sulphoaluminate cement.

3. The alkali-activated soil solidifying agent according to claim 1, characterized in that: The mineral admixture includes one or more of coal gangue powder, slag, silica fume and steel slag powder.

4. The alkali-activated soil solidifying agent according to claim 1, characterized in that: The alkaline activator is one or more of CaO, Ca(OH)2, NaOH, Na2SO4, Na2CO3, and water glass.

5. The alkali-activated soil solidifying agent according to claim 1, characterized in that: The fiber is one or more of corn straw fiber, polypropylene fiber, and basalt fiber.

6. The alkali-activated soil solidifying agent according to claim 1, characterized in that: The preparation method of the modified chitosan comprises the following steps: stirring acrylic acid and 2,4-hexadien-1-ol at a constant temperature of 70-80° C. for 1-2 hours, adding chitosan, toluene and concentrated sulfuric acid, stirring at a constant temperature of 60-70° C. for 5-6 hours, and drying to obtain the modified chitosan.

7. The alkali-activated soil solidifying agent according to claim 6, characterized in that: The mass ratio of the acrylic acid, 2,4-hexadien-1-ol and chitosan is (2.8-3):1:(0.8-1.2).

8. The alkali-activated soil solidifying agent according to claim 1, characterized in that: The alkali-activated soil solidifier further comprises 0.8-1.2 parts by weight of a solidification aid.

9. The alkali-activated soil solidifying agent according to claim 8, characterized in that: The preparation method of the curing auxiliary agent comprises the following steps: adding pentaerythritol and triphenylmethane triisocyanate into DMF, reacting at 60-70° C. for 5-6 hours, rotary evaporation, and drying to obtain the curing auxiliary agent.

10. A method for preparing the alkali-activated soil solidifying agent according to any one of claims 1 to 7, characterized in that: The method comprises the following steps: mixing cement, mineral admixture, wollastonite powder, fiber and modified chitosan and stirring for 10-15 minutes, then adding alkaline activator and continuing stirring for 20-30 minutes to obtain soil solidifying agent.

Citation Information

Patent Citations

  • Weak soil curing agent

    CN109369073A

  • Industrial solid waste-based spoil curing agent as well as preparation method and use method thereof

    CN117819845A

  • Novel collapsible loess curing agent and preparation and application thereof

    CN118271049A

  • Soil solidifying agent, soil paving material and method

    CN1614147A

Cited By

  • Frost-crack-resistant salinized soil curing agent based on nano material and preparation method thereof

    CN120647249A