Ceramic tile with holes in bottom surface and preparation method thereof

By designing an irregular hole structure of the combination of foaming powder and mullite-type powder at the bottom of the tile, the problem of low water absorption rate of the tile is solved, resulting in poor adhesion firmness, and the high strength and firm adhesion effect of the tile is achieved.

CN118978385AActive Publication Date: 2024-11-19FOSHAN DONGPENG CERAMIC +3
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411058330.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-19
Estimated Expiration
2044-08-02

AI Technical Summary

Technical Problem

Due to the low water absorption rate of existing ceramic tiles, the adhesion firmness is poor. The existing technology cannot effectively solve this problem by setting back shading on the bottom of the ceramic tiles.

Method used

Design a ceramic tile with holes on the bottom surface. By combining foaming powder and mullite-type powder, an irregular hole structure is formed to improve the adhesion firmness of the tile. The aluminum oxide content in the tile is 22% to 25 %, fracture modulus ≥47MPa, damage strength ≥2000N.

Benefits of technology

Through irregular hole structure and adhesive forming an inlaid mortise and tenon structure, the adhesion firmness of the tiles is significantly improved, the actual use needs are met, and the strength of the tiles is improved while reducing water absorption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004977067090000151
    Figure BDA0004977067090000151
Patent Text Reader

Abstract

The invention discloses a ceramic tile with holes in the bottom surface. The ceramic tile comprises a hole layer and a surface layer which are sequentially arranged from bottom to top. The hole layer is obtained by calcining hole powder, the surface layer is obtained by calcining surface layer powder, and the content of aluminum oxide in the ceramic tile is 22-25% according to mass percent; the hole powder comprises foaming powder and mullite type powder; wherein the foaming powder is prepared from the following raw materials in parts by mass: 10 to 12 parts of clay I, 8 to 12 parts of polishing slag, 15 to 20 parts of limestone and 53 to 67 parts of fluxing agent I; each of the surface layer powder and the mullite type powder is prepared from the following components in parts by mass: 17 to 31 parts of clay II, 1 to 3 parts of calcined coal gangue, 15 to 18 parts of green gangue, 10 to 16 parts of reclaimed material and 40 to 48 parts of fluxing agent II. According to the ceramic tile with the holes in the bottom surface and the preparation method of the ceramic tile, the pasting firmness of the ceramic tile is ensured on the premise that the water absorption rate of the ceramic tile is reduced and the strength of the ceramic tile is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of building ceramics, and in particular to a ceramic tile with holes on the bottom surface and a preparation method thereof. Background Art

[0002] Ceramic tiles are widely used in the field of building decoration, especially in interior decoration. Ceramic tiles have become the main material for wall and floor decoration. The construction method of tile laying usually uses cement mortar or adhesives to stick the tiles on the wall and floor surface. However, in order to ensure the strength of the tiles, the water absorption rate of the tiles is generally controlled below 3%. Due to the low water absorption rate of the tiles, it is not easy for cement mortar or adhesives to penetrate into the interior of the brick body and form a firm bonding surface with the wall and floor, resulting in poor tile bonding firmness.

[0003] In order to solve the technical problem of poor adhesion of tiles, some technical personnel in the field of building decoration and renovation began to set back patterns on the surface of the bottom of the tiles, thereby increasing the roughness of the bottom of the tiles, in order to achieve the purpose of firmly adhering the tiles. Although the above method can increase the adhesion of tiles to a certain extent, it is still difficult to solve the adhesion problem of tiles due to low water absorption. That is, the effect of setting back patterns on the surface of the bottom of the tiles in the prior art on improving the adhesion of tiles is very limited. Summary of the invention

[0004] The purpose of the present invention is to provide a ceramic tile with holes on the bottom surface and a preparation method thereof, wherein the water absorption rate of the ceramic tile is less than 0.05%, the rupture modulus is ≥47MPa, and the breaking strength is ≥2000N. On the premise of reducing the water absorption rate of the ceramic tile and improving the strength of the ceramic tile, the adhesive firmness of the ceramic tile is ensured to overcome the shortcomings of the prior art.

[0005] To achieve this object, the present invention adopts the following technical solutions:

[0006] A ceramic tile with holes on the bottom surface, comprising a hole layer and a surface layer arranged in sequence from bottom to top; the hole layer is obtained by calcining the hole powder, the surface layer is obtained by calcining the surface layer powder, and the content of aluminum oxide in the ceramic tile is 22% to 25% calculated by mass percentage;

[0007] The pore powder includes foaming powder and mullite powder; wherein, calculated by weight, the foaming powder includes the following raw materials: 10-12 parts of clay I, 8-12 parts of polishing residue, 15-20 parts of limestone and 53-67 parts of flux I;

[0008] Calculated by weight, the surface layer powder and the mullite powder both include 17 to 31 parts of clay II, 1 to 3 parts of calcined coal gangue, 15 to 18 parts of green gangue, 10 to 16 parts of recycled materials and 40 to 48 parts of flux II.

[0009] Further, calculated by mass percentage, the chemical composition of the polishing slag includes CaO 1.6-1.7%, SiO2 63.1-63.2%, Fe2O3 1.4-1.5%, MgO 0.8-0.9%, TiO2 0.2-0.3%, Al2O3 20.2-20.3%, K2O 3.7-3.8% and Na2O 1.9-2.0%, and the rest is loss on ignition;

[0010] Calculated by mass percentage, the chemical composition of the surface layer powder and the mullite powder includes CaO 0.9-1.0%, SiO2 64-66%, MgO 0.3-0.4%, Al2O3 19-19.5%, K2O 3.8-4.2% and Na2O1.6-1.8%, and the rest is ignition loss.

[0011] Furthermore, the pore powder includes 20-30% of foaming powder and 70-80% of mullite powder according to mass percentage;

[0012] The particle size of the limestone is 5 to 7 mm.

[0013] Furthermore, the particle gradation of the foaming powder is as follows: in terms of mass percentage, the residue on a 20-mesh sieve is 0.3-0.5%, the residue on a 40-mesh sieve is 1.5-2.5%, the residue on a 60-mesh sieve is 55-65% and the residue on a 100-mesh sieve is 97.5-98.5%.

[0014] Furthermore, the thickness of the hole layer is 2-3 mm, and the thickness of the surface layer is 7-8 mm.

[0015] Further, the clay II includes bentonite, washed kaolin and Luoshan soil, and the chemical composition of the Luoshan soil includes CaO 1.2-1.3%, SiO2 68.5-68.6%, Fe2O33.2-3.3%, MgO 0.7-0.8%, TiO2 0.4-0.5%, Al2O3 13.9-14.0%, K2O 3.0-3.1% and Na2O 1.1-1.3%, and the rest is loss on ignition;

[0016] Calculated by weight, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 10-16 parts of recycled material and 40-48 parts of flux II.

[0017] Further, the recycled materials include polishing mud, waste brick powder and recycled blanks;

[0018] Calculated by mass, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 5-7 parts of polishing mud, 4-6 parts of waste brick powder, 1-3 parts of recycled blanks and 40-48 parts of flux II.

[0019] Further, the clay I includes Honda clay and Dajiang black clay, and the mixing ratio of the Honda clay and the Dajiang black clay is (2-4):1 according to the mass ratio.

[0020] Calculated by mass percentage, the chemical composition of the Honda clay includes CaO 0.1-0.2%, SiO2 51.7-51.8%, Fe2O3 2.7-2.8%, MgO 0.6-0.7%, TiO2 0.4-0.5%, Al2O3 30.3-30.4%, K2O 2.9-3.0% and Na2O 0.01-0.02%, and the rest is loss on ignition;

[0021] Calculated by mass percentage, the chemical composition of the Dajiang black mud includes CaO 0.25-0.3%, SiO2 51.5-51.6%, Fe2O3 2.5-2.6%, MgO 0.6-0.7%, TiO2 0.3-0.4%, Al2O3 31.1-31.2%, K2O 2.7-2.8% and Na2O 0.2-0.25%, and the rest is loss on ignition.

[0022] Furthermore, the flux I includes nepheline, potassium feldspar and black talc, and calculated by weight, the foaming powder includes the following raw materials: 10 to 12 parts of clay I, 8 to 12 parts of polishing slag, 15 to 20 parts of limestone, 25 to 30 parts of nepheline, 20 to 25 parts of potassium feldspar and 8 to 12 parts of black talc.

[0023] A method for preparing a ceramic tile having holes on the bottom surface, for preparing the ceramic tile having holes on the bottom surface, comprising the following steps:

[0024] A. Mix clay I, polishing residue, limestone and flux I evenly according to the proportion to obtain foaming powder;

[0025] B. Mix clay II, calcined coal gangue, green gangue, recycled material and flux II in proportion to obtain mullite powder;

[0026] C. Mix the foaming powder and the mullite powder evenly according to the proportion to obtain the porous powder;

[0027] D. Spread the porous powder to obtain a porous layer; take mullite powder as the surface layer powder, spread the surface layer powder on the top of the porous layer to obtain a surface layer, and after pressing and calcining in a kiln, obtain a tile with holes on the bottom; wherein the calcination temperature is 1120-1125°C, and the calcination time is 35-40min.

[0028] The technical solution provided by the present invention may include the following beneficial effects:

[0029] 1. In this technical solution, the porous powder is designed to be a mixed powder including foaming powder and mullite powder, wherein the limestone (whose main component is calcium carbonate) in the foaming powder decomposes during high-temperature calcination to produce carbon dioxide gas and discharge it, thereby leaving an irregular porous structure on the bottom surface of the tile. At the same time, the amount of flux I added in the foaming powder formula is larger than the amount of flux II added in the mullite powder formula, so that the foaming powder forms a powder with a firing temperature of 1050-1100°C, and the mullite powder forms a powder with a firing temperature of 1120-1125°C, that is, the firing temperature of the foaming powder is lower than that of the mullite powder. Therefore, when the mullite powder in the porous powder produces a liquid phase and begins to vitrify, the foaming powder will promote the boiling of the mullite powder liquid phase due to its complete melting, which is also conducive to the generation of a large number of irregular porous structures.

[0030] 2. In this technical solution, the porous powder is a mixture of foaming powder and mullite powder, which is conducive to the formation of a large number of irregular holes during the calcination of the porous powder. It can not only utilize the high strength of the foaming powder, but also the high strength of the mullite powder, thereby giving the porous layer high strength. In addition, the formula of the surface layer powder is the same as that of the mullite powder, which is more conducive to improving the strength of the surface layer. Through the mutual cooperation of the porous layer and the surface layer, the rupture modulus of the tile is ≥47MPa, the breaking strength is ≥2000N, and it has high strength. DETAILED DESCRIPTION

[0031] The technical solution provides a ceramic tile with holes on the bottom surface, comprising a hole layer and a surface layer arranged in sequence from bottom to top; the hole layer is obtained by calcining the hole powder, the surface layer is obtained by calcining the surface layer powder, and the content of aluminum oxide in the ceramic tile is 22% to 25% by mass percentage;

[0032] The pore powder includes foaming powder and mullite powder; wherein, calculated by weight, the foaming powder includes the following raw materials: 10-12 parts of clay I, 8-12 parts of polishing residue, 15-20 parts of limestone and 53-67 parts of flux I;

[0033] Calculated by weight, the surface layer powder and the mullite powder both include 17 to 31 parts of clay II, 1 to 3 parts of calcined coal gangue, 15 to 18 parts of green gangue, 10 to 16 parts of recycled materials and 40 to 48 parts of flux II.

[0034] In order to solve the technical problem of the instability of ceramic tiles in the prior art, the present technical solution proposes a ceramic tile with holes on the bottom surface, comprising a hole layer and a surface layer arranged in sequence from bottom to top; the hole layer is obtained by calcining a hole powder, and the surface layer is obtained by calcining a surface layer powder, and the hole powder comprises a foaming powder and a mullite powder, and the raw materials and the amount of raw materials included in the surface layer powder and the mullite powder are the same. By optimizing the formula of the foaming powder, the mullite powder and the surface layer powder, the water absorption rate of the ceramic tile is <0.05%, the rupture modulus is ≥47MPa, and the destructive strength is ≥2000N. On the premise of reducing the water absorption rate of the ceramic tile and improving the strength of the ceramic tile, the firmness of the ceramic tile adhesion is ensured.

[0035] Specifically, the existing travertine bricks generally include a bottom layer and a surface layer stacked from bottom to top, and the hole effect of the travertine texture bricks only exists in the surface layer, but the travertine bricks with the hole effect only existing in the surface layer cannot solve the technical problem of the loose adhesion of the tiles in the technical solution. Therefore, the tiles with holes in the technical solution cannot be based on the above principle.

[0036] In order to improve the firmness of tile adhesion, the pore powder is designed as a mixed powder including foaming powder and mullite powder in the technical solution, wherein the limestone (whose main component is calcium carbonate) in the foaming powder decomposes and produces carbon dioxide gas during high-temperature calcination and is discharged, thereby leaving an irregular pore structure on the bottom surface of the tile. At the same time, the amount of flux I added in the foaming powder formula is larger than the amount of flux II added in the mullite powder formula, so that the foaming powder forms a powder with a firing temperature of 1050-1100°C, and the mullite powder forms a powder with a firing temperature of 1120-1125°C, that is, the firing temperature of the foaming powder is lower than that of the mullite powder. Therefore, when the mullite powder in the pore powder produces a liquid phase and begins to vitrify, the foaming powder will promote the boiling of the mullite powder liquid phase due to its complete melting, which is also conducive to the generation of a large number of irregular pore structures.

[0037] Therefore, the technical solution limits the raw material limestone in the foaming powder formula and the addition amount of flux I in the foaming powder formula and the addition amount of flux II in the mullite powder formula, so that a large number of irregular hole structures are generated on the bottom surface of the tile, so that the adhesive coated on the bottom surface of the tile forms a stable inlaid mortise and tenon structure with the brick body during the paving process, greatly enhancing the firmness of the adhesion and meeting the actual use requirements. In addition, compared with the regular hole structure, the irregular hole structure is conducive to the adhesive to quickly enter the hole through multiple directions and angles to form a more stable inlaid mortise and tenon structure with the brick body, thereby improving the firmness of the adhesion.

[0038] At the same time, the foaming powder in the present technical solution also includes clay I and polishing residue. The main chemical component of clay I is silicon dioxide, which mainly plays a plasticizing and binding role and is conducive to improving strength. Adding it to the foaming powder can improve the plasticity, strength and grouting formability of the foaming powder. At the same time, polishing residue is the solid waste generated during the production process of ceramic products (such as polished tiles and glazed tiles, etc.) after polishing and grinding to obtain a bright and delicate surface. Because it has high strength itself, it gives the foaming powder high strength. Therefore, the present technical solution introduces clay I and polishing residue into the foaming powder and limits the addition amount of the above two raw materials, so that the foaming powder has a higher strength.

[0039] In addition, the raw materials of the surface layer powder and mullite type powder also include clay II, calcined coal gangue, green gangue and recycled materials. The main chemical component of clay II is silicon dioxide, which is beneficial to improving the plasticity, strength and grouting formability of the surface layer powder and mullite type powder; coal gangue is the waste residue such as stones and mud left over in the process of coal mining, calcined coal gangue is the product obtained after high-temperature calcination of coal gangue, and its main component is aluminum oxide, and the main component of green gangue is also aluminum oxide. In addition to reacting with silicon dioxide in clay II to form mullite, aluminum oxide in calcined coal gangue and green gangue has high mechanical strength and excellent wear resistance. It is added to the surface layer powder and mullite type powder formula to provide a supporting skeleton, which is beneficial to improving the strength of the surface layer powder and mullite type powder formula; in addition, recycled materials are also beneficial to adjusting the strength of the surface layer powder and mullite type powder because of their own high strength.

[0040] Therefore, the technical solution introduces clay II, calcined coal gangue, green gangue and recycled materials into the surface layer powder and mullite type powder, and limits the addition amount of the above raw materials, so that the surface layer powder and mullite type powder have higher strength.

[0041] Therefore, based on the formula design of foaming powder and mullite powder, the hole powder in this technical solution is a mixture of foaming powder and mullite powder, which is conducive to the formation of a large number of irregular holes in the calcination process of the hole powder. It can not only utilize the high strength of the foaming powder, but also the high strength of the mullite powder, thereby giving the hole layer high strength. In addition, the formula of the surface layer powder is the same as that of the mullite powder, which is more conducive to improving the strength of the surface layer. Through the mutual cooperation of the hole layer and the surface layer, the rupture modulus of the tile is ≥47MPa, the destructive strength is ≥2000N, and it has a higher strength.

[0042] In addition, the aluminum oxide content in the ceramic tile of the technical solution is as high as 22% to 25%, which is 3% to 5% higher than that in conventional ceramic tiles. The high aluminum oxide content is conducive to producing more mullite during the calcination process, which is convenient for improving the firmness of the ceramic tile skeleton, so that the ceramic tile has a high strength under the premise of having a large number of irregular holes on the bottom surface. Furthermore, by optimizing the formula of the foaming powder, mullite powder and surface powder in the technical solution, it is also conducive to reducing the water absorption rate of the green body after firing, so that the water absorption rate of the ceramic tile is less than 0.05%, which is also conducive to ensuring its strength.

[0043] It should be noted that the manufacturer of the calcined coal gangue in this technical solution is Shandong Zibo Hengli Trading Co., Ltd., and the model is 50 calcined gangue; the manufacturer of green gangue is Yuanqu County Chengtaiyuan Trading Co., Ltd., and the model is 40 green gangue.

[0044] It is further explained that, calculated by mass percentage, the chemical composition of the polishing slag includes CaO 1.6-1.7%, SiO2 63.1-63.2%, Fe2O3 1.4-1.5%, MgO 0.8-0.9%, TiO2 0.2-0.3%, Al2O3 20.2-20.3%, K2O 3.7-3.8% and Na2O 1.9-2.0%, and the rest is loss on ignition;

[0045] Calculated by mass percentage, the chemical composition of the surface layer powder and the mullite powder includes CaO 0.9-1.0%, SiO2 64-66%, MgO 0.3-0.4%, Al2O3 19-19.5%, K2O 3.8-4.2% and Na2O1.6-1.8%, and the rest is ignition loss.

[0046] The polishing slag is preferably selected, wherein the chemical composition is calculated by mass percentage and includes CaO 1.6-1.7%, SiO2 63.1-63.2%, Fe2O3 1.4-1.5%, MgO 0.8-0.9%, TiO2 0.2-0.3%, Al2O3 20.2-20.3%, K2O3.7-3.8% and Na20 1.9-2.0%, wherein the SiO2 content is as high as 63.1-63.2%, which is more conducive to improving the strength of the foaming powder.

[0047] The preferred chemical composition includes CaO 0.9-1.0%, SiO2 64-66%, MgO 0.3-0.4%, Al2O3 19-19.5%, K2O 3.8-4.2% and Na20 1.6-1.8% of the surface powder and mullite powder, calculated by mass percentage. The SiO2 content is as high as 64-66%, and the Al2O3 content is as high as 19-19.5%. It is a high-silicon and high-aluminum powder, which is beneficial to ensure the hardness and strength of the surface powder and mullite powder.

[0048] Further, calculated by mass percentage, the pore powder includes 20-30% foaming powder and 70-80% mullite powder;

[0049] The particle size of the limestone is 5 to 7 mm.

[0050] In this technical solution, the amount of foaming powder and mullite powder added to the hole powder is optimized, which is conducive to making the porosity of the tile 25-35%, so that the adhesive enters the hole and forms a more embedded mortise and tenon structure with the brick body during paving, ensuring its paving firmness. At the same time, it is also conducive to adjusting the bulk density of the hole powder and ensuring the performance of the hole powder. It should be noted that the porosity of the tile is the result calculated according to the volume ratio.

[0051] Furthermore, in the technical solution, the particle size of the limestone is limited so that the diameter of the hole is 1.5-2 mm and the depth is 1.8-2 mm, which is not only conducive to ensuring the firmness of the adhesion, but also conducive to ensuring the strength of the tile.

[0052] It is further explained that the particle gradation of the foaming powder is as follows: according to mass percentage, the residue on a 20-mesh sieve is 0.3-0.5%, the residue on a 40-mesh sieve is 1.5-2.5%, the residue on a 60-mesh sieve is 55-65% and the residue on a 100-mesh sieve is 97.5-98.5%.

[0053] The technical scheme optimizes the particle grading of the foaming powder. On the one hand, it is conducive to the formation of holes of different sizes after calcination of foaming powders with different particle sizes, thereby increasing the irregularity and randomness of the hole structure and reducing the difficulty of preparation. At the same time, it is also more conducive to the adhesive to quickly enter the hole through multiple directions and angles to form a more stable inlaid mortise and tenon structure, thereby improving the firmness of the adhesive. On the other hand, under this particle grading, the bulk density of the foaming powder can reach 0.93-0.95 g / cm 3 , so that the porous powder obtained by mixing the foaming powder and the mullite powder has good fluidity, which is conducive to the molding and also helps the gas generated during the calcination of the porous powder to be discharged in time to form irregular holes.

[0054] It is further described that the thickness of the hole layer is 2 to 3 mm, and the thickness of the surface layer is 7 to 8 mm.

[0055] This technical solution also optimizes the thickness of the hole layer and the thickness of the surface layer, so that the adhesive and the brick body can form a stable inlaid mortise and tenon structure during paving, further ensuring the firmness of the paving while also helping to further ensure the strength of the tiles.

[0056] It is further explained that the clay II includes bentonite, washed kaolin and Luoshan soil, and the chemical composition of the Luoshan soil includes CaO 1.2-1.3%, SiO2 68.5-68.6%, Fe2O3 3.2-3.3%, MgO 0.7-0.8%, TiO2 0.4-0.5%, Al2O3 13.9-14.0%, K2O 3.0-3.1% and Na20 1.1-1.3%, and the rest is loss on ignition;

[0057] Calculated by weight, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 10-16 parts of recycled material and 40-48 parts of flux II.

[0058] Since bentonite, washed kaolin and Luoshan clay are all beneficial to improving the plasticity, grouting formability and strength of the surface layer powder and mullite-type powder, the technical scheme preferably uses clay II including bentonite, washed kaolin and Luoshan clay, and limits the addition amount of bentonite, washed kaolin and Luoshan clay, which is beneficial to further improve the performance of the surface layer powder and mullite-type powder.

[0059] It is further explained that the recycled materials include polishing mud, waste brick powder and recycled blanks;

[0060] Calculated by mass, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 5-7 parts of polishing mud, 4-6 parts of waste brick powder, 1-3 parts of recycled blanks and 40-48 parts of flux II.

[0061] Polishing mud refers to the recycled material obtained by recycling the materials used for polishing the surface of ceramics; waste brick powder refers to the powder particles obtained after waste bricks in construction waste are sorted, crushed, screened and ground; recycled blanks refer to blanks that are eliminated due to some reasons (such as shape that does not meet the requirements, surface defects and drying cracks, etc.) after initial forming or processing in the ceramic production process. The above three raw materials are all recycled materials in the ceramic field, and have the characteristics of low cost and high strength. The preferred recycled materials of this technical solution include polishing mud, waste brick powder and recycled blanks, and the addition amount of the above three raw materials is optimized, which is conducive to ensuring the performance of the product at a lower cost.

[0062] Preferably, calculated by mass percentage, the chemical composition of the polishing mud includes CaO 1.8-1.85%, SiO2 63.4-63.5%, Fe2O3 1.15-1.20%, MgO 0.8-0.9%, TiO2 0.4-0.45%, Al2O3 20.4-20.5%, K2O 3.6-3.65% and Na2O 1.8-1.9%, and the rest is loss on ignition;

[0063] Preferably, calculated by mass percentage, the chemical composition of the waste brick powder includes CaO 1.2-1.3%, SiO2 64.2-64.3%, Fe2O3 1.3-1.4%, MgO 0.3-0.4%, TiO2 0.3-0.4%, Al2O3 21.2-21.4%, K2O 4.0-4.1% and Na2O 1.8-1.9%, and the rest is loss on ignition;

[0064] Preferably, calculated by mass percentage, the chemical composition of the recycled blank includes CaO 1.1-1.2%, SiO2 62.8-62.9%, Fe2O3 1.3-1.4%, MgO 0.4-0.45%, TiO2 0.4-0.45%, Al2O3 20.4-20.5%, K2O 3.8-3.9% and Na2O 1.7-1.9%, and the rest is loss on ignition.

[0065] Preferably, the flux II comprises potassium feldspar, sodium feldspar and porcelain stone;

[0066] Calculated by mass, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 5-7 parts of polishing mud, 4-6 parts of waste brick powder, 1-3 parts of recycled green material, 8-10 parts of potassium feldspar, 27-31 parts of sodium feldspar and 5-7 parts of porcelain stone.

[0067] Since potassium feldspar, sodium feldspar and porcelain stone all have good fluxing effects, in order to reduce the sintering temperature of the surface layer powder and mullite powder, the technical scheme preferably uses flux II including potassium feldspar, sodium feldspar and porcelain stone, and limits the addition amount of potassium feldspar, sodium feldspar and porcelain stone to ensure the fluxing effect.

[0068] It should be noted that porcelain stone is a silicate rock mineral composed of quartz, sericite, feldspar and aluminum oxide, and its chemical composition mainly includes SiO2, Al2O3, K2O, Na2O and Fe2O3. The manufacturer of porcelain stone in this technical solution is Yuanqu Chengtaiyuan Trading Co., Ltd., and the model is 8 potassium porcelain stone.

[0069] Preferably, calculated by mass, the surface layer powder and the mullite powder both include 12.5 parts of bentonite, 4.0 parts of washed kaolin, 7.5 parts of Luoshan clay, 2.0 parts of calcined coal gangue, 16.5 parts of green gangue, 6.0 parts of polishing mud, 5.0 parts of waste brick powder, 2.0 parts of recycled green material, 9.0 parts of potassium feldspar, 29.5 parts of sodium feldspar and 6.0 parts of porcelain stone.

[0070] It is further described that the clay I includes Honda clay and Dajiang black clay, and the mixing ratio of the Honda clay and the Dajiang black clay is (2-4):1 according to the mass ratio.

[0071] Calculated by mass percentage, the chemical composition of the Honda clay includes CaO 0.1-0.2%, SiO2 51.7-51.8%, Fe2O3 2.7-2.8%, MgO 0.6-0.7%, TiO2 0.4-0.5%, Al2O3 30.3-30.4%, K2O 2.9-3.0% and Na2O 0.01-0.02%, and the rest is loss on ignition;

[0072] Calculated by mass percentage, the chemical composition of the Dajiang black mud includes CaO 0.25-0.3%, SiO2 51.5-51.6%, Fe2O3 2.5-2.6%, MgO 0.6-0.7%, TiO2 0.3-0.4%, Al2O3 31.1-31.2%, K2O 2.7-2.8% and Na2O 0.2-0.25%, and the rest is loss on ignition.

[0073] Honda clay and Dajiang black clay are both beneficial to improving the plasticity, grouting formability and strength of the foaming powder. Therefore, the preferred clay I of this technical solution includes Honda clay and Dajiang black clay to ensure the performance of the foaming powder. At the same time, since the content of silicon dioxide in Honda clay is higher than that of silicon dioxide in Dajiang black clay, the content of aluminum oxide in Honda clay is higher than that of aluminum oxide, which is more conducive to improving the performance of the foaming powder. Therefore, the preferred addition amount of Honda clay in this technical solution is greater than that of Dajiang black clay.

[0074] It is further explained that the flux I includes nepheline, potassium feldspar and black talc, and calculated by weight, the foaming powder includes the following raw materials: 10-12 parts of clay I, 8-12 parts of polishing slag, 15-20 parts of limestone, 25-30 parts of nepheline, 20-25 parts of potassium feldspar and 8-12 parts of black talc.

[0075] Nepheline, potassium feldspar and black talc all have good fluxing effects, and compared with conventional potassium and sodium feldspar, nepheline has a smaller expansion coefficient. The introduction of a large amount of nepheline can adjust the expansion coefficient of the foaming powder, so that the expansion coefficients of the foaming powder and the mullite powder match each other, avoiding cracking of the tiles after firing in the kiln, and ensuring the hardness and anti-fouling performance of the tiles. In addition, the chemical composition of black talc is mainly silicon dioxide and magnesium oxide, so that in addition to having a fluxing effect, it is also beneficial to improve the strength of the foaming powder. Therefore, the preferred flux I of this technical solution includes nepheline, potassium feldspar and black talc, which is beneficial to ensure the performance of the foaming powder.

[0076] Preferably, calculated by weight, the foaming powder includes 12 parts of clay I, 10 parts of polishing residue, 17 parts of limestone, 29 parts of nepheline, 22 parts of potassium feldspar and 10 parts of black talc.

[0077] A method for preparing a ceramic tile having holes on the bottom surface, for preparing the ceramic tile having holes on the bottom surface, comprising the following steps:

[0078] A. Mix clay I, polishing residue, limestone and flux I evenly according to the proportion to obtain foaming powder;

[0079] B. Mix clay II, calcined coal gangue, green gangue, recycled material and flux II in proportion to obtain mullite powder;

[0080] C. Mix the foaming powder and the mullite powder evenly according to the proportion to obtain the porous powder;

[0081] D. Spread the porous powder to obtain a porous layer; take mullite powder as the surface layer powder, spread the surface layer powder on the top of the porous layer to obtain a surface layer, and after pressing and calcining in a kiln, obtain a tile with holes on the bottom; wherein the calcination temperature is 1120-1125°C, and the calcination time is 35-40min.

[0082] The technical solution also proposes a method for preparing ceramic tiles with holes on the bottom surface. The preparation method is simple and easy to operate, which is conducive to ensuring that the water absorption rate of the ceramic tiles is less than 0.05%, the rupture modulus is ≥47MPa, and the destructive strength is ≥2000N. On the premise of reducing the water absorption rate of the ceramic tiles and improving the strength of the ceramic tiles, the firmness of the ceramic tiles' adhesion is ensured.

[0083] Furthermore, the calcination temperature is 1120-1125°C, and the calcination time is 35-40 minutes. Based on the performance of the foaming powder and the mullite powder, tiles can be calcined at a lower calcination temperature and a shorter calcination time, achieving low-cost and green production, which is conducive to improving the competitiveness of tile products.

[0084] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0085] Performance Test:

[0086] Water absorption: The water absorption is tested according to the test method of GBT3810.3-2016 Ceramic Tile Test Method Part 3: Determination of Water Absorption, Apparent Porosity, Apparent Relative Density and Bulk Density.

[0087] Modulus of rupture: The modulus of rupture is tested according to the test method of GB / T3810.7-2016 "Test methods for ceramic tiles Part 4: Determination of modulus of rupture and breaking strength".

[0088] Destructive strength: The destructive strength is tested according to the test method of GB / T3810.7-2016 "Test methods for ceramic tiles Part 4: Determination of rupture modulus and destructive strength".

[0089] Adhesion firmness: After the tiles are pasted, the five-point knocking test method is used, that is, knock on the four corners and the center of the tile respectively, and judge whether there are hollows by the changes in sound. If there are no hollows, the adhesion firmness is qualified.

[0090] The manufacturer of the calcined coal gangue used in the embodiments and comparative examples of the present invention is Shandong Zibo Hengli Trading Co., Ltd., and the model is 50 calcined gangue; the manufacturer of the green gangue is Yuanqu County Chengtaiyuan Trading Co., Ltd., and the model is 40 green gangue; the manufacturer of the porcelain stone is Yuanqu Chengtaiyuan Trading Co., Ltd., and the model is 8 potassium porcelain stone. According to the mass percentage, CaO1.68%, SiO2 63.12%, Fe2O3 1.4%, MgO 0.85%, TiO2 0.4%, Al2O3 20.29%, K2O 3.76% and Na2O 1.93%, and the rest is the loss on ignition; according to the mass percentage, the chemical composition of Honda mud includes CaO 0.17%, SiO2 51.72%, Fe2O3 2.7%, MgO0.6%, TiO2 0.49%, Al2O3 30.31%, K2O 2.99% and Na2O0.01%, and the rest is the loss on ignition; according to the mass percentage, the chemical composition of Dajiang black mud includes CaO 0.28%, SiO251.52%, Fe2O32.51%, MgO 0.68%, TiO2 The chemical composition of Luoshan soil includes CaO 1.24%, SiO2 68.59%, Fe2O3 3.24%, MgO0.77%, TiO2 0.42%, Al2O3 13.99%, K2O 3.03% and Na20 1.2%, and the rest is loss on ignition; the chemical composition of polishing mud includes CaO 1.83%, SiO2 63.49%, Fe2O3 1.19%, MgO 0.84%, TiO20.42%, Al2O320.49%, K2O 3.62% and Na20 1.87%, and the rest is loss on ignition; calculated by mass percentage, the chemical composition of waste brick powder includes CaO 1.27%, SiO2 64.26%, Fe2O3 1.33%, MgO 0.36%, TiO2 0.36%, Al2O3 21.3%, K2O 4.07% and Na2O 1.87%, and the rest is the loss on ignition; calculated by mass percentage, the chemical composition of the recycled blank includes CaO 1.18%, SiO2 62.83%, Fe2O3 1.34%, MgO 0.42%, TiO2 0.4%, Al2O3 20.44%, K2O3.85% and Na2O 1.8%, and the rest is the loss on ignition. In addition, if the specific technology or conditions are not specified in the embodiment, the technology or conditions described in the literature in this field or the product manual shall be followed. The reagents or instruments used without indicating the manufacturer are all conventional products that can be purchased commercially.

[0091] Example 1

[0092] A method for preparing a tile having holes on the bottom surface comprises the following steps:

[0093] A. 12 parts of clay I, 10 parts of polishing residue, 17 parts of limestone with a particle size of 5 mm, 29 parts of nepheline, 22 parts of feldspar and 10 parts of black talc, which are mixed in a ratio of 3:1, are uniformly mixed to obtain a foaming powder having a particle size of 0.3% on a 20-mesh sieve, 1.5% on a 40-mesh sieve, 60% on a 60-mesh sieve and 98% on a 100-mesh sieve;

[0094] B. 12.5 parts of bentonite, 4.0 parts of washed kaolin, 7.5 parts of Luoshan soil, 2.0 parts of calcined coal gangue, 16.5 parts of green gangue, 6.0 parts of polishing mud, 5.0 parts of waste brick powder, 2.0 parts of recycled blank, 9.0 parts of potassium feldspar, 29.5 parts of sodium feldspar and 6.0 parts of porcelain stone are mixed to obtain mullite type powder;

[0095] C. Calculated by mass percentage, 30% of the foaming powder and 70% of the mullite powder are mixed evenly to obtain a porous powder;

[0096] D. After spreading the porous powder, a porous layer with a thickness of 3 mm is obtained; mullite powder is taken as the surface layer powder, and the surface layer powder is spread on the top of the porous layer to obtain a surface layer with a thickness of 7 mm, and after pressing and calcining in a kiln, a tile with holes on the bottom is obtained; wherein, the calcination temperature is 1120°C, the calcination time is 40 minutes, and the content of alumina in the tile body is 25%.

[0097] Example 2

[0098] A method for preparing a tile having holes on the bottom surface comprises the following steps:

[0099] A. 10 parts of clay I, 12 parts of polishing residue, 20 parts of limestone with a particle size of 6 mm, 25 parts of nepheline, 20 parts of feldspar, and 8-12 parts of black talc, which are mixed in a ratio of 4:1, are uniformly mixed to obtain a foaming powder having a particle size distribution of 0.5% on a 20-mesh sieve, 2% on a 40-mesh sieve, 60% on a 60-mesh sieve, and 97.5% on a 100-mesh sieve;

[0100] B. Mix 15 parts of bentonite, 2 parts of washed kaolin, 5 parts of Luoshan soil, 3 parts of calcined coal gangue, 15 parts of green gangue, 6 parts of polishing mud, 6 parts of waste brick powder, 2 parts of recycled blank, 8 parts of potassium feldspar, 27 parts of sodium feldspar and 5 parts of porcelain stone to obtain mullite powder;

[0101] C. Calculate by mass percentage, and evenly mix 20% of the foaming powder and 80% of the mullite powder to obtain a porous powder;

[0102] D. After spreading the porous powder, a porous layer with a thickness of 2 mm is obtained; mullite powder is taken as the surface layer powder, and the surface layer powder is spread on the top of the porous layer to obtain a surface layer with a thickness of 8 mm, and after pressing and calcining in a kiln, a tile with holes on the bottom is obtained; wherein, the calcination temperature is 1120°C, the calcination time is 38 min, and the content of alumina in the tile body is 23.8%.

[0103] Example 3

[0104] A method for preparing a tile having holes on the bottom surface comprises the following steps:

[0105] A. 11 parts of clay I, 8 parts of polishing residue, 15 parts of limestone with a particle size of 7 mm, 30 parts of nepheline, 25 parts of feldspar, and 8 parts of black talc, which are mixed in a ratio of 2:1, are uniformly mixed to obtain a foaming powder with a particle size of 0.4% on a 20-mesh sieve, 2.5% on a 40-mesh sieve, 65% on a 60-mesh sieve, and 98.5% on a 100-mesh sieve;

[0106] B. Mix 10 parts of bentonite, 6 parts of washed kaolin, 10 parts of Luoshan soil, 1 part of calcined coal gangue, 18 parts of green gangue, 5 parts of polishing mud, 5 parts of waste brick powder, 3 parts of recycled blank, 9 parts of potassium feldspar, 30 parts of sodium feldspar and 5 parts of porcelain stone to obtain mullite powder;

[0107] C. Calculate by mass percentage, and evenly mix 25% of the foaming powder and 75% of the mullite powder to obtain a porous powder;

[0108] D. After spreading the porous powder, a porous layer with a thickness of 2.5 mm is obtained; mullite powder is taken as the surface layer powder, and the surface layer powder is spread on the top of the porous layer to obtain a surface layer with a thickness of 7.5 mm, and after pressing and calcining in a kiln, a tile with holes on the bottom is obtained; wherein, the calcination temperature is 1125°C, the calcination time is 35 minutes, and the content of alumina in the tile body is 22.6%.

[0109] Comparative Example 1

[0110] The preparation method and raw materials of Comparative Example 1 are the same as those of Example 1, except that limestone is not added to the foaming powder formula in Comparative Example 1.

[0111] Comparative Example 2

[0112] The preparation method and raw materials of Comparative Example 2 are the same as those of Example 1, except that the amount of flux I added in Comparative Example 2 is the same as the amount of flux II added, that is, in Comparative Example 2, calculated by mass, the foaming powder includes the following raw materials: 12 parts of clay I mixed with Honda mud and Dajiang black mud in a ratio of 3:1, 10 parts of polishing slag, 17 parts of limestone, 19 parts of nepheline, 14.5 parts of potassium feldspar and 10 parts of black talc.

[0113] The ceramic tiles were prepared by using the different preparation methods in the above embodiments and comparative examples, and the water absorption, rupture modulus, breaking strength and adhesive firmness of the prepared ceramic tiles were tested. The test results are shown in Table 1 below.

[0114] Table 1 Performance test results of different tiles in the embodiments and comparative examples

[0115]

[0116] From the performance test results of each embodiment in the above table, it can be seen that the ceramic tile prepared by the preparation method of a ceramic tile with holes on the bottom surface has a water absorption rate of less than 0.05%, a rupture modulus ≥47MPa, and a destructive strength ≥2000N. Under the premise of reducing the water absorption rate of the ceramic tile and improving the strength of the ceramic tile, the firmness of the ceramic tile adhesion is ensured.

[0117] Since no limestone was added to Comparative Example 1, the adhesion firmness of the tiles was poor and the adhesion firmness was unqualified.

[0118] In Comparative Example 2, since the amount of flux I added is the same as that of flux II, that is, the amount of flux I added is reduced, when the mullite powder produces a liquid phase and starts to vitrify, the foaming powder is not completely melted, which is not conducive to promoting the boiling of the mullite powder liquid phase, thereby not being conducive to the generation of a large number of irregular pore structures, resulting in a reduction in the void ratio, making the adhesion firmness worse and failing to meet the adhesion firmness requirements. At the same time, due to the reduction in the amount of flux I added, the calcination is incomplete, thereby affecting the water absorption and strength of the product.

[0119] The technical principle of the present invention is described above in conjunction with specific embodiments. These descriptions are only for explaining the principle of the present invention and cannot be interpreted as limiting the scope of protection of the present invention in any way. Based on the explanations herein, those skilled in the art can associate other specific implementations of the present invention without paying creative labor, and these methods will fall within the scope of protection of the present invention.

Claims

1. A ceramic tile having holes on the bottom surface, characterized in that: The ceramic tile comprises a hole layer and a surface layer arranged in sequence from bottom to top; the hole layer is obtained by calcining the hole powder, the surface layer is obtained by calcining the surface layer powder, and the content of aluminum oxide in the ceramic tile is 22% to 25% by mass percentage; The pore powder includes foaming powder and mullite powder; wherein, calculated by weight, the foaming powder includes the following raw materials: 10-12 parts of clay I, 8-12 parts of polishing residue, 15-20 parts of limestone and 53-67 parts of flux I; Calculated by weight, the surface layer powder and the mullite powder both include 17 to 31 parts of clay II, 1 to 3 parts of calcined coal gangue, 15 to 18 parts of green gangue, 10 to 16 parts of recycled materials and 40 to 48 parts of flux II.

2. A ceramic tile with holes on the bottom surface according to claim 1, characterized in that: Calculated by mass percentage, the chemical composition of the polishing slag includes CaO 1.6-1.7%, SiO2 63.1-63.2%, Fe2O3 1.4-1.5%, MgO 0.8-0.9%, TiO2 0.2-0.3%, Al2O3 20.2-20.3%, K2O 3.7-3.8% and Na2O1.9-2.0%, and the rest is ignition loss; Calculated by mass percentage, the chemical composition of the surface layer powder and the mullite powder includes CaO 0.9-1.0%, SiO2 64-66%, MgO 0.3-0.4%, Al2O3 19-19.5%, K2O 3.8-4.2% and Na20 1.6-1.8%, and the rest is ignition loss.

3. The ceramic tile with holes on the bottom surface according to claim 1, characterized in that: Calculated by mass percentage, the pore powder includes 20-30% foaming powder and 70-80% mullite powder; The particle size of the limestone is 5 to 7 mm.

4. The ceramic tile with holes on the bottom surface according to claim 1, characterized in that: The particle gradation of the foaming powder is as follows: according to mass percentage, the residue on a 20-mesh sieve is 0.3-0.5%, the residue on a 40-mesh sieve is 1.5-2.5%, the residue on a 60-mesh sieve is 55-65% and the residue on a 100-mesh sieve is 97.5-98.5%.

5. The ceramic tile with holes on the bottom surface according to claim 1, characterized in that: The thickness of the hole layer is 2-3 mm, and the thickness of the surface layer is 7-8 mm.

6. The ceramic tile with holes on the bottom surface according to claim 1, characterized in that: The clay II includes bentonite, washed kaolin and Luoshan clay, and the chemical composition of the Luoshan clay includes CaO 1.2-1.3%, SiO2 68.5-68.6%, Fe2O3 3.2-3.3%, MgO 0.7-0.8%, TiO2 0.4-0.5%, Al2O3 13.9-14.0%, K2O 3.0-3.1% and Na2O 1.1-1.3%, and the rest is loss on ignition; Calculated by weight, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 10-16 parts of recycled material and 40-48 parts of flux II.

7. The ceramic tile with holes on the bottom surface according to claim 6, characterized in that: The recycled materials include polishing mud, waste brick powder and recycled blanks; Calculated by mass, the surface layer powder and the mullite powder include 10-15 parts of bentonite, 2-6 parts of washed kaolin, 5-10 parts of Luoshan clay, 1-3 parts of calcined coal gangue, 15-18 parts of green gangue, 5-7 parts of polishing mud, 4-6 parts of waste brick powder, 1-3 parts of recycled blanks and 40-48 parts of flux II.

8. The ceramic tile with holes on the bottom surface according to claim 1, characterized in that: The clay I includes Honda clay and Dajiang black clay, and the mixing ratio of the Honda clay and the Dajiang black clay is (2-4):1 according to the mass ratio. Calculated by mass percentage, the chemical composition of the Honda clay includes CaO 0.1-0.2%, SiO2 51.7-51.8%, Fe2O3 2.7-2.8%, MgO 0.6-0.7%, TiO2 0.4-0.5%, Al2O3 30.3-30.4%, K2O 2.9-3.0% and Na2O 0.01-0.02%, and the rest is loss on ignition; Calculated by mass percentage, the chemical composition of the Dajiang black mud includes CaO 0.25-0.3%, SiO2 51.5-51.6%, Fe2O3 2.5-2.6%, MgO 0.6-0.7%, TiO2 0.3-0.4%, Al2O3 31.1-31.2%, K2O 2.7-2.8% and Na2O 0.2-0.25%, and the rest is loss on ignition.

9. The ceramic tile with holes on the bottom surface according to claim 1, characterized in that: The flux I includes nepheline, potassium feldspar and black talc, and the foaming powder includes the following raw materials calculated by weight: 10-12 parts of clay I, 8-12 parts of polishing slag, 15-20 parts of limestone, 25-30 parts of nepheline, 20-25 parts of potassium feldspar and 8-12 parts of black talc.

10. A method for preparing a tile having holes on the bottom surface, characterized in that: The method for preparing a ceramic tile having holes on the bottom surface as claimed in any one of claims 1 to 9 comprises the following steps: A. Mix clay I, polishing residue, limestone and flux I evenly according to the proportion to obtain foaming powder; B. Mix clay II, calcined coal gangue, green gangue, recycled material and flux II in proportion to obtain mullite powder; C. Mix the foaming powder and the mullite powder evenly according to the proportion to obtain the porous powder; D. Spread the porous powder to obtain a porous layer; take mullite powder as the surface layer powder, spread the surface layer powder on the top of the porous layer to obtain a surface layer, and after pressing and calcining in a kiln, obtain a tile with holes on the bottom; wherein the calcination temperature is 1120-1125°C, and the calcination time is 35-40min.

Citation Information

Patent Citations

  • Natural cavity stone imitation ceramic tile

    CN101016213A

  • Method for producing ceramic brick decorated with aperture

    CN101215185A

  • Production method for natural travertine-imitated glazed brick, and obtained green brick structure

    CN105036814A

  • Production method for travertine-imitated glazed brick

    CN105036815A