Archaized black brick based on blending of purple clay and solid waste and preparation method of archaized black brick

Through the preparation method of antique blue bricks mixed with purple clay and solid waste, combined with dry pressing or extrusion forming process and blue brick reduction process, the problems of solid waste disposal and industrial upgrading are solved, and efficient resource recycling and industrial linkage are achieved. , improving the industrial level and green development of Yan'an City.

CN118978386APending Publication Date: 2024-11-19YANAN HIGH-TECH ZONE CIRCULAR ECONOMY IND PARK CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
CN202411168263.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The existing technology has failed to effectively utilize purple clay clay and solid waste resources, resulting in the problem of solid waste disposal and the need for green upgrading of the traditional clay industry.

Method used

The antique blue brick preparation method of purple clay and solid waste is used to combine purple clay clay and solid waste. The antique blue brick with high compressive strength and low water absorption is prepared by dry pressing or extrusion forming process combined with blue brick reduction process. The antique blue brick with high compressive strength and low water absorption is used. Resources achieve green upgrading of the industry and resource recycling.

Benefits of technology

It has realized the recycling of solid waste resources, solved the worries of the energy industry, promoted the complementary linkage of industries in the region, and improved the industrial quality and efficiency improvement and green development of Yan'an City.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to an antique black brick based on purple clay and solid waste blending and a preparation method thereof. The antique black brick comprises the following raw materials: purple clay, coal gangue or fly ash and water. The preparation method comprises the following steps: aging and weathering the purple clay; weighing purple clay, coal gangue or fly ash, and uniformly stirring and mixing to obtain a mixed coarse material; crushing and sieving the mixed coarse material to obtain a mixed fine material; weighing water, adding the water into the mixed fine material, uniformly stirring to obtain a mixed raw material, warehousing the mixed raw material, and aging; carrying out dry pressing molding on the mixed raw material to obtain a wet green brick; drying the wet green brick to obtain a dry green brick; and firing the dry brick blank at the highest firing temperature of 960 DEG C to obtain the finished antique black brick. The purple clay and the solid waste resources are utilized, so that the problem of solid waste disposal can be solved, green upgrading of the traditional purple clay industry can be promoted, meanwhile, the solid waste resources are driven to be recycled, worries after development of the energy industry are solved, and complementary linkage between industries in a region is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and in particular relates to an antique blue brick based on mixing purple clay and solid waste and a preparation method thereof. Background Art

[0002] At present, Yan'an in my country has rich purple clay resources, which are relatively concentrated, with a thin covering layer and easy to mine. At the same time, as an important national comprehensive energy base, Yan'an has many coal mines and thermal power plants, which will produce a large amount of solid waste such as coal gangue, fly ash, slag, desulfurized gypsum, etc. during the production process. With the advancement of science and technology and industrial development, these solid wastes will also become available resources and be utilized.

[0003] For example, the Chinese invention application with publication number CN106278078A provides a fly ash antique blue brick, which uses fly ash, quicklime, yellow sand and a small amount of colorant to prepare steam-cured blue bricks; the Chinese invention application with publication number CN101519292A provides a machine-made lime sludge construction waste blue brick and its manufacturing method, and proposes to use raw materials such as construction waste, sludge, blue ash and cement to match the appearance and color similar to blue bricks, and then press and shape them, and steam and cure them to obtain finished products; however, none of the above patents use purple clay and solid waste at the same time. Therefore, how to use purple clay and solid waste resources to develop industries and solve the solid waste disposal problem at the same time is a problem that needs to be solved urgently. Summary of the invention

[0004] In view of the shortcomings of the prior art, the present invention provides an antique blue brick based on a mixture of purple clay and solid waste and a preparation method thereof. By utilizing purple clay and solid waste resources at the same time, it can not only solve the problem of solid waste disposal, but also promote the green upgrading of the traditional purple clay industry while driving the recycling of solid waste resources, solving the worries about the development of the energy industry and realizing the complementary linkage between industries in the region.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] The invention discloses an antique blue brick based on purple clay and solid waste, wherein the antique blue brick is composed of the following raw materials: 2.5-4 parts of purple clay, 1-2.5 parts of coal gangue or fly ash, and 0.35-0.4 parts of water; wherein the antique blue brick is made by a dry pressing process, and the length, width and height of the antique blue brick are 235-240mm*115-120mm*43-50mm.

[0007] Preferably, the compressive strength of the antique blue brick is greater than 35MP and the water absorption rate is less than 10%.

[0008] A method for preparing antique blue bricks by dry pressing process, the preparation method comprising the following steps:

[0009] The excavated purple clay is aged and weathered for at least 1 month;

[0010] Weigh purple clay, coal gangue or fly ash according to proportion, and stir and mix them evenly with a mixer to obtain a mixed coarse material;

[0011] The mixed coarse material is crushed, and the crushed mixed material is sieved using a 14-mesh drum screen to obtain a mixed fine material;

[0012] Weigh water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and store the mixed raw material in a warehouse for aging, and the aging time is not less than 12 hours;

[0013] The aged mixed raw materials in the warehouse are dry pressed into shape by a dry press to obtain wet bricks, and the color and strength of the wet bricks are tested;

[0014] The wet bricks are transported to the drying kiln by a kiln truck for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 240-245mm*120-125mm*45-55mm.

[0015] Transport dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0016] Preferably, the mixed coarse material is crushed by a breaker hammer or a crusher.

[0017] Preferably, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each time for 15 minutes.

[0018] Preferably, the green brick reduction process is to evenly spray natural gas in the kiln in an oxygen-deficient environment without igniting the kiln for 12-13 hours to form a reducing atmosphere in the kiln, and then spray tap water into the kiln for 24 hours. After the temperature in the kiln drops to 350°C, stop spraying tap water.

[0019] It should be noted that during the firing process, the iron element in the brick will generate red ferric oxide under an oxidizing atmosphere. By controlling the reducing atmosphere and cooling method, the ferric oxide can be reduced to bluish-gray ferrous oxide, making the brick appear bluish.

[0020] The invention discloses an antique blue brick based on a mixture of purple clay and solid waste, wherein the antique blue brick is composed of the following raw materials: 2.5-3.5 parts of purple clay, 1.5-2.5 parts of coal gangue and 0.4-0.45 parts of water; wherein the antique blue brick is manufactured by an extrusion molding process, and the length, width and height of the manufactured antique blue brick are 190-200mm*90-100mm*39-41mm.

[0021] A method for preparing antique blue bricks by using an extrusion molding process, the preparation method comprising the following steps:

[0022] The excavated purple clay is aged and weathered for at least 1 month;

[0023] Weigh purple clay, coal gangue or fly ash according to proportion, and stir and mix them evenly with a mixer to obtain a mixed coarse material;

[0024] The mixed coarse material is crushed, and the crushed mixed material is sieved using a 14-mesh drum screen to obtain a mixed fine material;

[0025] Weigh water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and store the mixed raw material in a warehouse for aging, and the aging time is not less than 12 hours;

[0026] The aged mixed raw materials in the warehouse are extruded into shapes by an extruder to obtain wet bricks, and the color and strength of the wet bricks are tested;

[0027] The wet bricks are transported to the drying kiln by a kiln truck for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 200-205mm*100-105mm*41-43mm.

[0028] Transport dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0029] Preferably, the green brick reduction process is to evenly spray natural gas in the kiln in an oxygen-deficient environment without igniting the kiln for 12-13 hours to form a reducing atmosphere in the kiln, and then spray tap water into the kiln for 24 hours. After the temperature in the kiln drops to 350°C, stop spraying tap water.

[0030] It should be noted that during the firing process, the iron element in the brick will generate red ferric oxide under an oxidizing atmosphere. By controlling the reducing atmosphere and cooling method, the ferric oxide can be reduced to bluish-gray ferrous oxide, making the brick appear bluish.

[0031] It should be noted that the purple clay used in this application is produced in Yan'an. The chemical composition of Yan'an purple clay is mainly SiO 2 、Al 2 O 3 , Fe 2 O 3 Mainly, among which SiO 2 :60.56%~61.99%, average 61.37%; Al 2 O 3 :15.98%~17.37%, average 16.69%; Fe 2 O 3 The content is relatively high, 6.34% to 7.54%, with an average of 6.78%; TiO 2 Content 1.08%~1.44%, average 1.23%; K 2 The O content is moderate, 1.88% to 3.63%, with an average of 2.42%; the CaO content is low, 0.23% to 0.58%, with an average of 0.39%; the MgO content is 2.45% to 2.88%, with an average of 2.68%; 2 O content is low, 0.21-0.68%, and average is 0.38%. 2 A moderate O content is beneficial to lowering the firing temperature, and a low CaO content is beneficial to preventing blistering and deformation during firing.

[0032] The fly ash used in this application is produced from Yan'an Datang Thermal Power Plant. The chemical composition of the fly ash includes SiO 2 :56.10%、Al 2 O 3 :24.50%、Fe 2 O 3 :5.01%、TiO 2 :0979%、K 2 O: 1.91%, CaO: 5.40%, MgO: 1.14%, Na 2 O: 0.80%.

[0033] The coal gangue used in this application is produced in Zichang City, Huangling County and Fu County. The chemical composition of the coal gangue includes SiO 2 :52.30%、Al 2 O 3 :26.03%、Fe 2 O 3 :2.66%、TiO2 :0.49%、K 2 O: 2.13%, CaO: 0.28%, MgO: 0.33%, Na 2 O: 0.41%.

[0034] Technical effects and advantages of the present invention:

[0035] The present invention provides an antique blue brick prepared by mixing purple clay and solid waste, which has a compressive strength greater than 35MP and a water absorption rate less than 10%, and the sample shrinkage ratio, loss on ignition and other parameters can meet the national standard requirements, and can be used for house wall construction; and by simultaneously utilizing purple clay and solid waste resources, it can not only solve the problem of solid waste disposal, but also promote the green upgrading of the traditional purple clay industry while driving the recycling of solid waste resources, solve the worries about the development of the energy industry, and realize the complementary linkage between industries in the region, which is of great significance to the overall industrial quality improvement and efficiency enhancement and green development of Yan'an City. DETAILED DESCRIPTION

[0036] The following examples are given to further illustrate the present invention in detail.

[0037] Since Yan'an has rich purple clay resources, the distribution is relatively concentrated, and the covering layer is thin and easy to mine. The chemical composition of Yan'an purple clay is mainly SiO 2 、Al 2 O 3 , Fe 2 O 3 Mainly, among which SiO 2 :60.56%~61.99%, average 61.37%; Al 2 O 3 :15.98%~17.37%, average 16.69%; Fe 2 O 3 The content is relatively high, 6.34% to 7.54%, with an average of 6.78%; TiO 2 Content 1.08%~1.44%, average 1.23%; K 2 The O content is moderate, 1.88% to 3.63%, with an average of 2.42%; the CaO content is low, 0.23% to 0.58%, with an average of 0.39%; the MgO content is 2.45% to 2.88%, with an average of 2.68%; 2 O content is low 0.21~0.68%, average 0.38%. 2 A moderate O content is beneficial to lowering the firing temperature, and a low CaO content is beneficial to preventing blistering and deformation during firing.

[0038] At the same time, Yan'an is an important national comprehensive energy base with many coal mines and thermal power plants. During the production process, a large amount of solid waste such as coal gangue, fly ash, slag, desulfurized gypsum, etc. will be generated. With the advancement of science and technology and industrial development, these solid wastes will also become available resources and be utilized. Among them, the chemical composition of fly ash includes SiO 2 :56.10%、Al 2 O 3 :24.50%、Fe 2 O 3 :5.01%、TiO 2 :0979%、K 2 O: 1.91%, CaO: 5.40%, MgO: 1.14%, Na 2 O: 0.80%. The chemical composition of coal gangue includes SiO 2 :52.30%、Al 2 O 3 :26.03%、Fe 2 O 3 :2.66%、TiO 2 :0.49%、K 2 O: 2.13%, CaO: 0.28%, MgO: 0.33%, Na 2 O: 0.41%.

[0039] After analysis, the above-mentioned Yan'an purple clay, coal gangue and fly ash are all suitable for the preparation of antique blue bricks. Therefore, how to use Yan'an purple clay and solid waste resources to develop industries and solve the problem of solid waste disposal at the same time, promote the green upgrading of the traditional purple clay industry while driving the recycling of solid waste resources, solve the worries of energy industry development, realize the complementary linkage between industries in the region, and promote the overall quality improvement, efficiency enhancement and green development of Yan'an City's industries, is an urgent problem to be solved.

[0040] Against this background technology, the present application discloses an antique blue brick based on a mixture of purple clay and solid waste. By utilizing purple clay and solid waste resources at the same time, it can not only solve the problem of solid waste disposal, but also promote the green upgrade of the traditional purple clay industry while driving the recycling of solid waste resources, solving the worries of the development of the energy industry and realizing the complementary linkage between industries in the region.

[0041] The antique blue brick made of purple clay and solid waste disclosed in the embodiment of the present invention comprises the following raw materials: purple clay, coal gangue and water; the antique blue brick is made by dry pressing process, and the length, width and height of the antique blue brick are 235-240mm*115-120mm*43-50mm; wherein the purple clay is 2.5-4 parts, the coal gangue is 1-2.5 parts, and the water is 0.35-0.4 parts. The preparation method of the antique blue brick in this embodiment is as follows:

[0042] 1) Weigh purple clay and coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0043] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0044] 3) Weigh water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and store the mixed raw material in a warehouse for aging, and the aging time is not less than 12 hours;

[0045] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0046] 5) The wet bricks are transported to the drying kiln by a kiln truck for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 240-245mm*120-125mm*45-55mm;

[0047] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0048] The green brick reduction process is to evenly spray natural gas in the kiln in an oxygen-deficient environment without igniting the kiln for 12-13 hours to form a reducing atmosphere in the kiln, and then spray tap water into the kiln for 24 hours. After the temperature in the kiln drops to 350°C, stop spraying tap water.

[0049] It should be noted that during the firing process, the iron element in the brick will generate red ferric oxide under an oxidizing atmosphere. By controlling the reducing atmosphere and cooling method, the ferric oxide can be reduced to bluish-gray ferrous oxide, making the brick appear bluish.

[0050] In one embodiment, the antique blue brick has a compressive strength greater than 35MP and a water absorption rate less than 10%.

[0051] Another preferred embodiment of the present invention provides an antique blue brick made of purple clay and solid waste, comprising the following raw materials: purple clay, fly ash and water; the antique blue brick is made by dry pressing process, and the length, width and height of the antique blue brick are 235-240mm*115-120mm*43-50mm; wherein the purple clay is 2.5-4 parts, the fly ash is 1-2.5 parts, and the water is 0.35-0.4 parts. The preparation method of the antique blue brick in this embodiment is as follows:

[0052] 1) Weigh purple clay and fly ash according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0053] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0054] 3) Weigh water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and store the mixed raw material in a warehouse for aging, and the aging time is not less than 12 hours;

[0055] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0056] 5) The wet bricks are transported to the drying kiln by a kiln truck for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 240-245mm*120-125mm*45-55mm;

[0057] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0058] The green brick reduction process is to evenly spray natural gas in the kiln in an oxygen-deficient environment without igniting the kiln for 12-13 hours to form a reducing atmosphere in the kiln, and then spray tap water into the kiln for 24 hours. After the temperature in the kiln drops to 350°C, stop spraying tap water.

[0059] It should be noted that during the firing process, the iron element in the brick will generate red ferric oxide under an oxidizing atmosphere. By controlling the reducing atmosphere and cooling method, the ferric oxide can be reduced to bluish-gray ferrous oxide, making the brick appear bluish.

[0060] In one embodiment, the antique blue brick has a compressive strength greater than 35MP and a water absorption rate less than 10%.

[0061] Another preferred embodiment of the present invention provides an antique blue brick made of purple clay and solid waste, comprising the following raw materials: purple clay, coal gangue and water; the antique blue brick is made by extrusion molding process, and the length, width and height of the antique blue brick are 190-200mm*90-100mm*39-41mm; wherein the purple clay is 2.5-3.5 parts, the fly ash is 1.5-2.5 parts, and the water is 0.4-0.45 parts. The preparation method of the antique blue brick in this embodiment is as follows:

[0062] 1) Weigh purple clay and coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0063] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0064] 3) Weigh water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and store the mixed raw material in a warehouse for aging, and the aging time is not less than 12 hours;

[0065] 4) Extruding the aged mixed raw materials into a warehouse by an extruder to obtain wet bricks, and testing the color and strength of the wet bricks;

[0066] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 200-205mm*100-105mm*41-43mm.

[0067] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0068] The green brick reduction process is to evenly spray natural gas in the kiln in an oxygen-deficient environment without igniting the kiln for 12-13 hours to form a reducing atmosphere in the kiln, and then spray tap water into the kiln for 24 hours. After the temperature in the kiln drops to 350°C, stop spraying tap water.

[0069] It should be noted that during the firing process, the iron element in the brick will generate red ferric oxide under an oxidizing atmosphere. By controlling the reducing atmosphere and cooling method, the ferric oxide can be reduced to bluish-gray ferrous oxide, making the brick appear bluish.

[0070] In one embodiment, the antique blue brick has a compressive strength greater than 35MP and a water absorption rate less than 10%.

[0071] In the embodiments of the present invention, by utilizing purple clay and solid waste resources, not only can the problem of solid waste disposal be solved, but also the green upgrading of the traditional purple clay industry can be promoted while driving the recycling of solid waste resources, effectively solving the worries about the development of the energy industry and realizing the complementary linkage between industries in the region, which is of great significance to the overall quality improvement and efficiency enhancement of Yan'an's industry and green development.

[0072] The technology of antique blue bricks based on purple clay and solid waste blended according to the present invention is further described below by listing specific embodiments.

[0073] Example 1

[0074] Antique blue bricks are prepared using purple clay, coal gangue and water as raw materials and are made using a dry pressing process. The preparation method is as follows:

[0075] 1) Weigh 80% of purple clay and 20% of coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0076] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0077] 3) Weigh 8% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0078] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0079] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 242mm*122mm*47mm.

[0080] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0081] In this implementation, purple clay accounts for 80% and coal gangue accounts for 20%. The finished antique blue brick has a shrinkage ratio of 10.5%, a water absorption rate of 5.3%, and a compressive strength of 45.3MP, all of which can meet national standard requirements.

[0082] Example 2

[0083] Antique blue bricks are prepared using purple clay, coal gangue and water as raw materials and are made using a dry pressing process. The preparation method is as follows:

[0084] 1) Weigh 70% of purple clay and 30% of coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0085] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0086] 3) Weigh 8% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0087] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0088] 5) The wet bricks are transported to the drying kiln by a kiln truck for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 243mm*123mm*44mm;

[0089] 6) Transport the dry bricks to 60m 3The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0090] In this implementation, purple clay accounts for 70% and coal gangue accounts for 30%. The finished antique blue brick has a shrinkage ratio of 3.9%, a water absorption rate of 4.7%, and a compressive strength of 40.1MP, all of which can meet national standard requirements.

[0091] Example 3

[0092] Antique blue bricks are prepared using purple clay, coal gangue and water as raw materials and are made using a dry pressing process. The preparation method is as follows:

[0093] 1) Weigh 50% of purple clay and 50% of coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0094] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0095] 3) Weigh 9% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0096] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0097] 5) The wet bricks are transported to the drying kiln by a kiln loading vehicle for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 244mm*123mm*49mm.

[0098] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0099] In this implementation, purple clay accounts for 80% and coal gangue accounts for 20%. The finished antique blue brick has a shrinkage ratio of 5.6%, a water absorption rate of 5.5%, and a compressive strength of 35.1MP, all of which can meet national standard requirements.

[0100] Example 4

[0101] Antique blue bricks are prepared using purple clay, fly ash and water as raw materials and dry pressed. The preparation method is as follows:

[0102] 1) Weigh 80% of purple clay and 20% of fly ash according to the proportion, and stir and mix them evenly with a mixer (during stirring, the power of the mixer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0103] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0104] 3) Weigh 9% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0105] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0106] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 243mm*123mm*52mm.

[0107] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0108] In this implementation, purple clay accounts for 80% and fly ash accounts for 20%. The finished antique blue brick has a shrinkage ratio of 13.1%, a water absorption rate of 7.2%, and a compressive strength of 36.6MP, all of which can meet national standard requirements.

[0109] Example 5

[0110] Antique blue bricks are prepared using purple clay, fly ash and water as raw materials and dry pressed. The preparation method is as follows:

[0111] 1) Weigh 70% of purple clay and 30% of fly ash according to the proportion, and stir and mix them evenly with a mixer (during stirring, the power of the mixer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0112] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0113] 3) Weigh 8% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0114] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0115] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 244mm*123mm*53mm.

[0116] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0117] In this implementation, purple clay accounts for 70% and fly ash accounts for 30%. The finished antique blue brick has a shrinkage ratio of 15%, a water absorption rate of 5%, and a compressive strength of 41.5MP, all of which can meet national standard requirements.

[0118] Example 6

[0119] Antique blue bricks are prepared using purple clay, fly ash and water as raw materials and dry pressed. The preparation method is as follows:

[0120] 1) Weigh 50% of purple clay and 50% of fly ash according to the proportion, and stir and mix them evenly with a mixer (during stirring, the power of the mixer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0121] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0122] 3) Weigh 9% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0123] 4) Dry-pressing the aged mixed raw materials into a dry press to obtain wet bricks, and testing the color and strength of the wet bricks;

[0124] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 244mm*124mm*49mm.

[0125] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0126] In this implementation, purple clay accounts for 50% and fly ash accounts for 50%. The finished antique blue brick has a shrinkage ratio of 19.6%, a water absorption rate of 9.3%, and a compressive strength of 47.5MP, all of which can meet national standard requirements.

[0127] Example 7

[0128] Antique blue bricks are prepared using purple clay, coal gangue and water as raw materials and are made using an extrusion process. The preparation method is as follows:

[0129] 1) Weigh 70% of purple clay and 30% of coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0130] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0131] 3) Weigh 8% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0132] 4) Extruding the aged mixed raw materials into a warehouse by an extruder to obtain wet bricks, and testing the color and strength of the wet bricks;

[0133] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 209mm*101mm*42mm.

[0134] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0135] In this implementation, purple clay accounts for 70% and coal gangue accounts for 30%. The finished antique blue brick has a shrinkage ratio of 11.2%, a water absorption rate of 3.0%, and a compressive strength of 45MP, all of which can meet national standard requirements.

[0136] Example 8

[0137] Antique blue bricks are prepared using purple clay, coal gangue and water as raw materials and are made using an extrusion process. The preparation method is as follows:

[0138] 1) Weigh 50% of purple clay and 50% of coal gangue according to the proportion, and stir and mix them evenly with a stirrer (during stirring, the power of the stirrer is 1500 kilowatts, and the stirring is divided into 3 times, each stirring for 15 minutes) to obtain a mixed coarse material;

[0139] 2) crushing the coarse mixed material (crushing method is crushing by a breaker or a crusher), and sieving the crushed mixed material through a 14-mesh drum screen to obtain a mixed fine material;

[0140] 3) Weigh 9% water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and put the mixed raw material into a warehouse for aging, and the aging time is not less than 12 hours;

[0141] 4) Extruding the aged mixed raw materials into a warehouse by an extruder to obtain wet bricks, and testing the color and strength of the wet bricks;

[0142] 5) The wet bricks are transported to the drying kiln for drying by a kiln loading vehicle. The frequency of the drying kiln is in the range of 30HZ-40HZ. The moisture content of the bricks is dried to less than 2% to obtain dry bricks. The length, width and height of the dry bricks are 208mm*101mm*43mm.

[0143] 6) Transport the dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

[0144] In this implementation, purple clay accounts for 50% and coal gangue accounts for 50%. The finished antique blue brick has a shrinkage ratio of 13.2%, a water absorption rate of 3.4%, and a compressive strength of 52.1MP, all of which can meet national standard requirements.

[0145] The above is only a preferred embodiment of the present invention. It should be pointed out that a person skilled in the art can make several modifications and improvements without departing from the inventive concept of the present invention, which all belong to the protection scope of the present invention.

Claims

1. An antique blue brick based on purple clay and solid waste, characterized in that: The antique blue brick is composed of the following raw materials: 2.5-4 parts of purple clay, 1-2.5 parts of coal gangue or fly ash and 0.35-0.4 parts of water; the antique blue brick is made by dry pressing process, and the length, width and height of the antique blue brick are 235-240mm*115-120mm*43-50mm.

2. An antique blue brick based on purple clay and solid waste as claimed in claim 1, characterized in that: The antique blue brick is composed of the following raw materials: 2.5-3.5 parts of purple clay, 1.5-2.5 parts of coal gangue and 0.4-0.45 parts of water; the antique blue brick is made by an extrusion molding process, and the length, width and height of the antique blue brick are 190-200mm*90-100mm*39-41mm.

3. The antique blue brick based on purple clay and solid waste blended according to claim 1 or 2, characterized in that: The chemical composition of the purple sand pottery clay includes SiO2: 60.56% to 61.99%, Al2O3: 15.98% to 17.37%, Fe2O3: 6.34% to 7.54%, TiO2: 1.08% to 1.44%, K2O: 1.88% to 3.63%, CaO: 0.23% to 0.58%, MgO: 2.45% to 2.88%, and Na2O: 0.21% to 0.68%.

4. The antique blue brick based on purple clay and solid waste blended according to claim 2 is characterized by: The chemical composition of the fly ash includes SiO2: 56.10%, Al2O3: 24.50%, Fe2O3: 5.01%, TiO2: 0979%, K2O: 1.91%, CaO: 5.40%, MgO: 1.14%, and Na2O: 0.80%.

5. The antique blue brick based on purple clay and solid waste blended according to claim 2 is characterized by: The chemical composition of the coal gangue includes SiO2: 52.30%, Al2O3: 26.03%, Fe2O3: 2.66%, TiO2: 0.49%, K2O: 2.13%, CaO: 0.28%, MgO: 0.33%, and Na2O: 0.41%.

6. The antique blue brick based on purple clay and solid waste blended soil according to any one of claims 1 to 5, characterized in that: The compression strength of the antique blue brick is greater than 35MP and the water absorption rate is less than 10%.

7. An antique blue brick based on purple clay and solid waste as claimed in claim 1, prepared by dry pressing process, characterized in that: The preparation method comprises the following steps: The excavated purple clay is aged and weathered for at least 1 month; Weigh purple clay, coal gangue or fly ash according to proportion, and stir and mix them evenly with a mixer to obtain a mixed coarse material; The mixed coarse material is crushed, and the crushed mixed material is sieved using a 14-mesh drum screen to obtain a mixed fine material; Weigh water according to the proportion and add it to the mixed fine material and stir evenly to obtain a mixed raw material, and store the mixed raw material in a warehouse for aging, and the aging time is not less than 12 hours; The aged mixed raw materials in the warehouse are dry pressed into shape by a dry press to obtain wet bricks, and the color and strength of the wet bricks are tested; The wet bricks are transported to the drying kiln by a kiln truck for drying. The frequency of the drying kiln is in the range of 30HZ-40HZ, and the moisture content of the bricks is dried to less than 2% to obtain dry bricks. Transport dry bricks to 60m 3 The shuttle kiln is used for firing, with the maximum firing temperature of 960℃ and the firing time of 108 hours. Calculated from the time of ignition, the temperature in the kiln rises to 200℃ within 48 hours, and then rises to 960℃ within 60 hours, reaching the maximum temperature. After keeping warm for 8 hours, the fired bricks are restored to green color by the green brick reduction process, and the kiln temperature is reduced to 100℃ before being taken out of the kiln to obtain the finished antique green bricks.

8. The method for preparing antique blue bricks by dry pressing process according to claim 7, characterized in that: The mixed coarse material is crushed by a breaker hammer or a crusher.

9. The method for preparing antique blue bricks by dry pressing process according to claim 7, characterized in that: The power of the mixer is 1500 kilowatts, and the stirring is divided into 3 times, each time for 15 minutes.

10. The method for preparing antique blue bricks by dry pressing process according to claim 7, characterized in that: The green brick reduction process is to evenly spray natural gas in the kiln in an oxygen-deficient environment without igniting the kiln for 12-13 hours to form a reducing atmosphere in the kiln, and then spray tap water into the kiln for 24 hours. After the temperature in the kiln drops to 350°C, stop spraying tap water.

Citation Information

Patent Citations

  • Grey brick mechanically manufactured from lime sludge and construction wastes and method for manufacturing same

    CN101519292A

  • Fly ash archaized black brick

    CN106278078A

  • Raw material formula for preparing decorating tile from coal gangue and preparation

    CN101475343A

  • Multicolor rustic brick and preparation method thereof

    CN102503360A

  • Production method of environment-friendly antiqued black bricks

    CN103351152A