Preparation method of transparent aluminum nitride ceramic substrate

Through the sintering process of high-purity materials and the transparent light-transmissive layer composite technology, the problem of insufficient brittleness and transparency of aluminum nitride ceramic substrates is solved, and a ceramic substrate with high strength and excellent optical properties is prepared, which is suitable for high mechanical strength and Applications with excellent optical performance.

CN118978403AInactive Publication Date: 2024-11-19FUJIAN HUAQING ELECTRONICS MATERIAL TECH
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411130504.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing aluminum nitride ceramic substrates have insufficient brittleness and transparency, which limits them in applications where high mechanical strength and excellent optical properties are required.

Method used

Using the mixing and sintering process of high-purity aluminum nitride powder, zirconia powder, alumina powder and other materials, combined with the composite technology of transparent light-transmitting layer, it is prepared by drying, sintering and surface treatment. Performance ceramic substrate.

Benefits of technology

The mechanical strength and optical properties of the aluminum nitride ceramic substrate are improved, their transmittance to light is enhanced, their reflection and absorption of light are reduced, and a protective layer is provided to prevent mechanical damage and contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118978403A_ABST
    Figure CN118978403A_ABST
Patent Text Reader

Abstract

The invention relates to a preparation method of a transparent aluminum nitride ceramic substrate, and belongs to the technical field of aluminum nitride ceramic substrates, and the preparation method comprises the following steps: S1, selecting raw materials: selecting high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, a stabilizer, a binder, a surfactant and a sintering aid; s2, mixing and sampling the raw materials, namely mixing the high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, a stabilizer, a binder, a surfactant and a sintering aid selected in the step S1 according to a certain proportion, controlling the mixing time, and after mixing is completed, sampling and inspecting the mixture to obtain a sample; checking whether the uniformity and the particle size distribution meet requirements or not; s3, molding the raw materials: putting the mixed raw materials in the step S2 into molding equipment, and making the mixed raw materials into a green body with a certain shape and size; the high-strength transparent light-transmitting glass has the advantages of high strength, transparency and light-transmitting performance at the same time.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of aluminum nitride ceramic substrates, and in particular to a method for preparing a transparent aluminum nitride ceramic substrate. Background Art

[0002] Aluminum nitride ceramics are a type of ceramic material with aluminum nitride (AIN) as the main crystal phase. It has many excellent physical and chemical properties. The following is a detailed introduction to aluminum nitride ceramics. Chemical formula: AlN, structure: AIN crystals use 〔AIN4〕tetrahedron as the structural unit, covalent bond compounds, have a wurtzite structure, and belong to the hexagonal crystal system. Color and transparency: white or grayish white, single crystal is colorless and transparent, specific gravity: 3.261g / cm³, thermal expansion coefficient: (4.0-6.0)×10^-6 / ℃, thermal conductivity: The thermal conductivity of polycrystalline AIN is 260W / (mk), and the thermal conductivity of aluminum nitride ceramics is about 200-300 W / mK, and can even reach about 320W / m·K, which is close to BeO and SiC, and more than 5 times that of Al2O3. Sublimation decomposition temperature: The sublimation decomposition temperature under normal pressure is 2450℃, and it can withstand extreme heat of 2200℃. Aluminum nitride ceramics have a high melting point of about 2200℃, which makes it have good stability in high temperature environments. High thermal conductivity is one of the most significant characteristics of aluminum nitride ceramics, which makes it have great advantages in the fields of heat dissipation materials and heating elements. Aluminum nitride ceramics can resist the erosion of chemical substances such as acids, alkalis, and salts, but are easily corroded in alkaline solutions.

[0003] Aluminum nitride ceramics are widely used in heat sinks, substrates and packaging materials in electronic devices due to their excellent thermal conductivity, especially in the fields of LED lighting, power modules, semiconductor manufacturing equipment, etc. The high thermal conductivity and low dielectric constant of aluminum nitride ceramics make it an ideal material for microwave equipment and used to manufacture substrates and packages for microwave circuits. In the aerospace field, the high temperature resistance, light weight and wear resistance of aluminum nitride ceramics make them an ideal choice for engine components, thermal protection systems and other key structures. With the development of electric vehicles and hybrid vehicles, aluminum nitride ceramics are used to manufacture automotive cooling modules and motor components due to their excellent thermal conductivity. In short, the application field of aluminum nitride ceramics is very wide. The existing aluminum nitride ceramic substrates are brittle and have low strength. They are prone to cracking when subjected to external forces. This characteristic limits their application in situations where high mechanical strength is required. In addition, the transparency and light transmittance of the existing aluminum nitride ceramic substrates need to be improved. Summary of the invention

[0004] In order to overcome the technical defects of the prior art, the present invention provides a method for preparing a transparent aluminum nitride ceramic substrate. The prepared ceramic substrate has the advantages of high strength and transparency and light transmittance.

[0005] The technical solution adopted by the present invention is: comprising the following steps: Step S1: selecting raw materials, including high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, stabilizer, binder, surfactant and sintering aid; Step S2: mixing and sampling of raw materials, mixing the high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, stabilizer, binder, surfactant and sintering aid selected in step S1 in a certain proportion, and controlling the mixing time. After the mixing is completed, sampling and testing the mixture to check whether its uniformity and particle size distribution meet the requirements; Step S3: raw material molding, placing the raw materials mixed in step S2 into a molding device to mold the mixed raw materials into a green body with a certain shape and size; Step S4: drying, removing moisture from the body of the body in step S3 through a drying device, and controlling the drying temperature and drying time; Step S5: sintering; placing the green body dried in step S4 into a sintering device for sealed sintering, and controlling the sintering temperature, holding time and pressure, and using an inert gas as a protective atmosphere to produce a ceramic substrate; Step S6: post-processing process, performing surface treatment on the ceramic substrate manufactured in step S5; Step S7: manufacturing and installing a transparent light-transmitting layer, first manufacturing a transparent light-transmitting layer, and then compounding the manufactured transparent light-transmitting layer onto the ceramic substrate in step S6; Step S8: Testing and evaluation: testing the ceramic substrate manufactured in step S7.

[0006] Preferably, in step S1, high-purity aluminum nitride powder is prepared by carbon thermal reduction method, high-purity aluminum oxide and carbon powder are evenly mixed in a ratio of 95%:5%, and then the aluminum oxide and carbon are reduced in a heating furnace at 1800 degrees. After the reaction is completed, it is cooled under nitrogen protection, and crushed and graded to obtain high-purity aluminum nitride powder.

[0007] Preferably, in step S2, the high-purity aluminum nitride powder accounts for 80%, the zirconium oxide powder accounts for 5%, the aluminum oxide powder accounts for 10%, the stabilizer accounts for 1%, the binder accounts for 1%, the surfactant accounts for 1%, and the sintering aid accounts for 2%. The above materials are mixed by a mixer for 5-8 hours. When the materials are mixed, the environment should be kept clean to avoid the introduction of impurities. At the same time, the purity and quality of all raw materials should be ensured to meet the requirements to avoid adverse effects on the performance of the final product. After the raw materials are mixed, a certain amount of samples are randomly taken out from the mixed raw materials to check whether their uniformity and particle size distribution meet the requirements. If they do not meet the requirements, continue mixing, otherwise stop mixing.

[0008] Preferably, in step S3, the molding equipment is one of a tape casting machine, a compression molding machine, an isostatic pressing machine and an injection molding machine.

[0009] Preferably, in step S4, when the moisture in the embryo is removed by the drying equipment, the temperature of the drying equipment is controlled between 100 degrees and 145 degrees, and the drying time is controlled at about 30 minutes. During the drying process of the embryo, the embryo should avoid direct contact with the high-temperature metal surface or other heat source to prevent local overheating from causing deformation or cracking. After the drying is completed, the embryo should be inspected to ensure that the embryo has no defects such as deformation and cracking.

[0010] Preferably, in step S5, when the embryo is sintered, the sintering temperature is between 1700 degrees and 2200 degrees, the heat preservation sintering time is controlled between 1.5 hours and 2 hours, and the embryo is pressurized during sintering, wherein the pressure is 1.2 GPa, and the inert gas in step S5 is nitrogen.

[0011] Preferably, in step S6, when processing the surface of the ceramic substrate, a grinder is used to grind the surface of the ceramic substrate, and a polishing device is used to polish the surface of the ceramic substrate. The surface of the ceramic substrate is made relatively smooth and flat by grinding and polishing. There is dust on the surface of the ceramic substrate after grinding, and the dust on the surface of the ceramic substrate is removed by cleaning.

[0012] Preferably, in step S7, the transparent light-transmitting layer is made of high-purity glass raw materials. The specific production method is: first, the high-purity glass raw materials are crushed by a crushing device, and the crushing effect of the high-purity glass raw materials must also be ensured. After the high-purity glass raw materials are crushed, they are screened by a screening device to ensure the uniformity and consistency of the high-purity glass raw materials. The pretreated high-purity glass raw materials are sent to a glass melting furnace, and are uniformly melted and mixed under high temperature conditions, wherein the temperature is controlled between 1700 degrees and 1850 degrees. During the melting process, impurities and bubbles in the high-purity glass raw materials will gradually float up and be removed. Thereafter, the transparent light-transmitting layer is produced after processing steps such as molding, annealing and cutting. After the transparent light-transmitting layer is cut into a shape matching the ceramic substrate, the transparent light-transmitting layer is composited to the ceramic substrate by using an adhesive, heat treatment to promote bonding, or mechanical fixing.

[0013] Preferably, in step S8, the detection method is to use appearance detection equipment to detect the surface flatness, cracks and bubbles, contamination and scratches of the ceramic substrate, use size detection equipment to detect the thickness, length and width of the ceramic substrate, and use performance detection equipment to test the thermal conductivity, thermal resistance, dielectric constant and surface resistance of the ceramic substrate, use bending strength testing equipment, hardness testing equipment and tensile testing equipment to test the bending strength, hardness and tensile strength of the ceramic substrate, and evaluate and analyze the ceramic substrate after detection.

[0014] The beneficial effects of the present invention are: The ceramic substrate prepared by the present invention has the advantage of high strength. The high strength enables the aluminum nitride ceramic substrate to bear greater weight and stress. At the same time, the ceramic substrate also has transparent light-transmitting properties, so that light can pass through the substrate more smoothly, reducing light reflection, scattering and absorption, thereby improving the overall optical performance. The transparent light-transmitting layer can serve as a protective layer to prevent the ceramic substrate from being mechanically damaged, scratched or contaminated during subsequent processing or use. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 The present invention is a flow chart of the preparation method.

[0016] Figure 2 This is a diagram showing the proportions of raw materials in the steps of mixing and sampling raw materials in the preparation method of the present invention.

[0017] Figure 3 The figure is a flow chart of the preparation of the transparent light-transmitting layer in the present invention. DETAILED DESCRIPTION

[0018] The present invention will be further described below in conjunction with the accompanying drawings: like Figure 1 Figure 3 As shown, this embodiment provides a method for preparing a transparent aluminum nitride ceramic substrate, comprising the following steps: 1: Selection of raw materials: high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, stabilizer, binder, surfactant and sintering aid. High-purity aluminum nitride powder is made by carbon thermal reduction method. High-purity aluminum oxide and carbon powder are evenly mixed in a ratio of 95%:5%. Then, aluminum oxide and carbon are reduced in a heating furnace at 1800 degrees. After the reaction, it is cooled under nitrogen protection, and crushed and graded to obtain high-purity aluminum nitride powder. The high thermal conductivity of aluminum nitride ceramic substrate is one of its significant features, and high-purity aluminum nitride powder can further ensure the high thermal conductivity of aluminum nitride ceramic substrate, and is conducive to heat dissipation, reducing thermal resistance, and improving the operating efficiency and stability of equipment. At the same time, high-purity aluminum nitride powder can improve the bending strength and hardness of aluminum nitride ceramic substrate, so that it has better mechanical properties. High-purity aluminum nitride powder has better sintering performance, which helps to form dense ceramic materials during the sintering process to meet the needs of high-precision products.

[0019] 2: Mixing and sampling of raw materials. The high-purity aluminum nitride powder, zirconium oxide powder, alumina powder, stabilizer, binder, surfactant and sintering aid selected in step S1 are mixed in a certain proportion and the mixing time is controlled. After the mixing is completed, the mixture is sampled and inspected to check whether its uniformity and particle size distribution meet the requirements. The high-purity aluminum nitride powder accounts for 80%, the zirconium oxide powder accounts for 5%, the alumina powder accounts for 10%, the stabilizer accounts for 1%, the binder accounts for 1%, the surfactant accounts for 1%, and the sintering aid accounts for 2%. The above materials are mixed by a mixer for 5-8 hours. When the materials are mixed, the environment should be kept clean to avoid the introduction of impurities, and at the same time, the purity and quality of all raw materials should be ensured to meet the requirements. In order to avoid adverse effects on the performance of the final product, after the raw materials are mixed, a certain amount of samples are randomly taken out from the mixed raw materials to check whether their uniformity and particle size distribution meet the requirements. If they do not meet the requirements, continue mixing, otherwise stop mixing. Alumina powder is an effective reinforcing agent. Its high toughness and good thermal stability help to improve the fragility of aluminum nitride ceramic substrates. Alumina is a commonly used reinforcing material and can be added to aluminum nitride ceramic substrates to improve their mechanical properties. Zirconia powder also has a high melting point and excellent chemical stability, which enables it to maintain stable performance under high temperature and harsh environment, further ensuring the reliability and durability of aluminum nitride ceramic substrates during use. The right amount of alumina can enhance the toughness and bending strength of the substrate. In summary, the strength of the ceramic substrate can be improved.

[0020] 3: Raw material molding, placing the raw materials mixed in step S2 into a molding device to make the mixed raw materials into a green body with a certain shape and size. The molding device is one of a tape casting machine, a compression molding machine, an isostatic pressing machine and an injection molding machine. The green body can be processed by the above equipment.

[0021] 4: Drying. The body in step S3 is passed through a drying device to remove moisture from the body, and the drying temperature and drying time are controlled. When the moisture in the body is removed through the drying device, the temperature of the drying device is controlled between 100 degrees and 145 degrees, and the drying time is controlled to be about 30 minutes. During the drying process of the body, the body should avoid direct contact with high-temperature metal surfaces or other heat sources to prevent local overheating from causing deformation or cracking. After drying, the body should be inspected to ensure that the body has no defects such as deformation and cracking. The moisture content of the body is reduced by drying to make it ready for subsequent sintering processes.

[0022] 5: Sintering; Place the dried green body in step S4 into a sintering device for sealed sintering, and control the sintering temperature, insulation time and pressure, and use an inert gas as a protective atmosphere to produce a ceramic substrate. When the green body is sintered, the sintering temperature is between 1700 degrees and 2200 degrees, and the insulation sintering time is controlled between 1.5 hours and 2 hours. During the sintering process of the green body, pressurization is performed, wherein the pressure is 1.2GPa. In step S5, the inert gas is nitrogen. The pores and impurities in the green body are removed by sintering, thereby improving the density of the ceramic substrate. Density is one of the important indicators for measuring the performance of ceramic materials. High-density ceramic substrates have better mechanical and thermal properties, and the performance of the ceramic substrate will be significantly improved during the sintering process. This includes hardness, strength, thermal conductivity and electrical insulation.

[0023] 6: Post-processing process, the ceramic substrate made in step S5 is subjected to surface treatment. When the surface of the ceramic substrate is treated, the surface of the ceramic substrate is ground by a grinder, and the surface of the ceramic substrate is polished by a polishing device. The surface of the ceramic substrate is relatively smooth and flat through grinding and polishing. There is dust on the surface of the ceramic substrate after grinding. The dust on the surface of the ceramic substrate is removed by cleaning. The original surface of the ceramic substrate is often uneven, with microscopic pits and protrusions. This uneven surface state will directly affect the performance of the ceramic substrate in subsequent applications. On the basis of grinding, polishing is performed to make its surface achieve extremely high smoothness and finish.

[0024] Step S7: preparation and installation of a transparent light-transmitting layer. First, a transparent light-transmitting layer is prepared, and then the prepared transparent light-transmitting layer is compounded onto the ceramic substrate in step S6. The transparent light-transmitting layer is prepared using high-purity glass raw materials. The specific preparation method is to first crush the high-purity glass raw materials through a crushing device, and at the same time, the crushing effect of the high-purity glass raw materials must be ensured. After the high-purity glass raw materials are crushed, they are screened through a screening device to ensure the uniformity and consistency of the high-purity glass raw materials. The pretreated high-purity glass raw materials are sent to a glass melting furnace for uniform melting and mixing under high temperature conditions, wherein the temperature is controlled between 1700 degrees and 1850 degrees. During the melting process, Impurities and bubbles in the high-purity glass raw material will gradually float up and be eliminated. After that, a transparent light-transmitting layer is produced through processing steps such as molding, annealing and cutting. After the transparent light-transmitting layer is cut into a shape matching the ceramic substrate, the transparent light-transmitting layer is compounded onto the ceramic substrate by using an adhesive, heat treatment to promote bonding or mechanical fixation. The transparent light-transmitting layer can significantly increase the transmittance of the ceramic substrate to light, allowing light to pass through the substrate more smoothly, reducing light reflection, scattering and absorption, thereby improving the overall optical performance. The transparent light-transmitting layer can serve as a protective layer to prevent the ceramic substrate from being mechanically damaged, scratched or contaminated during subsequent processing or use.

[0025] Step S8: Inspection and evaluation. The ceramic substrate produced in step S7 is inspected. In step S8, the inspection method is to use appearance inspection equipment to inspect the surface flatness, cracks and bubbles, pollution and scratches of the ceramic substrate, and use size inspection equipment to inspect the thickness, length and width of the ceramic substrate. At the same time, performance inspection equipment is used to test the thermal conductivity, thermal resistance, dielectric constant and surface resistance of the ceramic substrate. Bending strength testing equipment, hardness testing equipment and tensile testing equipment are used to test the bending strength, hardness and tensile strength of the ceramic substrate. Evaluation and analysis are carried out after the ceramic substrate is inspected. The above inspections can ensure the quality of the products.

[0026] When preparing a transparent aluminum nitride ceramic substrate, the user can first prepare the raw materials, which include aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, stabilizer, binder, surfactant and sintering aid. Then the user can mix the above raw materials through a mixer. After the mixing is completed, the mixture is sampled and inspected to check whether its uniformity and particle size distribution meet the requirements. The user places the mixed raw materials into a drying device, and removes moisture from the body through the drying device. After the body is dried, it is placed in a sintering device for sealed sintering, and the sintering temperature, insulation time and pressure are controlled. The inert gas is used as a protective atmosphere to produce a ceramic substrate. The surface of the ceramic substrate is then treated, and then a transparent light-transmitting layer can be produced. After the transparent light-transmitting layer is produced, the transparent light-transmitting layer is installed on the ceramic substrate. Finally, the user can test and evaluate the performance of the ceramic substrate.

[0027] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which shall fall within the scope of the present invention to be protected. The scope of protection of the present invention is defined by the attached claims and their equivalents.

Claims

1. A method for preparing a transparent aluminum nitride ceramic substrate, Features: The following steps are involved: Step S1: selecting raw materials, including high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, stabilizer, binder, surfactant and sintering aid; Step S2: mixing and sampling of raw materials, mixing the high-purity aluminum nitride powder, zirconium oxide powder, aluminum oxide powder, stabilizer, binder, surfactant and sintering aid selected in step S1 in a certain proportion, and controlling the mixing time. After the mixing is completed, sampling and testing the mixture to check whether its uniformity and particle size distribution meet the requirements; Step S3: raw material molding, placing the raw materials mixed in step S2 into a molding device to mold the mixed raw materials into a green body with a certain shape and size; Step S4: drying, removing moisture from the body of the body in step S3 through a drying device, and controlling the drying temperature and drying time; Step S5: sintering; placing the green body dried in step S4 into a sintering device for sealed sintering, and controlling the sintering temperature, holding time and pressure, and using an inert gas as a protective atmosphere to produce a ceramic substrate; Step S6: post-processing process, performing surface treatment on the ceramic substrate manufactured in step S5; Step S7: manufacturing and installing a transparent light-transmitting layer, first manufacturing a transparent light-transmitting layer, and then compounding the manufactured transparent light-transmitting layer onto the ceramic substrate in step S6; Step S8: Testing and evaluation: testing the ceramic substrate manufactured in step S7.

2. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In step S1, high-purity aluminum nitride powder is prepared by carbon thermal reduction method, high-purity aluminum oxide and carbon powder are evenly mixed in a ratio of 95%:5%, and then the aluminum oxide and carbon are reduced in a heating furnace at 1800 degrees. After the reaction is completed, it is cooled under nitrogen protection, and crushed and graded to obtain high-purity aluminum nitride powder.

3. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In the step S2, the high-purity aluminum nitride powder accounts for 80%, the zirconium oxide powder accounts for 5%, the aluminum oxide powder accounts for 10%, the stabilizer accounts for 1%, the binder accounts for 1%, the surfactant accounts for 1%, and the sintering aid accounts for 2%. The above materials are mixed by a mixer for 5-8 hours. After the raw materials are mixed, a certain amount of samples are randomly taken out from the mixed raw materials to check whether their uniformity and particle size distribution meet the requirements. If they do not meet the requirements, the mixing is continued, otherwise the mixing is stopped.

4. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In the step S3, the molding equipment is one of a tape casting machine, a compression molding machine, an isostatic pressing machine and an injection molding machine.

5. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In step S4, when the moisture in the embryo is removed by the drying equipment, the temperature of the drying equipment is controlled between 100 degrees and 145 degrees, and the drying time is controlled to be about 30 minutes. During the drying process of the embryo, the embryo should avoid direct contact with the high-temperature metal surface or other heat source. After the drying is completed, the embryo should be inspected to ensure that the embryo has no defects such as deformation and cracking.

6. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In the step S5, when the embryo is sintered, the sintering temperature is between 1700 degrees and 2200 degrees, the heat preservation sintering time is controlled between 1.5 hours and 2 hours, and the embryo is pressurized during the sintering process, wherein the pressure is 1.2 GPa, and the inert gas in the step S5 is nitrogen.

7. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In step S6, when processing the surface of the ceramic substrate, a grinder is used to grind the surface of the ceramic substrate, and a polishing device is used to polish the surface of the ceramic substrate. The surface of the ceramic substrate is made relatively smooth and flat by grinding and polishing. There is dust on the surface of the ceramic substrate after grinding, and the dust on the surface of the ceramic substrate is removed by cleaning.

8. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In step S7, the transparent light-transmitting layer is made of high-purity glass raw materials. The specific production method is as follows: first, the high-purity glass raw materials are crushed by a crushing device, and the crushing effect of the high-purity glass raw materials must also be ensured. After the high-purity glass raw materials are crushed, they are screened by a screening device to ensure the uniformity and consistency of the high-purity glass raw materials. The pretreated high-purity glass raw materials are sent to a glass melting furnace to be uniformly melted and mixed under high temperature conditions, wherein the temperature is controlled between 1700 degrees and 1850 degrees. During the melting process, impurities and bubbles in the high-purity glass raw materials will gradually float up and be removed. After that, the transparent light-transmitting layer is manufactured through processing steps such as molding, annealing and cutting. After the transparent light-transmitting layer is cut into a shape matching the ceramic substrate, the transparent light-transmitting layer is composited to the ceramic substrate by using an adhesive, heat treatment to promote bonding, or mechanical fixing.

9. The method for preparing the transparent aluminum nitride ceramic substrate according to claim 1, Features: In the step S8, the detection method is to use appearance detection equipment to detect the surface flatness, cracks and bubbles, pollution and scratches of the ceramic substrate, use size detection equipment to detect the thickness, length and width of the ceramic substrate, and use performance detection equipment to test the thermal conductivity, thermal resistance, dielectric constant and surface resistance of the ceramic substrate. Use bending strength testing equipment, hardness testing equipment and tensile testing equipment to test the bending strength, hardness and tensile strength of the ceramic substrate, and evaluate and analyze the ceramic substrate after testing.

Citation Information

Patent Citations

  • Ceramic fluorescent body capable of effectively eliminating edge aberration effect in white light LED light source packaging and preparation method thereof

    CN104112812A

  • LED flip chip package substrate and LED package structure

    CN106299084A

  • Particle dispersion toughened aluminum nitride ceramic substrate and preparation method thereof

    CN110436932A

  • Ceramic shell, preparation method thereof and electronic equipment

    CN113691664A

  • Dental cast porcelain and preparation method thereof

    CN118267302A