Chain extension type PVC paste resin, PVC foaming composite special material, foaming product, preparation method and application
By adding chain extender and acrylate monomer to the PVC paste resin, copolymerizing and combining with other additives, chain extending PVC paste resin is prepared, and the foaming ratio of PVC paste resin in foamed products in the prior art is solved. Due to the problem of difficult balance of mechanical properties, PVC foamed products with high tensile strength and compression permanent deformation are achieved.
Patent Information
- Application Number
- CN202411265388.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-10
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing PVC paste resins are difficult to balance the foaming ratio and mechanical properties in foamed products, resulting in insufficient performance of foamed products.
Using chain-extended PVC paste resin, copolymerizes vinyl chloride monomer with acrylate monomers, and adds chain-extended agent, surfactant and dispersion medium, and prepares by microsuspension method, combining inorganic fillers, plasticizers and foaming. The agent is prepared for high tensile strength and permanent compression deformation of PVC foaming composite materials, and high-temperature foaming.
The foaming ratio and mechanical properties are improved, and PVC foamed products with high tensile strength and permanent compression deformation are prepared, meeting the balance of performance and ratio.
Abstract
Description
Technical Field
[0001] The invention relates to the field of PVC foaming materials, and in particular to a chain-extended PVC paste resin, a PVC foaming composite special material, a foaming product, and a preparation method and application thereof. Background Art
[0002] Polyvinyl chloride (PVC) paste resin has the characteristics of stable performance and easy processing. It can be used to prepare foamed products by adding foaming agents, etc., and is widely used in the production of artificial leather, wallpaper, etc. However, there are still some problems with general PVC paste resin as a foaming raw material, such as the foaming ratio of foamed products needs to be improved, and the mechanical properties of foamed products are difficult to balance with the foaming ratio. The application of PVC paste resin in the field of foamed products needs further improvement. Summary of the invention
[0003] In view of the above-mentioned deficiencies in the prior art, the purpose of the present invention is to provide a chain-extended PVC paste resin, a PVC foam composite special material, a foamed product, and a preparation method and application thereof, aiming to solve the defects existing in the prior art when PVC paste resin is used as a raw material to prepare foamed products. The chain-extended PVC paste resin and the PVC foam composite special material provided in this application can be used to prepare PVC foamed products with good foaming properties and mechanical properties.
[0004] Specifically, the present invention provides the following technical solutions:
[0005] In a first aspect of the present invention, there is provided a chain-extended PVC paste resin, which is prepared by polymerizing the following raw materials:
[0006] 15 to 75 parts by weight of vinyl chloride monomer,
[0007] 10 to 70 parts by weight of acrylic acid ester monomers,
[0008] 3 to 7 parts by weight of a chain extender,
[0009] 0.5 to 1 parts by weight of an initiator,
[0010] 10 to 15 parts by weight of a surfactant, and
[0011] 60 to 90 parts by weight of a dispersion medium.
[0012] According to an embodiment of the present invention, the chain-extended PVC paste resin provided above may also include the following technical features:
[0013] According to an embodiment of the present invention, the acrylic acid ester monomer is selected from at least one of methyl acrylate, ethyl acrylate and butyl acrylate. Copolymerization of vinyl chloride monomer and acrylic acid ester monomer can reduce the melt viscosity, thereby making the prepared chain-extended PVC paste resin easy to foam and increasing the foaming ratio.
[0014] According to an embodiment of the present invention, the chain extender is at least one of diallyl phthalate (DAP), triallyl cyanurate (TAIC), and polyethylene glycol dimethacrylate. The chain extender containing multifunctionality is selected to prepare the chain-extended PVC paste resin, so that the molecular weight is increased and the molecular weight distribution is broadened, and the prepared foamed product has higher tensile strength and better compression permanent deformation.
[0015] According to an embodiment of the present invention, the initiator is at least one of di(2-ethylhexyl) peroxydicarbonate, benzoyl peroxide, azobisisoheptanenitrile, azobisisobutyronitrile, and ammonium persulfate.
[0016] According to an embodiment of the present invention, the surfactant is at least one of hexadecyltrimethylammonium bromide and sodium dodecyl sulfate.
[0017] According to an embodiment of the present invention, the dispersion medium is deionized water.
[0018] In a second aspect of the present invention, there is provided a method for preparing the chain-extended PVC paste resin described in the first aspect, which is prepared by a microsuspension method. According to an embodiment of the present invention, the method comprises mixing the raw materials to form an emulsion, polymerizing the emulsion at 50 to 55 degrees Celsius for 8 to 12 hours.
[0019] According to a specific embodiment, the method comprises: stirring at a rotation speed of 400 to 700 rpm for 40 to 50 minutes to prepare an emulsion, and then polymerizing at a temperature of 50 to 55° C. for 8 to 12 hours to obtain the chain-extended PVC paste resin.
[0020] In the third aspect of the present invention, a special PVC foam composite material is provided, comprising: the chain-extended PVC paste resin described in the first aspect and the chain-extended PVC paste resin obtained according to the preparation method described in the second aspect, an inorganic filler, a plasticizer, a foaming agent and a stabilizer.
[0021] According to an embodiment of the present invention, the inorganic filler is silicon dioxide.
[0022] According to an embodiment of the present invention, the plasticizer is selected from at least one of dioctyl phthalate (DOP), dibutyl phthalate (DBP), and diisononyl phthalate (DINP).
[0023] According to an embodiment of the present invention, the foaming agent is azodicarbonamide (AC) or a compound of azodicarbonamide and sodium bicarbonate.
[0024] According to an embodiment of the present invention, the stabilizer is at least one of a calcium-zinc composite stabilizer and a potassium-zinc composite stabilizer.
[0025] According to an embodiment of the present invention, the mass ratio of the chain-extended PVC paste resin, the inorganic filler, the plasticizer, the foaming agent, and the stabilizer is 100:1-3:60-70:3-5:1-3.
[0026] In the fourth aspect of the present invention, there is provided a use of the chain-extended PVC paste resin described in the first aspect, the chain-extended PVC paste resin obtained according to the preparation method described in the second aspect, and the PVC foam composite special material described in the third aspect in the field of foam products.
[0027] In the fifth aspect of the present invention, a foamed product is provided, which is prepared by mixing the chain-extended PVC paste resin described in the first aspect or the chain-extended PVC paste resin obtained according to the preparation method described in the second aspect, an inorganic filler, a plasticizer, a foaming agent and a stabilizer in a predetermined mass ratio and foaming the mixture at a high temperature of 200 to 210 degrees Celsius for 5 to 10 minutes.
[0028] According to an embodiment of the present invention, the predetermined mass ratio is 100:1-3:60-70:3-5:1-3 among the chain-extended PVC paste resin, inorganic filler, plasticizer, foaming agent and stabilizer.
[0029] The beneficial effects achieved by the present invention are at least:
[0030] The PVC paste resin and the PVC foam composite special material mentioned in the present invention increase the molecular weight of the PVC paste resin by adding a chain extender, broaden the molecular weight distribution, and are used in the preparation of foamed products, so that the prepared foamed products have higher tensile strength and better compression permanent deformation. In addition, by copolymerizing vinyl chloride monomers with acrylic acid ester monomers, the melt viscosity is reduced, so that the foaming ratio of the prepared foamed products is improved. DETAILED DESCRIPTION
[0031] Embodiments of the present invention are described in detail below. The embodiments are exemplary and intended to be used to explain the present invention, but should not be construed as limiting the present invention.
[0032] The present invention provides a chain-extended PVC paste resin, which is prepared by polymerizing the following raw materials:
[0033] 15 to 75 parts by weight of vinyl chloride monomer,
[0034] 10 to 70 parts by weight of acrylic acid ester monomers,
[0035] 3 to 7 parts by weight of a chain extender,
[0036] 0.5 to 1 parts by weight of an initiator,
[0037] 10 to 15 parts by weight of a surfactant, and
[0038] 60 to 90 parts by weight of a dispersion medium.
[0039] During the research, it was found that if the chain extender is not added, the molecular weight and molecular weight distribution of the prepared chain-extended PVC paste resin will be affected, and the mechanical properties of the foamed product will be affected; if the acrylic ester monomer is not added for copolymerization, the melt viscosity will be high, and it will not be easy to foam, which will affect the foaming ratio. If the quality of each raw material is too high or too low, for example, the quality of the chain extender is too high, cross-linking will occur, which will make the resin melt viscosity too high and the foaming ratio will be reduced; for example, if the quality of the acrylic ester monomer is too low, the melt viscosity will be high, which is not conducive to foaming.
[0040] According to a preferred embodiment, the chain-extended PVC paste resin is prepared by polymerizing the following raw materials, including: 50 to 75 parts by weight of vinyl chloride monomer, 20 to 50 parts by weight of acrylic acid ester monomer, 3 to 5 parts by weight of chain extender, 0.5 to 1 part by weight of initiator, 10 to 15 parts by weight of surfactant, and 60 to 90 parts by weight of dispersion medium.
[0041] According to a specific embodiment, the acrylic acid ester monomer includes but is not limited to at least one of methyl acrylate, ethyl acrylate, and butyl acrylate. According to a preferred embodiment, the acrylic acid ester monomer is butyl acrylate.
[0042] The chain extender mentioned includes but is not limited to diallyl phthalate (DAP), triallyl cyanurate (TAIC), polyethylene glycol dimethacrylate, etc. According to a preferred embodiment, the chain extender is triallyl cyanurate (TAIC).
[0043] The initiator mentioned includes but is not limited to di(2-ethylhexyl) peroxydicarbonate, benzoyl peroxide, azobisisoheptanitrile, azobisisobutyronitrile, ammonium persulfate, etc. According to a preferred embodiment, the initiator is azobisisoheptanitrile.
[0044] The surfactant mentioned includes but is not limited to hexadecyltrimethylammonium bromide, sodium lauryl sulfate, etc. According to a preferred embodiment, the surfactant is hexadecyltrimethylammonium bromide.
[0045] The dispersion medium mentioned is deionized water.
[0046] The chain-extended PVC paste resin can be prepared by a microsuspension method. According to a specific implementation, the raw materials are mixed, stirred at a speed of 400 to 700 rpm (stirring time is 40 to 50 minutes) to prepare an emulsion, and then polymerized at 50 to 55° C. for 8 to 12 hours.
[0047] According to a specific embodiment, the chain-extended PVC paste resin can be prepared by the following method:
[0048] (1) Add deionized water into a reaction kettle, raise the temperature to 70-75° C., add a surfactant, and stir at a speed of 600-700 r / min for 40-50 min;
[0049] (2) cooling after stirring, adding initiator, acrylic acid ester monomer, chain extender, and passing vinyl chloride monomer in an inert gas;
[0050] (3) stirring at a speed of 400 r / min, polymerizing at a temperature of 50-55° C. for 8-12 hours, removing unreacted vinyl chloride monomer, and obtaining the chain-extended PVC paste resin.
[0051] The chain-extended PVC paste resin mentioned above and the chain-extended PVC paste resin prepared according to the above method can be compounded with an inorganic filler, a plasticizer, a foaming agent and a stabilizer to prepare a special PVC paste resin foaming composite material.
[0052] According to a specific embodiment, the inorganic filler is silicon dioxide.
[0053] The plasticizer includes, but is not limited to, one of dioctyl phthalate (DOP), dibutyl phthalate (DBP), and diisononyl phthalate (DINP), and according to a preferred embodiment, it is dioctyl phthalate (DOP).
[0054] The foaming agent includes but is not limited to azodicarbonamide (AC) or a compound of azodicarbonamide and sodium bicarbonate. These substances can be used as foaming agents and can be decomposed at high temperature to generate gas for foaming.
[0055] The stabilizer mentioned includes but is not limited to calcium zinc composite stabilizer, potassium zinc composite stabilizer, etc. According to a preferred embodiment, it is a potassium zinc composite stabilizer.
[0056] The chain-extended PVC paste resin, inorganic filler, plasticizer, foaming agent and stabilizer can be mixed in a certain mass ratio. According to a specific implementation manner, the mass ratio of each raw material is 100:1-3:60-70:3-5:1-3. According to a preferred implementation manner, the mass ratio of each raw material is 100:2:65:5:3.
[0057] After the bubbles are removed from the chain-extended PVC paste resin foaming composite material in a vacuum environment, a film with uniform thickness is scraped on a glass sheet, and then placed in an oven for foaming to prepare a foamed product.
[0058] The foaming conditions are a temperature of 200-210° C. and a foaming time of 5-10 minutes. According to a preferred embodiment, the foaming time is 8 minutes.
[0059] The technical scheme of the present invention is described below by specific examples. It should be noted that these examples are only used to facilitate the understanding of those skilled in the art and should not be regarded as limiting the scope of protection of the present invention. Unless otherwise specified, the reagents used in the examples can be obtained commercially.
[0060] Example 1
[0061] Example 1: A chain-extended PVC paste resin, a foaming composite material and a corresponding foamed product are prepared by the following method, including:
[0062] 30g of deionized water was added to the reactor, and the temperature was raised to 70℃. 1g of surfactant sodium dodecyl sulfate (SDS) was added and stirring was started at a speed of 700r / min for 45min. After stirring, the mixture was cooled and 0.05g of initiator azobisisoheptanenitrile was added, and 3.7g of butyl acrylate and 0.3g of chain extender triallyl cyanurate (TAIC) were added according to the mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 60:37:3. Then, argon was passed to replace the air in the reactor, and 6g of vinyl chloride monomer was passed in. Stirring was started at a speed of 400r / min, the polymerization temperature was 55℃, and the polymerization time was 10h.
[0063] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0064] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0065] Example 2
[0066] Example 2: Chain-extended PVC paste resin, PVC foam composite special material and corresponding foamed products are prepared by the following method, including:
[0067] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add 1g of surfactant sodium dodecyl sulfate (SDS), start stirring, the speed is 700r / min, the stirring time is 45min, cool after stirring, add 0.05g of initiator azobisisoheptanenitrile into the reactor, according to the feeding mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 46:50:4, continue to add 5g of butyl acrylate and 0.4g of chain extender triallyl cyanurate (TAIC), then introduce argon to replace the air in the kettle, and introduce 4.6g of vinyl chloride monomer, start stirring, the speed is 400r / min, the polymerization temperature is 55℃, and the polymerization time is 10h.
[0068] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0069] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0070] Example 3
[0071] Example 3: A chain-extended PVC paste resin, a foaming composite material and corresponding foamed products are prepared by the following method, including:
[0072] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add 1g of surfactant sodium dodecyl sulfate (SDS), start stirring, the speed is 700r / min, the stirring time is 45min, cool it after stirring, add 0.05g of initiator azobisisoheptanenitrile into the reactor, according to the feeding mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 75:20:5, continue to add 2g of butyl acrylate, 0.5g of chain extender triallyl o-cyanurate (TAIC), then introduce argon to replace the air in the kettle, and introduce 7.5g of vinyl chloride monomer, start stirring, the speed is 400r / min, the polymerization temperature is 55℃, and the polymerization time is 8h.
[0073] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0074] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0075] Example 4
[0076] Example 4: A chain-extended PVC paste resin, a foaming composite material and a corresponding foamed product are prepared by the following method, including:
[0077] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add 1g of surfactant sodium dodecyl sulfate (SDS), start stirring, the speed is 700r / min, the stirring time is 45min, cool it after stirring, add 0.05g of initiator azobisisoheptanenitrile into the reactor, and continue to add 3.6g of butyl acrylate and 0.4g of chain extender polyethylene glycol dimethacrylate according to the feeding mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 60:36:4, then introduce argon to replace the air in the kettle, and introduce 6g of vinyl chloride monomer, start stirring, the speed is 400r / min, the polymerization temperature is 55℃, and the polymerization time is 8h.
[0078] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0079] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0080] Example 5
[0081] Example 5: A chain-extended PVC paste resin, a foaming composite material and corresponding foamed products are prepared by the following method, including:
[0082] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add 1g of surfactant sodium dodecyl sulfate (SDS), start stirring, the speed is 700r / min, the stirring time is 45min, cool it after stirring, add 0.05g of initiator azobisisoheptanenitrile into the reactor, according to the feeding mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 60:36:4, continue to add 3.6g of butyl acrylate and 0.4g of chain extender diallyl phthalate (DAP), then introduce argon to replace the air in the kettle, and introduce 6g of vinyl chloride monomer, start stirring, the speed is 400r / min, the polymerization temperature is 55℃, and the polymerization time is 10h.
[0083] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0084] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0085] Example 6
[0086] Example 6: A chain-extended PVC paste resin, a foaming composite material and corresponding foamed products are prepared by the following method, including:
[0087] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add 1g of surfactant sodium dodecyl sulfate (SDS), start stirring, the speed is 700r / min, the stirring time is 45min, cool after stirring, add 0.05g of initiator di(2-ethylhexyl) oxydicarbonate into the reactor, according to the feeding mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 60:36:4, continue to add 3.6g of butyl acrylate and 0.4g of chain extender triallyl cyanurate (TAIC), then introduce argon to replace the air in the kettle, and introduce 6g of vinyl chloride monomer, start stirring, the speed is 400r / min, the polymerization temperature is 55℃, and the polymerization time is 8h.
[0088] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0089] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0090] Example 7
[0091] Example 7: A chain-extended PVC paste resin, a foaming composite material and a corresponding foamed product are prepared by the following method, including:
[0092] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add 1g of surfactant hexadecyltrimethylammonium bromide and start stirring at a speed of 700r / min for 45min. Cool it after stirring, add 0.1g of initiator azobisisoheptanenitrile into the reactor, and continue to add 3.6g of butyl acrylate and 0.4g of chain extender triallyl cyanurate (TAIC) according to the feed mass ratio of vinyl chloride monomer: butyl acrylate: chain extender = 60:36:4. Then, introduce argon to replace the air in the kettle, and introduce 6g of vinyl chloride monomer, start stirring at a speed of 400r / min, the polymerization temperature is 55℃, and the polymerization time is 10h.
[0093] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0094] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0095] Comparative Example 1
[0096] Comparative Example 1: A chain-extended PVC paste resin, a foaming composite special material and a corresponding foamed product are prepared by the following method, including:
[0097] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add sodium dodecyl sulfate (SDS) emulsifier and start stirring at a speed of 700r / min for 45min. Cool after stirring, add 0.05g of azobisisoheptanenitrile as initiator into the reactor, add 4g of butyl acrylate at a feed mass ratio of vinyl chloride monomer: butyl acrylate = 60:40, then introduce argon to replace the air in the kettle, and introduce 6g of vinyl chloride monomer, start stirring at a speed of 400r / min, the polymerization temperature is 55℃, and the polymerization time is 10h.
[0098] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0099] The special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after uniform mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0100] Comparative Example 2
[0101] Comparative Example 2: A chain-extended PVC paste resin, a foaming composite special material and a corresponding foamed product are prepared by the following method, including:
[0102] Add 30g of deionized water into the polymerization kettle, heat it to 70℃, add sodium dodecyl sulfate (SDS) emulsifier and start stirring at a speed of 700r / min for 45min. Cool after stirring, add 0.05g of azobisisoheptanenitrile as initiator into the reactor, and continue to add 0.4g of chain extender triallyl cyanurate (TAIC) according to the feed mass ratio of vinyl chloride monomer: chain extender = 96:4. Then, replace the air in the kettle with argon, and introduce 9.6g of vinyl chloride monomer. Start stirring at a speed of 400r / min, polymerization temperature of 55℃, and polymerization time of 10h.
[0103] After the reaction is completed, the unreacted vinyl chloride monomer is removed, washed and dried to obtain a PVC copolymer, namely, a chain-extended PVC paste resin.
[0104] Then, a special foaming composite material is prepared according to the ratio of PVC copolymer: plasticizer DOP: foaming agent azodicarbonamide: potassium zinc composite stabilizer: silicon dioxide = 100:65:5:3:2, and after evenly mixing, vacuum degassing is carried out, and foaming is carried out in an oven at a foaming temperature of 210°C and a foaming time of 8 minutes to obtain a PVC foamed product.
[0105] The chain-extended PVC paste resins obtained in Examples 1-7 and Comparative Examples 1-2 were characterized by molecular weight, and the test results are shown in Table 1.
[0106] Table 1 Molecular weight and molecular weight distribution of chain-extended PVC paste resin
[0107] Mn (number average molecular weight) Mw (weight average molecular weight) PDI (polydispersity index) Example 1 <![CDATA[7.96×10 4 ]]> <![CDATA[1.69×10 4 ]]> 5.2 Example 2 <![CDATA[8.19×10 4 ]]> <![CDATA[1.88×10 4 ]]> 5.7 Example 3 <![CDATA[8.22×10 4 ]]> <![CDATA[2.90×10 4 ]]> 6.3 Example 4 <![CDATA[8.43×10 4 ]]> <![CDATA[3.76×10 4 ]]> 6.4 Example 5 <![CDATA[7.93×10 4 ]]> <![CDATA[1.98×10 4 ]]> 5.2 Example 6 <![CDATA[8.15×10 4 ]]> <![CDATA[2.57×10 4 ]]> 5.1 Example 7 <![CDATA[8.02×10 4 ]]> <![CDATA[2.15×10 4 ]]> 6.5 Comparative Example 1 <![CDATA[7.40×10 4 ]]> <![CDATA[1.78×10 4 ]]> 4.8 Comparative Example 2 <![CDATA[8.09×10 4 ]]> <![CDATA[3.09×10 4 ]]> 5.9
[0108] The foamed products obtained in Examples 1-7 and Comparative Examples 1-2 were subjected to a foaming ratio test and a mechanical property test (tensile properties were tested in accordance with GB / T 1040.3-2006). The test results are shown in Table 2.
[0109] Table 2 Foaming ratio and mechanical properties test
[0110] Foaming ratio Tensile strength(MPa) Compression set (%) Example 1 2.6 6.4 10.2 Example 2 2.9 6.8 9.3 Example 3 2.8 7.2 9.6 Example 4 2.8 7.5 9.5 Example 5 2.6 7.1 9.8 Example 6 2.7 6.1 10.7 Example 7 2.6 6.7 10.1 Comparative Example 1 2.3 3.4 14 Comparative Example 2 2.2 6.8 9.5
[0111] Combined with the results given in the above examples 1 to 7, it can be seen that the chain-extended PVC paste resin prepared by the present invention has a high number average molecular weight and a high weight average molecular weight, a wide molecular weight distribution, and the prepared foamed product has a high tensile strength and a good compression permanent deformation. The copolymerization with butyl acrylate makes the prepared foamed product have a high foaming ratio; while the chain-extended PVC paste resin prepared in comparative example 1 does not add a chain extender, and the number average molecular weight and the weight average molecular weight are both low, the molecular weight distribution is narrow, the tensile strength of the foamed product is low and the compression permanent deformation is poor. Comparative example 2 does not add an acrylic acid ester monomer, the number average molecular weight does not change much, the weight average molecular weight is high, the molecular weight distribution is wide, and the foaming ratio is low. The foaming ratio of the PVC foamed product prepared by the present invention is significantly higher than that of comparative examples 1 and 2, both of which are above 2.6. Moreover, the tensile strength of the prepared foamed product is significantly higher than that of comparative example 1, and the compression permanent deformation (%) is also significantly lower than that of comparative example 1.
[0112] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "specific implementation methods", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example.
[0113] Although the embodiments of the present invention have been shown and described above, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations of the present invention. A person skilled in the art may change, modify, replace and vary the above embodiments within the scope of the present invention.
Claims
1. A chain-extended PVC paste resin, characterized in that: Prepared by polymerizing the following raw materials: 15 to 75 parts by weight of vinyl chloride monomer, 10 to 70 parts by weight of acrylic acid ester monomers, 3 to 7 parts by weight of a chain extender, 0.5 to 1 parts by weight of an initiator, 10 to 15 parts by weight of a surfactant, and 60 to 90 parts by weight of a dispersion medium.
2. The chain-extended PVC paste resin according to claim 1, characterized in that: The acrylic acid ester monomer is selected from at least one of methyl acrylate, ethyl acrylate and butyl acrylate.
3. The chain-extended PVC paste resin according to claim 1, characterized in that: The chain extender is selected from at least one of diallyl phthalate (DAP), triallyl cyanurate (TAIC), and polyethylene glycol dimethacrylate.
4. The chain-extended PVC paste resin according to claim 1, characterized in that: The initiator is selected from at least one of di(2-ethylhexyl) peroxydicarbonate, benzoyl peroxide, azobisisoheptanenitrile, azobisisobutyronitrile and ammonium persulfate.
5. The chain-extended PVC paste resin according to claim 1, characterized in that: The surfactant is selected from at least one of hexadecyltrimethylammonium bromide and sodium dodecyl sulfate; Optionally, the dispersion medium is deionized water.
6. The method for preparing the chain-extended PVC paste resin according to any one of claims 1 to 5, characterized in that: The raw materials are mixed to form an emulsion, and polymerization is carried out at a temperature of 50 to 55° C. for 8 to 12 hours to obtain the chain-extended PVC paste resin.
7. A special PVC foam composite material, characterized in that: include: The chain-extended PVC paste resin according to any one of claims 1 to 5, and the chain-extended PVC paste resin, inorganic filler, plasticizer, foaming agent and stabilizer obtained by the preparation method according to claim 6.
8. The PVC foam composite material according to claim 7, characterized in that: The inorganic filler is silicon dioxide; Optionally, the plasticizer is selected from at least one of dioctyl phthalate, dibutyl phthalate, and diisononyl phthalate; Optionally, the foaming agent is azodicarbonamide or a compound of azodicarbonamide and sodium bicarbonate; Optionally, the stabilizer is selected from at least one of a calcium zinc composite stabilizer and a potassium zinc composite stabilizer; Optionally, the mass ratio of the chain-extended PVC paste resin, inorganic filler, plasticizer, foaming agent and stabilizer is 100:1-3:60-70:3-5:1-3.
9. Use of the chain-extended PVC paste resin according to any one of claims 1 to 5, the chain-extended PVC paste resin obtained by the preparation method according to claim 6, and the PVC foam composite special material according to any one of claims 7 to 8 in the field of foam products.
10. A foamed product, characterized in that: The PVC foam composite special material is prepared by mixing chain-extended PVC paste resin, inorganic filler, plasticizer, foaming agent and stabilizer in a predetermined mass ratio and foaming the mixture at a high temperature of 200 to 210 degrees Celsius for 5 to 10 minutes; The chain-extended PVC paste resin is the chain-extended PVC paste resin according to any one of claims 1 to 5 or the chain-extended PVC paste resin obtained by the preparation method according to claim 6; Optionally, the predetermined mass ratio is that the mass ratio of the chain-extended PVC paste resin, the inorganic filler, the plasticizer, the foaming agent, and the stabilizer is 100:1-3:60-70:3-5:1-3.
Citation Information
Patent Citations
Method for producing paste resin by using chain extender
CN102093500A
High-performance copolymerized paste resin and preparation method thereof
CN102807644A
Matt PVC paste resin and preparation method thereof
CN111057177A
Vinyl chloride resin for paste processing and vinyl chloride resin composition for paste processing using the same
JP2015124317A
Cited By
Melt-processable PVC (polyvinyl chloride) resin and plasticizing method thereof
CN121108532A