Polymer-based working condition self-adaptive additive, preparation method thereof, liquid lubrication system, gel lubrication system and application of liquid lubrication system and gel lubrication system
Through the development of polymer-based working conditions adaptive additives, the problems of single functions and poor environmental adaptability of existing lubricating materials under complex working conditions have been solved, and the excellent grinding reduction of polymer-based working conditions has been achieved in the lubricating system. , anti-wear and extreme pressure properties, and oxidation resistance, simplifying composition and reducing costs.
Patent Information
- Application Number
- CN202411069492.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
Existing lubricating materials cannot respond in a timely manner and adjust their own characteristics under complex and variable working conditions, and it is difficult to meet extreme lubrication needs. There are problems such as single functions, extreme performance and poor environmental adaptability.
Develop a polymer-based condition adaptive additive to form urea groups and disulfide bond monomers by the addition of isocyanoethyl methacrylate with octadecylamine, hydroxyethyl methacrylate and lipoic acid. The polymer-based working condition adaptive additive with abrasion resistance, wear reduction, extreme pressure, oxidation resistance and viscosity adjustment are prepared. Liquid and gel lubrication system.
The additive forms strong chemical adsorption and complex friction chemical reactions at the friction pair interface, significantly improving the tribological properties of traditional base oils, providing excellent wear reduction, wear resistance and extremely high load-bearing capacity, and through macromolecular chain entanglement and hydrogen bonding, it also provides excellent wear reduction, wear resistance and high load-bearing capacity. Form a stable oil film, improves lubricating performance and wear resistance, and has excellent oxidation resistance, simplifies composition and reduces costs.
Smart Images

Figure CN118978629A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of industrial lubricating additives, and in particular to a polymer-based working condition adaptive additive and a preparation method thereof, a liquid lubricating system and a gel lubricating system and applications thereof. Background Art
[0002] As one of the most mature and widely used energy-saving technologies, lubrication technology is of great significance in reducing friction and wear, improving energy utilization, and ensuring the reliable operation of military equipment. However, existing lubricating materials cannot respond and adjust their own characteristics in a timely manner under complex and changeable working conditions, and it is difficult to meet the needs of extreme lubrication. It is urgent to create revolutionary adaptive lubricating materials and technologies to fundamentally solve the problems of existing lubricating materials such as single function, extreme performance and poor environmental adaptability under complex and changeable harsh working conditions.
[0003] As a type of liquid lubricant, lubricating oil is the most widely used. However, it is difficult to achieve the ideal lubrication effect under certain extreme or harsh working conditions. There are problems such as poor anti-wear and limited friction reduction effects. Therefore, a variety of additives are added to commercial base oils, such as anti-wear agents, extreme pressure agents, gel factors, viscosity modifiers and antioxidants. For the anti-wear agents currently available on the market, their anti-wear and extreme pressure properties are poor; for anti-wear agents, their anti-wear and extreme pressure properties are relatively poor; for extreme pressure agents, their anti-wear and friction reduction properties are poor; for gel factors, most of them are small molecular monomers with poor lubrication performance. In other words, the functions of commercially available additives are relatively simple. In order to improve the comprehensive performance of commercial base oils, it is necessary to add a variety of additives with complex ingredients and high costs. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a polymer-based working condition adaptive additive and a preparation method thereof, a liquid lubrication system and a gel lubrication system and applications thereof. The polymer-based working condition adaptive additive provided by the present invention has the functions of anti-wear, anti-friction, extreme pressure, anti-oxidation, viscosity adjustment and gel factor, and is applied to the lubrication system, which simplifies the ingredients and reduces the cost.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a polymer-based working condition adaptive additive having a structure shown in Formula I:
[0007]
[0008] In formula I, the ratio of x:y:z is 1:1:2 to 2.5.
[0009] The present invention also provides a method for preparing the polymer-based working condition adaptive additive described in the above technical solution, comprising the following steps:
[0010] Isocyanoethyl methacrylate and octadecylamine undergo a first addition reaction to obtain a urea monomer;
[0011] Hydroxyethyl methacrylate and lipoic acid, through a second addition reaction, obtain a disulfide bond monomer;
[0012] The urea monomer, the disulfide bond monomer, the hexadecyl methacrylate monomer, the initiator and the organic solvent are mixed and polymerized to obtain the polymer-based working condition adaptive additive.
[0013] Preferably, the molar ratio of the isocyanoethyl methacrylate to octadecylamine is 1:1.1-1.2, and the temperature of the first addition reaction is 20-30° C., and the time is 0.5-1 h.
[0014] Preferably, the molar ratio of hydroxyethyl methacrylate to lipoic acid is 1:1.1-1.2, and the temperature of the second addition reaction is 20-30° C. and the time is 18-24 hours.
[0015] Preferably, the molar ratio of the urea monomer, the disulfide bond monomer and the hexadecyl methacrylate monomer is 1:1:2 to 2.5;
[0016] The initiator is azobisisobutyronitrile;
[0017] The mass of the initiator is 1 to 1.5% of the total mass of the urea monomer, the disulfide bond monomer and the hexadecyl methacrylate monomer;
[0018] The polymerization reaction temperature is 75-85° C. and the reaction time is 8-10 hours.
[0019] The present invention also provides a liquid lubrication system, comprising the following components in percentage by mass:
[0020] Base oil 97.01~99.5%, additive 0.5~2.99%;
[0021] The additive is the polymer-based adaptive working condition additive described in the above technical solution or the polymer-based adaptive working condition additive prepared by the preparation method described in the above technical solution.
[0022] Preferably, the base oil comprises 500SN and / or PAO10.
[0023] The present invention also provides a gel lubrication system, comprising the following components in percentage by mass:
[0024] Base oil 91-97%, additives 3-9%;
[0025] The additive is the polymer-based adaptive working condition additive described in the above technical solution or the polymer-based adaptive working condition additive prepared by the preparation method described in the above technical solution.
[0026] Preferably, the base oil comprises 500SN and / or PAO10.
[0027] The present invention also provides application of the liquid lubrication system described in the above technical solution or the gel lubrication system described in the above technical solution in lubrication of mechanical parts.
[0028] The present invention provides a polymer-based working condition adaptive additive having a structure shown in Formula I.
[0029] The polymer-based adaptive working condition additive of the present invention can produce a strong chemical adsorption effect on the interface of the friction pair to form an adsorption film; at the same time, the polymer-based adaptive working condition additive will undergo a complex friction chemical reaction during the friction process to form a thicker friction film. The combined effect of the two makes the polymer-based adaptive working condition additive have a good lubrication effect, that is, the polymer-based adaptive working condition additive provided by the present invention can significantly improve the tribological properties of traditional base oils, and has very excellent wear reduction, anti-wear performance and extremely high load-bearing capacity (above 900N). In addition, due to the entanglement between macromolecules and macromolecular chains in the structure of the polymer-based adaptive working condition additive, and the simultaneous presence of urea groups and disulfide bonds, the urea groups can provide hydrogen bonding forces, and the disulfide bonds can be broken and polymerized at high temperatures. These reasons enable the polymer-based adaptive working condition additive to increase the viscosity and viscosity index of traditional base oils. The high viscosity brought by the polymer-based adaptive working condition additive can enable the lubrication system to form a thicker oil film on the surface of the friction pair, and the oil film is also more stable, thereby effectively preventing direct contact between the friction pairs, and ultimately improving the lubrication performance and anti-wear properties of the lubrication system. In addition, there are entanglements of macromolecular chains (covalent bonds) in the structure of the polymer-based adaptive working condition additive, the presence of urea groups forms hydrogen bonds (non-covalent bonds), and the breakage polymerization of dynamic disulfide bonds (covalent bonds). These reasons enable the lubricating oil to gel; the polymer-based adaptive working condition additive is added to the base oil at a mass percentage of 3-9%, which can cause the traditional base oil to undergo a phase change to form a gel lubrication system. The polymer-based adaptive working condition additive is used as a gel factor. Compared with the commercially available small molecule monomer gel factor, it can also improve the lubrication performance and wear resistance. The polymer-based adaptive working condition additive cannot become a gel at a low addition concentration of 0.5-2.99% by mass because the forces of covalent bonds and non-covalent bonds do not reach the critical gelation value. In addition, the dynamic disulfide bonds in the polymer-based adaptive working condition additive are very sensitive to redox conditions, so the polymer-based adaptive working condition additive also has excellent antioxidant properties. It can be seen that the polymer-based adaptive working condition additive of the present invention has multiple functions of wear reduction, anti-wear, extreme pressure, anti-oxidation, viscosity regulation and gel factor. When applied to the lubrication system, it can simplify the components of the lubrication system and ultimately reduce costs.
[0030] The present invention also provides a method for preparing the polymer-based working condition adaptive additive described in the above technical solution. The preparation method provided by the present invention is simple, the raw materials are green and non-toxic, and it has broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the H NMR spectrum of the polymer-based working condition adaptive additive obtained in Example 1;
[0032] Figure 2The friction coefficient curves of base oil 500SN and liquid lubrication systems A1 to A4 are shown;
[0033] Figure 3 The wear volume diagrams of base oil 500SN and liquid lubrication systems A1 to A4;
[0034] Figure 4 The load-carrying capacity test results of base oil 500SN and liquid lubrication systems A1 to A4;
[0035] Figure 5 The results of the temperature-dependent friction tests of base oil 500SN and liquid lubrication systems A1 to A4;
[0036] Figure 6 The results of variable frequency friction tests of base oil 500SN and liquid lubrication systems A1 to A4;
[0037] Figure 7 The thermal weight loss curves of base oil 500SN and liquid lubrication system A1~A4;
[0038] Figure 8 This is the friction coefficient curve of base oil 500SN and gel lubrication system B1~B4;
[0039] Fig. 9 The wear volume diagram of base oil 500SN and gel lubrication system B1 to B4;
[0040] Fig.10 The load-carrying capacity test results of base oil 500SN and gel lubrication systems B1 to B4;
[0041] Fig.11 These are the friction test results of base oil 500SN and gel lubrication systems B1 to B4 under variable temperature conditions;
[0042] Fig.12 The results of the variable frequency friction test of base oil 500SN and gel lubrication systems B1 to B4;
[0043] Fig.13 These are the thermal gravimetric curves of base oil 500SN and gel lubrication systems B1 to B4. DETAILED DESCRIPTION
[0044] The present invention provides a polymer-based working condition adaptive additive having a structure shown in Formula I:
[0045]
[0046] In formula I, the ratio of x:y:z is 1:1:2 to 2.5.
[0047] In the present invention, the ratio of x:y:z is preferably 1:1:2.
[0048] The polymer-based working condition adaptive additive (hereinafter referred to as additive) of the present invention can produce strong chemical adsorption on the interface of the friction pair to form an adsorption film; at the same time, the additive will undergo complex friction chemical reactions during the friction process to form a thicker friction film. The combined effect of the two makes the additive have a good lubricating effect, that is, the additive provided by the present invention can significantly improve the tribological properties of traditional base oils, and has very excellent wear reduction, anti-wear performance and extremely high load-bearing capacity (above 900N). In addition, due to the entanglement between macromolecules and macromolecular chains in the additive structure, and the simultaneous presence of urea groups and disulfide bonds, the urea groups can provide hydrogen bonding forces, and the disulfide bonds can break and polymerize at high temperatures. These reasons enable the additive to increase the viscosity and viscosity index of traditional base oils. The high viscosity brought by the additive can enable the lubrication system to form a thicker oil film on the surface of the friction pair, and the oil film is also more stable, thereby effectively preventing direct contact between the friction pairs, and ultimately improving the lubrication performance and anti-wear properties of the lubrication system. In addition, the existence of entanglement of macromolecular chains (covalent bonds) in the additive structure, the presence of urea groups to form hydrogen bonds (non-covalent bonds), and the breaking and polymerization of dynamic disulfide bonds (covalent bonds) enable the lubricating oil to gel; the additive is added to the base oil at a mass percentage of 3-9%, which can cause the traditional base oil to undergo a phase change to form a gel lubrication system. The additive, as a gel factor, can also improve the lubrication performance and wear resistance compared to the commercially available small molecule monomer gel factors. The additive cannot become a gel at a low addition concentration of 0.5-2.99% by mass because the forces of covalent bonds and non-covalent bonds do not reach the critical gelation value. In addition, the dynamic disulfide bonds in the additive are very sensitive to redox conditions, so the additive also has excellent antioxidant properties. It can be seen that the additive of the present invention has multiple functions of wear reduction, anti-wear, extreme pressure, anti-oxidation, viscosity regulation and gel factor. When applied to a lubrication system, the composition of the lubrication system can be simplified, and ultimately cost reduction can be achieved.
[0049] The present invention also provides a method for preparing the polymer-based working condition adaptive additive described in the above technical solution, comprising the following steps:
[0050] Isocyanoethyl methacrylate and octadecylamine undergo a first addition reaction to obtain a urea monomer;
[0051] Hydroxyethyl methacrylate and lipoic acid, through a second addition reaction, obtain a disulfide bond monomer;
[0052] The urea monomer, the disulfide bond monomer, the hexadecyl methacrylate monomer, the initiator and the organic solvent are mixed and polymerized to obtain the polymer-based working condition adaptive additive.
[0053] In the present invention, unless otherwise specified, the raw materials used in the present invention are preferably commercially available products.
[0054] The invention conducts a first addition reaction between isocyanoethyl methacrylate and octadecylamine to obtain a urea monomer.
[0055] In the present invention, the medium of the first addition reaction is preferably an organic solvent, and the organic solvent preferably includes one or more of dichloromethane, chloroform and tetrahydrofuran, and is more preferably dichloromethane.
[0056] In the present invention, the molar ratio of isocyanoethyl methacrylate to octadecylamine is preferably 1:1.1-1.2.
[0057] In the present invention, the first addition reaction of isocyanoethyl methacrylate and octadecylamine preferably comprises: dissolving octadecylamine in the medium of the first addition reaction, then dropping isocyanoethyl methacrylate, and continuously stirring until a large amount of white solid appears. In the present invention, the dissolution is preferably carried out under stirring, the stirring temperature is preferably 25° C., and the time is preferably 30 minutes; the dropping method is preferably dropwise addition.
[0058] In the present invention, the temperature of the first addition reaction is preferably 20-30° C., and the time is preferably 0.5-1 h.
[0059] After the first addition reaction, the present invention preferably further comprises post-treatment, and the post-treatment preferably comprises: filtering the obtained feed liquid, rinsing and vacuum drying the obtained filter residue to obtain the urea-based monomer; the rinsing reagent is preferably dichloromethane; the number of rinsing is preferably 3 times, the temperature of the vacuum drying is preferably 25-35°C, and the time is preferably 24 hours.
[0060] The invention conducts a second addition reaction on hydroxyethyl methacrylate and lipoic acid to obtain a disulfide bond monomer.
[0061] In the present invention, the medium of the second addition reaction is preferably an organic solvent, and the organic solvent preferably includes one or more of dichloromethane, chloroform and tetrahydrofuran.
[0062] In the present invention, the catalyst for the second addition reaction preferably includes EDH-HCl and 4-dimethylaminopyridine (DMAP); the molar ratio of EDH-HCl to lipoic acid is preferably 1:1, and the molar ratio of 4-dimethylaminopyridine to lipoic acid is preferably 0.1 to 0.2:1.
[0063] In the present invention, the molar ratio of the hydroxyethyl methacrylate to lipoic acid is preferably 1:1.1-1.2.
[0064] In the present invention, the temperature of the second addition reaction is preferably 20 to 30° C., and the time is preferably 18 to 24 hours.
[0065] The second addition reaction of hydroxyethyl methacrylate and lipoic acid in the present invention preferably comprises: adding hydroxyethyl methacrylate and lipoic acid into the second addition medium, stirring in an ice-water bath for 30 minutes; then adding a catalyst for the second addition reaction to carry out the second addition reaction.
[0066] After the second addition reaction, the present invention preferably further includes post-treatment, and the post-treatment preferably includes the following steps: adjusting the obtained feed liquid to be acidic, extracting and separating to obtain a first organic layer; adjusting the first organic layer to be neutral, extracting and separating to obtain a second organic layer; mixing the second organic layer and a saturated sodium chloride solution, extracting and separating to obtain a third organic layer; drying and rotary evaporating the third organic layer to obtain the disulfide bond monomer; the acidic pH value is less than 2, and the reagent for adjusting the obtained feed liquid to be acidic is preferably 1 mol / L; the reagent for adjusting the first organic layer to be neutral is preferably a saturated NaHCO3 solution; the drying method is preferably drying with a desiccant, and the desiccant is preferably MgSO4.
[0067] After obtaining the urea monomer and the disulfide bond monomer, the present invention mixes the urea monomer, the disulfide bond monomer, the hexadecyl methacrylate monomer, an initiator and an organic solvent to carry out a polymerization reaction to obtain the polymer-based working condition adaptive additive.
[0068] In the present invention, the organic solvent is preferably N,N-dimethylformamide. In the present invention, the mass proportion of the organic solvent in the raw materials of the polymerization reaction is preferably 50-60%.
[0069] In the present invention, the initiator is preferably azobisisobutyronitrile. In the present invention, the mass of the initiator is preferably 1 to 1.5% of the total mass of the urea monomer, the disulfide bond monomer and the hexadecyl methacrylate monomer.
[0070] In the present invention, the molar ratio of the urea monomer, the disulfide bond monomer and the hexadecyl methacrylate monomer is preferably 1:1:2 to 2.5, and more preferably 1:1:2.
[0071] In the present invention, the urea monomer, the disulfide bond monomer, the hexadecyl methacrylate monomer, the initiator and the organic solvent are preferably mixed under stirring, and the stirring method is preferably magnetic stirring. The present invention has no special limitation on the stirring rate, and the stirring can be carried out according to the process well known in the art. In the present invention, mixing under stirring can ensure that the materials are fully dispersed and contacted.
[0072] Before the polymerization reaction, the present invention preferably further comprises: introducing nitrogen into the mixed system obtained by the mixing, and the time of introducing nitrogen is preferably 0.5 to 1 hour. In the present invention, the introduction of nitrogen can fully exclude oxygen.
[0073] In the present invention, the polymerization reaction temperature is preferably 75 to 85° C., and the time is preferably 8 to 10 hours. In the present invention, the polymerization reaction is preferably carried out under the conditions of oil bath and stirring.
[0074] After the polymerization reaction, the present invention preferably includes: dripping the obtained polymerization reaction liquid into anhydrous ethanol, during the dripping process, the reaction product precipitates out, and after filtering, the precipitate is collected; the precipitate is sequentially recrystallized and vacuum dried to obtain the polymer-based working condition adaptive additive. In the present invention, the temperature of the anhydrous ethanol is preferably 0 to 25°C. In the present invention, the recrystallization reagent is preferably anhydrous ethanol. In the present invention, the temperature of the vacuum drying is preferably 25 to 35°C, the time is preferably 24 to 48h, and the vacuum drying is preferably carried out in a vacuum drying oven.
[0075] In the present invention, the reaction formula of the polymerization reaction is as follows:
[0076]
[0077] The present invention also provides a liquid lubrication system, comprising the following components in percentage by mass:
[0078] Base oil 97.01~99.5%, additive 0.5~2.99%;
[0079] The additive is the polymer-based adaptive working condition additive described in the above technical solution or the polymer-based adaptive working condition additive prepared by the preparation method described in the above technical solution.
[0080] The liquid lubricating system provided by the present invention comprises 97.01-99.5% by mass of base oil, more preferably 98-99% by mass. In the present invention, the base oil preferably comprises 500SN and / or PAO10, more preferably 500SN.
[0081] The liquid lubrication system provided by the present invention comprises 0.5-2.99% additive by mass, preferably 1-2%. In the present invention, the additive is the polymer-based adaptive working condition additive described in the above technical solution or the polymer-based adaptive working condition additive prepared by the preparation method described in the above technical solution.
[0082] In the present invention, the preparation method of the liquid lubricating system preferably comprises the following steps:
[0083] The base oil and the additive are stirred and mixed to obtain the liquid lubricating system.
[0084] In the present invention, the stirring and mixing temperature is preferably 110-130° C., and the time is preferably 30 minutes.
[0085] After the stirring and mixing, the present invention preferably further comprises cooling to room temperature to obtain the liquid lubricating system.
[0086] The present invention also provides a gel lubrication system, comprising the following components in percentage by mass:
[0087] Base oil 91-97%, additives 3-9%;
[0088] The additive is the polymer-based adaptive working condition additive described in the above technical solution or the polymer-based adaptive working condition additive prepared by the preparation method described in the above technical solution.
[0089] The gel lubrication system provided by the present invention comprises 91-97% by mass of base oil, preferably 91-93% by mass. In the present invention, the base oil preferably comprises 500SN and / or PAO10, more preferably 500SN.
[0090] The gel lubrication system provided by the present invention comprises 3-9% additive by mass, preferably 7-9%. In the present invention, the additive is the polymer-based adaptive working condition additive described in the above technical solution or the polymer-based adaptive working condition additive prepared by the preparation method described in the above technical solution.
[0091] In the present invention, the preparation method of the gel lubrication system preferably comprises the following steps:
[0092] The base oil and the additive are stirred and mixed to obtain the gel lubrication system.
[0093] In the present invention, the stirring and mixing temperature is preferably 110-130° C., and the time is preferably 30 minutes.
[0094] After the stirring and mixing, the present invention preferably further comprises cooling to room temperature to obtain the gel lubricating system.
[0095] The present invention also provides application of the liquid lubrication system described in the above technical solution or the gel lubrication system described in the above technical solution in lubrication of mechanical parts.
[0096] The present invention does not specifically limit the application mode of the liquid lubrication system and the gel lubrication system, and those skilled in the art can set them according to the reagent requirements.
[0097] The polymer-based working condition adaptive additive and its preparation method, liquid lubrication system and gel lubrication system and their applications provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be understood as limiting the scope of protection of the present invention.
[0098] Example 1
[0099] 12.42 g (0.04 mol) of hexadecyl methacrylate, 8.49 g (0.02 mol) of urea monomer, 6.40 g (0.02 mol) of disulfide monomer, 0.28 g (1 wt%) of azobisisobutyronitrile (AIBN) and 42 mL of N,N-dimethylformamide (DMF) were mixed in a round-bottom flask, and nitrogen was introduced for 30 min to exclude oxygen. A water condenser was placed in an 85°C oil bath, and the mixture was reacted for 8 h under magnetic stirring. The obtained mixture was purified by precipitation into an excess of anhydrous ethanol at a temperature of 0°C, and the precipitate was collected by filtration; the precipitate was recrystallized using anhydrous ethanol, and then dried in a vacuum drying oven at 30°C for 24 h to obtain 22.17 g of light yellow powder with a yield of 80.36%.
[0100] The preparation method of the urea-based monomer comprises the following steps:
[0101] 0.11 mol of octadecylamine was dissolved in 250 mL of dichloromethane. After stirring at 25°C for 30 min, the octadecylamine was completely dissolved. Then 0.1 mol of isocyanoethyl methacrylate was added dropwise to the solution. The mixture was stirred continuously until a large amount of white solid appeared. After filtration, the solid was washed with dichloromethane and filtered. The mixture was repeated 3 times. The solid was dried under vacuum at 35°C for 24 h to obtain a urea monomer.
[0102] Wherein, the preparation method of disulfide bond monomer comprises the following steps:
[0103] In 150mL of dichloromethane, add 0.1mol of hydroxyethyl methacrylate and 0.11mol of lipoic acid, stir for 30min in an ice bath, then add 0.11mol of EDH-HCl and 0.02mol of DMAP, stir at room temperature for 24h. The reaction mixture is extracted with 1mol / L HCl, saturated NaHCO3, and saturated brine in sequence. Dry the organic layer with magnesium sulfate, filter, and rotary evaporate to obtain the disulfide bond monomer.
[0104] Characterization
[0105] The polymer-based working condition adaptive additive prepared in Example 1 was characterized by NMR, and the results are shown in Figure 1 . Figure 1 is the H NMR spectrum of the obtained polymer-based working condition adaptive additive. Figure 1 The successful synthesis of the polymer-based condition-adaptive additive can be demonstrated.
[0106] Application Example 1
[0107] The polymer additive obtained in Example 1 was added to the base oil 500SN in proportions of 0.25%, 0.50%, 0.75% and 1% by mass, and the remainder was the base oil, which were respectively recorded as liquid lubrication systems A1, A2, A3 and A4.
[0108] Comparative application example 1
[0109] The base oil 500SN was used as the control solution.
[0110] Performance Testing
[0111] 1. Friction coefficient test
[0112] The friction and wear performance of base oil 500SN and liquid lubrication systems A1 to A4 were evaluated using the SRV-IV micro-vibration friction and wear tester produced by Optimol Grease Company of Germany. The test conditions were: load 300N, temperature 25℃, frequency 25Hz, amplitude 1mm, test time 30min, the upper test ball was a steel ball, and the lower test sample was a GCr steel block.
[0113] The test results are shown in Table 1 and Figure 2 As shown, Figure 2 This is the friction coefficient curve of base oil 500SN and liquid lubrication systems A1 to A4.
[0114] Table 1 Average friction coefficient of base oil 500SN and liquid lubrication systems A1 to A4
[0115] type 500SN A1 A2 A3 A4 Average friction coefficient 0.2101 0.1501 0.1204 0.1203 0.1202
[0116] According to the data in Table 1, it can be seen that compared with the base oil, the friction coefficients of the liquid lubricating systems A1 to A4 containing the polymer-based adaptive working condition additive are significantly reduced, and with the increase in the amount of the polymer-based adaptive working condition additive prepared in Example 1, the average friction coefficients of the liquid lubricating systems A1 to A4 gradually decrease. The average friction coefficient of the liquid lubricating system A4 is the lowest, indicating that the polymer-based adaptive working condition additive provided by the present invention has excellent wear reduction properties.
[0117] The wear volume of the obtained wear scar was measured and the result was Figure 3 . Figure 3 The wear volume diagram of base oil 500SN and liquid lubrication system A1~A4 is shown in Figure 2. Figure 3 It can be seen that the wear volume of the wear scar after lubrication by the liquid lubrication system is significantly smaller than that of the base oil, and the wear volume gradually decreases with the increase of the added concentration, indicating that the polymer-based working condition adaptive additive provided by the present invention has excellent anti-wear properties.
[0118] 2. Load-bearing capacity test
[0119] The load-bearing capacity of base oil 500SN and liquid lubrication systems A1-A4 prepared in Application Example 1 was tested. The test conditions were: load 50-1000N (increased by 50N every two minutes), frequency 25Hz, amplitude 1mm, temperature 25°C, the diameter of the upper test ball was 10mm, and the lower test sample was a steel block with a hardness of 700HV.
[0120] The test results are shown in Table 2 and Figure 4 , Figure 4 These are the load-bearing capacity test results for base oil 500SN and liquid lubrication systems A1 to A4.
[0121] Table 2 Maximum load-bearing capacity of base oil 500SN and liquid lubrication systems A1 to A4
[0122] type 500SN A1 A2 A3 A4 Seizure load (N) 250 250 750 850 950
[0123] According to Table 2 and Figure 4 It can be seen from the results that the liquid lubrication system provided by the present invention has significantly improved load-bearing capacity compared with the base oil, and its anti-friction and anti-wear performance is far superior to that of the base oil 500SN. In addition, the load-bearing capacity of the liquid lubrication system increases with the increase in the content of the polymer-based working condition adaptive additive. This indicates that the polymer-based working condition adaptive additive provided by the present invention has excellent extreme pressure properties.
[0124] 3. Variable temperature friction test
[0125] The temperature resistance and friction ability of the base oil 500SN and the liquid lubrication system A1-A4 prepared in Application Example 1 were tested. The test conditions were: temperature 25-175°C (increased by 25°C every two minutes. Due to the properties of the friction pair material itself, the temperature resistance needs to be controlled within 180°C, so the maximum temperature in this experiment was increased to 175°C), load 300N, frequency 25Hz, amplitude 1mm, the diameter of the upper test ball was 10mm, and the lower test sample was a steel block with a hardness of 700HV.
[0126] The test results are shown in Table 3 and Figure 5 , Figure 5 These are the temperature-dependent friction test results for base oil 500SN and liquid lubrication systems A1 to A4.
[0127] Table 3 Temperature and friction resistance of base oil 500SN and liquid lubrication systems A1 to A4
[0128] type 500SN A1 A2 A3 A4 Friction temperature resistance (℃) 25 25 125 175 175
[0129] According to Table 3 and Figure 5It can be seen from the results in that the liquid lubrication system provided by the present invention still has good wear reduction and anti-wear performance in the variable temperature friction test compared with the base oil, and the effective lubrication temperature increases with the increase in the content of the polymer-based working condition adaptive additive.
[0130] 4. Frequency conversion friction test
[0131] The variable frequency friction performance of base oil 500SN and liquid lubrication systems A1-A4 prepared in Application Example 1 was tested. The test conditions were: frequency 10-80 Hz (increased by 5 Hz every two minutes), load 300 N, temperature 25 ° C, amplitude 1 mm, the diameter of the upper test ball was 10 mm, and the lower test sample was a steel block with a hardness of 700 HV.
[0132] The test results are shown in Table 4 and Figure 6 , Figure 6 These are the results of variable frequency friction tests of base oil 500SN and liquid lubrication systems A1 to A4.
[0133] Table 4 Temperature and friction resistance of base oil 500SN and liquid lubrication systems A1 to A4
[0134] type 500SN A1 A2 A3 A4 Lubrication failure frequency (Hz) 10 10 - - -
[0135] According to Table 4 and Figure 6 It can be seen from the results in that the liquid lubrication system provided by the present invention still has good wear reduction and anti-wear performance in the variable frequency friction test compared with the base oil, and still exhibits excellent lubrication performance under heavy load low / high frequency conditions.
[0136] The results of the variable temperature friction test and the variable frequency friction test show that the polymer-based working condition adaptive additive provided by the present invention has excellent working condition adaptability and still has good lubrication performance as the working conditions change.
[0137] 5. Thermal stability test
[0138] The liquid lubrication systems A1 to A4 prepared in Example 1 and the base oil 500SN were subjected to thermogravimetric testing. The results are as follows: Figure 7 As shown, Figure 7 The thermal weight loss curves of base oil 500SN and liquid lubrication system A1~A4. Figure 7 It can be seen that the liquid lubrication system provided by the present invention has excellent thermal stability.
[0139] 6. Viscosity test
[0140] The kinematic viscosity of the liquid lubrication systems A1 to A4 and the base oil 500SN was tested at 40°C and 100°C using a SYP1003-III kinematic viscosity tester. The results are shown in Table 5.
[0141] Table 5 Kinematic viscosity of base oil 500SN and liquid lubrication systems A1-A4 at 40℃ and 100℃
[0142] type <![CDATA[Viscosity at 40 °C / (mm 2 / s)]]> <![CDATA[Viscosity at 100 °C (mm 2 / s)]]> 500SN 90.04 10.49 A1 91.06 11.06 A2 92.95 12.89 A3 93.38 13.09 A4 93.55 13.24
[0143] It can be seen from Table 5 that compared with the base oil 500SN, with the increase of the amount of polymer-based condition-adaptive additive added in the liquid lubrication system, the kinematic viscosity of the liquid lubrication system at 40°C and 100°C increases step by step with the concentration of the polymer-based condition-adaptive additive. The kinematic viscosity of the liquid lubrication system A4 is the largest and decreases with the increase of temperature.
[0144] Application Example 2
[0145] The polymer-based working condition adaptive additive prepared in Example 1 was added to the base oil 500SN in a ratio of 3%, 5%, 7% and 9% by mass, and the balance was the base oil, to obtain four gel lubrication system experimental groups with different contents of the polymer-based working condition adaptive additive, which were respectively recorded as gel lubrication systems B1, B2, B3 and B4.
[0146] Comparative Application Example 2
[0147] The base oil 500SN was used as the control solution.
[0148] Performance Testing
[0149] 1. Friction coefficient test
[0150] The friction and wear performance of gel lubrication systems B1-B4 and base oil 500SN was evaluated using the SRV-IV micro-vibration friction and wear tester produced by Optimol Grease Company of Germany. The test conditions were: load 300N, temperature 25℃, frequency 25Hz, amplitude 1mm, test time 30min, the upper test ball was a steel ball, and the lower test sample was a GCr steel block.
[0151] The test results are shown in Table 6 and Figure 8 As shown, Figure 8 This is the friction coefficient curve of base oil 500SN and gel lubrication system B1~B4.
[0152] Table 6 Average friction coefficient of base oil 500SN and gel lubrication systems B1 to B4
[0153] type 500SN B1 B2 B3 B4 Average friction coefficient 0.1586 0.1159 0.1157 0.1142 0.1141
[0154] According to the data in Table 6, it can be seen that compared with the base oil, the friction coefficient of the gel lubrication systems B1 to B4 containing the polymer-based adaptive working condition additive is significantly reduced, and with the increase in the amount of the polymer-based adaptive working condition additive prepared in Example 1, the average friction coefficient of the gel lubrication systems B1 to B4 gradually decreases. The average friction coefficient of the gel lubrication system B4 is the lowest, indicating that the polymer-based adaptive working condition additive provided by the present invention has excellent wear reduction properties.
[0155] The wear volume of the obtained wear scar was measured and the result was Fig. 9 , Fig. 9 The wear volume diagram of base oil 500SN and gel lubrication system B1~B4; Fig. 9 It can be seen that the wear volume of the wear scar after lubrication by the gel lubrication system is significantly smaller than that of the base oil, and the wear volume gradually decreases with increasing addition concentration, indicating that the polymer-based working condition adaptive additive provided by the present invention has excellent anti-wear properties.
[0156] 2. Load-bearing capacity test
[0157] The load-bearing capacity of the base oil 500SN and the gel lubrication system B1-B4 prepared in Application Example 2 was tested. The test conditions were: load 50-1500N (increased by 50N every two minutes), frequency 25Hz, amplitude 1mm, temperature 25°C, the diameter of the upper test ball was 10mm, and the lower test sample was a steel block with a hardness of 700HV.
[0158] The test results are shown in Table 7 and Fig.10 , Fig.10 These are the load-bearing capacity test results of base oil 500SN and gel lubrication systems B1 to B4.
[0159] Table 7 Maximum load-bearing capacity of base oil 500SN and gel lubrication systems B1 to B4
[0160] type 500SN B1 B2 B3 B4 Bearing load (N) 250 1500 1500 1500 1500
[0161] Due to the nature of the friction machine itself, the maximum load applied under this condition is 1500N, and the gel lubrication system provided by the present invention does not cause seizure within this range. Fig.10 It can be seen from the results that the gel lubrication system provided by the present invention has significantly improved load-bearing capacity compared with the base oil, and its anti-friction and anti-wear performance is far superior to that of the base oil 500SN. This indicates that the polymer-based working condition adaptive additive provided by the present invention has excellent extreme pressure properties.
[0162] 3. Variable temperature friction test
[0163] The temperature and friction resistance of the base oil 500SN and the gel lubrication system B1-B4 prepared in Application Example 2 were tested. The test conditions were: temperature 25-175°C (increased by 25°C every two minutes. Due to the properties of the friction pair material itself, the temperature resistance needs to be controlled within 180°C, so the maximum temperature in this experiment was increased to 175°C), load 300N, frequency 25Hz, amplitude 1mm, the diameter of the upper test ball in the experiment was 10mm, and the lower sample was a steel block with a hardness of 700HV.
[0164] The test results are shown in Table 8 and Fig.11 , Fig.11 These are the friction test results of base oil 500SN and gel lubrication systems B1 to B4 under variable temperature conditions.
[0165] Table 8 Temperature and friction resistance of base oil 500SN and gel lubrication systems B1 to B4
[0166] type 500SN B1 B2 B3 B4 Friction temperature resistance (℃) 25 175 175 175 175
[0167] According to Table 8 and Fig.11 It can be seen from the results in that the gel lubrication system provided by the present invention still has good wear reduction and anti-wear performance in the variable temperature friction test compared with the base oil.
[0168] 4. Frequency conversion friction test
[0169] The variable frequency friction performance of the base oil 500SN and the gel lubrication system B1-B4 prepared in Application Example 2 was tested. The test conditions were: frequency 10-80 Hz (increased by 5 Hz every two minutes), load 300 N, temperature 25 ° C, amplitude 1 mm, the upper test ball diameter was 10 mm, and the lower sample was a steel block with a hardness of 700 HV.
[0170] The test results are shown in Table 9 and Fig.12 , Fig.12 These are the results of the variable frequency friction test of base oil 500SN and gel lubrication systems B1 to B4.
[0171] Table 9 Temperature and friction resistance of base oil 500SN and gel lubrication systems B1 to B4
[0172] type 500SN A1 A2 A3 A4 Lubrication failure frequency (Hz) 10 - - - -
[0173] According to Table 9 and Fig.12 It can be seen from the results in that the gel lubrication system provided by the present invention still has good wear reduction and anti-wear performance in the variable frequency friction test compared with the base oil, and still exhibits excellent lubrication performance under heavy load low / high frequency conditions.
[0174] 5. Thermal stability test
[0175] The gel lubrication system B1-B4 prepared in Example 2 and the base oil 500SN were subjected to thermogravimetric testing. The results are as follows: Fig.13 As shown, Fig.13 This is the thermal weight loss curve of base oil 500SN and gel lubrication system B1~B4. Fig.13 It can be seen that the gel lubrication system provided by the present invention has excellent thermal stability.
[0176] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A polymer-based working condition adaptive additive, characterized in that: It has the structure shown in formula I: In formula I, the ratio of x:y:z is 1:1:2 to 2.
5.
2. The method for preparing the polymer-based working condition adaptive additive according to claim 1, characterized in that: The following steps are involved: Isocyanoethyl methacrylate and octadecylamine undergo a first addition reaction to obtain a urea monomer; Hydroxyethyl methacrylate and lipoic acid, through a second addition reaction, obtain a disulfide bond monomer; The urea monomer, the disulfide bond monomer, the hexadecyl methacrylate monomer, the initiator and the organic solvent are mixed and polymerized to obtain the polymer-based working condition adaptive additive.
3. The preparation method according to claim 2, characterized in that: The molar ratio of the isocyanoethyl methacrylate to octadecylamine is 1:1.1-1.2, the temperature of the first addition reaction is 20-30° C., and the time is 0.5-1 h.
4. The preparation method according to claim 2, characterized in that: The molar ratio of the hydroxyethyl methacrylate to lipoic acid is 1:1.1-1.2, the temperature of the second addition reaction is 20-30° C., and the time is 18-24 hours.
5. The preparation method according to claim 2, characterized in that: The molar ratio of the urea monomer, the disulfide bond monomer and the hexadecyl methacrylate monomer is 1:1:2 to 2.5; The initiator is azobisisobutyronitrile; The mass of the initiator is 1 to 1.5% of the total mass of the urea monomer, the disulfide bond monomer and the hexadecyl methacrylate monomer; The polymerization reaction temperature is 75-85° C. and the reaction time is 8-10 hours.
6. A liquid lubrication system, characterized in that: The following components are included in mass percentage: Base oil 97.01~99.5%, additive 0.5~2.99%; The additive is the polymer-based self-adaptive additive according to claim 1 or the polymer-based self-adaptive additive prepared by the preparation method according to any one of claims 2 to 5.
7. The liquid lubrication system according to claim 6, characterized in that: The base oil includes 500SN and / or PAO10.
8. A gel lubrication system, characterized in that: The following components are included in mass percentage: Base oil 91-97%, additives 3-9%; The additive is the polymer-based self-adaptive additive according to claim 1 or the polymer-based self-adaptive additive prepared by the preparation method according to any one of claims 2 to 5.
9. The gel lubrication system according to claim 8, characterized in that: The base oil includes 500SN and / or PAO10.
10. Use of the liquid lubricating system according to any one of claims 6 to 7 or the gel lubricating system according to any one of claims 8 to 9 in lubricating mechanical parts.
Citation Information
Patent Citations
Ureido polymer gelator and preparation method thereof, and gel lubricant and preparation method and application thereof
CN112724312A
Method for improving dispersion stability of inorganic nanoparticles in base oil and method for improving lubricating property and wear resistance of lubricating oil
CN115368950A
Method for improving dispersion stability of inorganic nanoparticles in base oil and method for improving lubricating property and wear resistance of lubricating oil
CN116024031A
Multifunctional viscosity index improver as well as preparation method and application thereof
CN118290646A
Use of a lipoic acid ester as an Anti-wear additive and / or friction modifier
WO2018138261A1