Dye dispersant and preparation method thereof
By preparing oleic acid polyethylene glycol, the sodium carboxylic acid sulfonate as dye dispersant, the problem of phenol hazards in traditional dye dispersants is solved, and a safe and environmentally friendly dye dispersion effect is achieved, and the production cost is reduced.
Patent Information
- Application Number
- CN202411052797.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
Tristyrene phenol polyoxyethylene polyether ammonium sulfate, commonly used in existing dye dispersants, contains phenol structure, which has great harm, and the preparation method is not environmentally friendly.
Oleic acid polyethylene glycol male-diester sodium carboxylic acid sulfonate is used as dye dispersant, and the reaction between oleic acid and polyethylene glycol is carried out under a catalyst, and then maleic anhydride and sodium sulfite are added to form oleic acid polyethylene oleic acid The diol mastyldiester carboxylic acid sodium sulfonate avoids the use of phenol structure and controls the reaction through specific process conditions.
It realizes safe and environmentally friendly dye dispersant preparation, with better results than traditional products, and reduces production costs due to the use of renewable resource oleic acid.
Smart Images

Figure CN118978686A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of dye dispersants, and in particular to a dye dispersant and a preparation method thereof. Background Art
[0002] Dispersant is a surfactant with two opposite properties, lipophilicity and hydrophilicity, in the molecule. It can evenly disperse the solid and liquid particles of inorganic and organic pigments that are difficult to dissolve in liquids, and at the same time prevent the sedimentation and aggregation of particles, forming the amphiphilic reagent required for a stable suspension.
[0003] The dye dispersants currently used are mostly tristyrylphenol polyoxyethylene polyether ammonium sulfate, and the preparation method thereof is mainly through sulfonation reaction of tristyrylphenol polyoxyethylene polyether and aminosulfonic acid. This type of product also has a phenol structure and has great hazards. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a dye dispersant, which has the same application effect as tristyrylphenol polyoxyethylene polyether and aminosulfonic acid, and is less harmful.
[0005] According to an embodiment of the present invention, a dye dispersant is provided, wherein the dye dispersant is oleic acid polyethylene glycol maleic acid diester carboxylic acid sulfonic acid sodium salt, and its structural formula is
[0006]
[0007] Preferably, the dye dispersant is first obtained by reacting oleic acid polyethylene glycol ester with maleic anhydride to obtain oleic acid polyethylene glycol maleate carboxylic acid; and then obtained by reacting oleic acid polyethylene glycol maleate carboxylic acid with sodium sulfite.
[0008] Further preferably, the structural formula of the oleic acid polyethylene glycol maleate carboxylic acid is
[0009]
[0010] According to an embodiment of the present invention, there is also provided a method for preparing the above-mentioned dye dispersant, comprising the following steps:
[0011] Step 1: Add a catalyst to oleic acid and polyethylene glycol at a temperature of 60-70°C and stir evenly, then evacuate and slowly heat to 150-160°C to react to obtain oleic acid polyethylene glycol ester, then cool to 60°C and break the vacuum to normal pressure;
[0012] Step 2, adding maleic anhydride, slowly heating to 60-70° C., reacting to obtain polyethylene glycol oleate and maleic anhydride;
[0013] Step 3, slowly add water and sodium sulfite, stir evenly, slowly raise the temperature to 50-60° C., and react to obtain sodium salt of oleic acid polyethylene glycol maleic acid ester carboxylic acid sulfonate.
[0014] Preferably, in step 1, the catalyst is p-toluenesulfonic acid.
[0015] Further preferably, in the step 1, when the acid value of the reaction solution is measured to be less than 1, the reaction is completed.
[0016] Further preferably, in the step 1, when oleic acid and polyethylene glycol are stirred, the temperature is raised to 60-70° C. by steam.
[0017] Further preferably, in step 1, the vacuum is broken by using an inert gas.
[0018] Further preferably, in the step 2, the acid value of the reaction solution is measured to be between 110-115, and the reaction is completed.
[0019] Still further preferably, in the step 3, when the pH of the 1% aqueous solution after the reaction is measured to be greater than 6, the reaction is completed.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] It does not contain banned substances such as phenol, is safe to use, and is an environmentally friendly product; the application effect is equivalent to that of conventional products, and slightly better than tristyrylphenol polyoxyethylene polyether ammonium sulfate; oleic acid is a renewable resource, which makes the production cost lower than conventional products. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the test results of the A1 solution in Example 4 of the present invention;
[0023] Figure 2 This is a schematic diagram of the test results of the B1 solution in Example 4 of the present invention;
[0024] Figure 3 This is a schematic diagram of the test results of the C1 solution in Example 4 of the present invention;
[0025] Figure 4 This is a schematic diagram of the test results of the A2 solution in Example 5 of the present invention;
[0026] Figure 5 This is a schematic diagram of the test results of the B2 solution in Example 5 of the present invention;
[0027] Figure 6 This is a schematic diagram of the test results of the C2 solution in Example 5 of the present invention;
[0028] Figure 7 This is a schematic diagram of the test results of the A3 solution in Example 6 of the present invention;
[0029] Figure 8 This is a schematic diagram of the test results of the B3 solution in Example 6 of the present invention;
[0030] Fig. 9 This is a schematic diagram of the test results of the C3 solution in Example 6 of the present invention;. DETAILED DESCRIPTION
[0031] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and embodiments.
[0032] The preparation reaction formula of oleic acid polyethylene glycol maleic acid diester carboxylic acid sulfonic acid sodium salt is as follows:
[0033]
[0034] Embodiment 1:
[0035] Add 282g oleic acid and 600g polyethylene glycol to the reactor, heat it to 60-70°C by steam, add 0.5g p-toluenesulfonic acid as a catalyst, and stir evenly;
[0036] Start to evacuate the mixture and slowly raise the temperature to 150-160°C. Keep the temperature for 4 hours. When the acid value is less than 1, the reaction is complete.
[0037] Cool down to 60℃, break the vacuum with nitrogen, and close the vacuum after reaching normal pressure;
[0038] Add 98g of maleic anhydride, slowly raise the temperature to 60-70°C, keep the temperature for 2 hours, and the reaction is complete when the acid value is between 110-115;
[0039] Slowly add 180g water and 126g sodium sulfite, stir evenly, slowly heat to 50-60°C, stir and react for 2 hours at this temperature, and measure the pH of 1% aqueous solution>6, the reaction is complete;
[0040] The temperature was lowered to below 50°C and a light yellow to yellow liquid was collected.
[0041] Embodiment 2:
[0042] Add 275g oleic acid and 588g polyethylene glycol to the reactor, heat it to 60-70°C by steam, add 0.49g p-toluenesulfonic acid as a catalyst, and stir evenly;
[0043] Start to evacuate the mixture and slowly raise the temperature to 150-160°C. Keep the temperature for 4 hours. When the acid value is less than 1, the reaction is complete.
[0044] Cool down to 60℃, break the vacuum with nitrogen, and close the vacuum after reaching normal pressure;
[0045] Add 97g of maleic anhydride, slowly raise the temperature to 60-70°C, keep the temperature for 2 hours, and the reaction is complete when the acid value is between 110-115;
[0046] Slowly add 177g water and 124g sodium sulfite, stir evenly, slowly heat to 50-60°C, stir and react for 2 hours at this temperature, and measure the pH of 1% aqueous solution>6, the reaction is complete;
[0047] The temperature was lowered to below 50°C and a light yellow to yellow liquid was collected.
[0048] Embodiment three:
[0049] Add 285g oleic acid and 612g polyethylene glycol to the reactor, heat it to 60-70°C by steam, add 0.51g p-toluenesulfonic acid as a catalyst, and stir evenly;
[0050] Start to evacuate the mixture and slowly raise the temperature to 150-160°C. Keep the temperature for 4 hours. When the acid value is less than 1, the reaction is complete.
[0051] Cool down to 60℃, break the vacuum with nitrogen, and close the vacuum after reaching normal pressure;
[0052] Add 99g of maleic anhydride, slowly raise the temperature to 60-70°C, keep the temperature for 2 hours, and the reaction is complete when the acid value is between 110-115;
[0053] Slowly add 183g water and 128g sodium sulfite, stir evenly, slowly heat to 50-60°C, stir and react for 2 hours at this temperature, and measure the pH of 1% aqueous solution>6, the reaction is complete;
[0054] The temperature was lowered to below 50°C and a light yellow to yellow liquid was collected.
[0055] Embodiment 4:
[0056] Weigh three portions of 0.2g of Disperse Red SR respectively to prepare 200ml solutions A1, B1 and C1, add the product obtained in Example 1 to A1 in an amount of 3g / L, add tristyrylphenol polyoxyethylene polyether ammonium sulfate to B1 in an amount of 3g / L, do not add any product to C1, adjust the pH to 5 with acetic acid, add the above three liquids to a sealed steel cup, put it in an all-purpose color tester (RAPID 2010ECO DYER), set the temperature to rise at 2°C / min, keep the dye solution at 130°C for 40 minutes, cool it to 90°C, use qualitative filter paper to measure the dispersibility, and obtain the following: Figure 1 , Figure 2 , Figure 3 Results shown.
[0057] Embodiment five:
[0058] Weigh three portions of 0.2g of Disperse Red SR respectively to prepare 200ml solutions A2, B2 and C2, add the product obtained in Example 1 to A2 in an amount of 2g / L, add tristyrylphenol polyoxyethylene polyether ammonium sulfate to B2 in an amount of 2g / L, do not add any product to C2, adjust the pH to 5 with acetic acid, add the above three liquids to a sealed steel cup, put it in an all-purpose color tester (RAPID 2010ECO DYER), set the temperature to rise at 2°C / min, keep the dye solution at 130°C for 40 minutes, cool it to 90°C, use qualitative filter paper to measure the dispersibility, and obtain the following: Figure 4 , Figure 5 , Figure 6 Results shown.
[0059] Embodiment six:
[0060] Weigh three portions of 0.2g of Disperse Red SR respectively to prepare 200ml solutions A3, B3 and C3, add the product obtained in Example 1 to A3 in an amount of 1g / L, add tristyrylphenol polyoxyethylene polyether ammonium sulfate to B3 in an amount of 1g / L, do not add any product to C3, adjust the pH to 5 with acetic acid, add the above three liquids to a sealed steel cup, put it in an all-purpose color tester (RAPID 2010ECO DYER), set the temperature to rise at 2°C / min, keep the dye solution at 130°C for 40 minutes, cool it to 90°C, use qualitative filter paper to measure the dispersibility, and obtain the following: Figure 7 , Figure 8 , Fig. 9 Results shown.
[0061] according to Figure 1-3 , Figure 4-6 , Figure 7-9 It can be seen that compared with the test results without adding any dispersant, the product prepared in Example 1 and the tristyrylphenol polyoxyethylene polyether ammonium sulfate in the prior art have good dispersion effects, and by comparing the test results of A1 and B1, A2 and B2, A3 and B3, it can be seen that the dispersion effect of the product prepared in Example 1 is slightly better than that of tristyrylphenol polyoxyethylene polyether ammonium sulfate; Figure 1 , Figure 4 , Figure 7 It can be seen from the changes that with the increase in the amount of this product added, the dispersion effect gradually increases.
[0062] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution of the present invention, which should be included in the scope of the claims of the present invention.
Claims
1. A dye dispersant, characterized in that: The dye dispersant is oleic acid polyethylene glycol maleic acid diester carboxylic acid sulfonic acid sodium salt, and its structural formula is 2. A dye dispersant according to claim 1, characterized in that: The dye dispersant is firstly obtained by reacting oleic acid polyethylene glycol ester with maleic anhydride to obtain oleic acid polyethylene glycol maleic acid ester carboxylic acid; and then obtained by reacting oleic acid polyethylene glycol maleic acid ester carboxylic acid with sodium sulfite.
3. A dye dispersant according to claim 2, characterized in that, The structural formula of the oleic acid polyethylene glycol maleate carboxylic acid is 4. A method for preparing a dye dispersant, characterized in that: The following steps are involved: Step 1: Add a catalyst to oleic acid and polyethylene glycol at a temperature of 60-70°C and stir evenly, then evacuate and slowly heat to 150-160°C to react to obtain oleic acid polyethylene glycol ester, then cool to 60°C and break the vacuum to normal pressure; Step 2, adding maleic anhydride, slowly heating to 60-70° C., reacting to obtain polyethylene glycol oleate and maleic anhydride; Step 3, slowly add water and sodium sulfite, stir evenly, slowly raise the temperature to 50-60° C., and react to obtain oleic acid polyethylene glycol maleic acid diester carboxylic acid sulfonic acid sodium salt.
5. The method for preparing a dye dispersant according to claim 4, characterized in that: In the step 1, the catalyst is p-toluenesulfonic acid.
6. The method for preparing a dye dispersant according to claim 4, characterized in that: In the step 1, when the acid value of the reaction solution is measured to be less than 1, the reaction is completed.
7. The method for preparing a dye dispersant according to claim 4, characterized in that: In the step 1, when oleic acid and polyethylene glycol are stirred, the temperature is raised to 60-70° C. by steam.
8. The method for preparing a dye dispersant according to claim 4, characterized in that: In the step 1, the vacuum is broken by using an inert gas.
9. The method for preparing a dye dispersant according to claim 4, characterized in that: In the step 2, the acid value of the reaction solution is measured to be between 110-115, and the reaction is completed.
10. The method for preparing a dye dispersant according to claim 4, characterized in that: In the step 3, when the pH of the 1% aqueous solution after the reaction is measured to be greater than 6, the reaction is completed.