Method for recovering carbon fibers in carbon fiber composite material
Through the swelling pretreatment and catalytic degradation treatment, the problem of carbon fiber recycling in carbon fiber pultrusion plates is solved, and low-temperature and efficient recycling is achieved, energy consumption is reduced and the recycling value of carbon fiber is improved.
Patent Information
- Application Number
- CN202411303085.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-19
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art is difficult to effectively recycle carbon fiber in carbon fiber pultruded plates, resulting in waste of resources and environmental pollution, and the recycling temperature is high and energy consumption is large, which limits the recycling value of carbon fiber.
The carbon fiber composite material is swelled pretreated by using the first solvent, and then the resin is degraded using an inorganic base and/or a catalytic solution prepared by organic base and organic amine to reduce the recovery temperature and achieve efficient separation of carbon fiber and resin.
Efficient recycling of carbon fiber at lower temperatures reduces energy consumption, retains the length of carbon fiber, improves its reuse value, and simplifies the recycling process.
Smart Images

Figure CN118978744A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of wind turbine blade materials, and in particular relates to a method for recycling carbon fibers in carbon fiber composite materials. Background Art
[0002] The development of renewable clean energy resources such as wind power will help significantly reduce air and water pollution and promote environmental sustainable development. In response to the cost pressure of the wind power industry in the era of parity, the wind power industry has achieved a reduction in the cost per kilowatt-hour by continuously increasing the length of wind turbine blades and expanding the capacity of wind turbine units.
[0003] Due to the characteristics of light weight and high strength, carbon fiber is usually prepared into carbon fiber pultruded plates for making the main beam components of wind turbine blades to ensure that the design load of super-large wind turbine blades is met. Under the premise of meeting the stiffness and strength, carbon fiber is 25% to 30% lighter than fiberglass blades. Carbon fiber pultruded plates are usually made of thermosetting resin and carbon fiber yarn through pultrusion. A large amount of waste carbon fiber pultruded plate materials will be generated in the manufacturing process of carbon fiber pultruded plates and main beams. However, due to its abnormal chemical stability, the thermosetting resin in the carbon fiber pultruded plate makes it extremely difficult to degrade and recycle the carbon fiber pultruded plate, and a large amount of accumulated waste plates will have a huge impact on the environment. In addition, the carbon fiber in the carbon fiber pultruded plate is expensive, and the continuous abandonment of the carbon fiber pultruded plate also causes a waste of carbon fiber resources.
[0004] The prior art has disclosed a method for dissolving epoxy thermosetting materials by mild alcoholysis, a method for recovering epoxy thermosetting resins and composite materials by exchange reactions assisted by good solvents and involving small molecules, and a dual monomer reuse method for recovering and decomposing anhydride-cured epoxy resins. However, the degradation temperature of anhydride-cured epoxy resin composite materials with a similar structure to pultruded resins exceeds 50°C, and the energy consumption is relatively large. In addition, the use of a complex mechanical grinding pretreatment method has a significant impact on the size of the recycled carbon fiber, limiting the reuse value of the recycled carbon fiber. Compared with the homemade carbon fiber composite materials used in the prior art, the commercial carbon fiber pultruded board has a higher degree of resin curing, a smaller porosity of the composite material, and greater difficulty in efficient degradation. Therefore, it is urgent to develop a low-temperature, simple method for recovering carbon fiber and resin from composite materials such as carbon fiber pultruded boards. Summary of the invention
[0005] The embodiments of the present application provide a method for recycling carbon fibers in carbon fiber composite materials, which can efficiently recycle carbon fibers from carbon fiber composite materials at a relatively low recycling temperature.
[0006] In a first aspect, the present application provides a method for recycling carbon fibers in carbon fiber composite materials, comprising:
[0007] Using a first solvent to perform swelling pretreatment on the carbon fiber composite material to swell the resin of the carbon fiber composite material to obtain a pretreated composite material;
[0008] The resin of the pre-treated composite material is degraded by using a catalytic solution prepared with an inorganic base and / or an organic base and an organic amine to recover the carbon fiber.
[0009] According to an embodiment of the first aspect of the present application, the first solvent is selected from dichloromethane, dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetic acid or a combination thereof.
[0010] According to an embodiment of the first aspect of the present application, the volume ratio of the mass of the carbon fiber composite material to the first solvent is 1:(1-50).
[0011] According to an embodiment of the first aspect of the present application, a first solvent is used to perform swelling pretreatment on a carbon fiber composite material, comprising:
[0012] The carbon fiber composite material is placed in a first solvent for swelling pretreatment, and the swelling pretreatment time is 12 hours to 300 hours.
[0013] According to an embodiment of the first aspect of the present application, the inorganic base is selected from hydroxides of alkali metals.
[0014] According to an embodiment of the first aspect of the present application, the inorganic base is selected from sodium hydroxide, potassium hydroxide, lithium hydroxide or a combination thereof.
[0015] According to an embodiment of the first aspect of the present application, the organic base is selected from alkyl compounds of lithium, sodium and potassium.
[0016] According to an embodiment of the first aspect of the present application, the organic base is selected from butyl lithium, sodium tert-butoxide, potassium tert-butoxide or a combination thereof.
[0017] According to an embodiment of the first aspect of the present application, the organic amine is selected from 2-aminoethanol, iminodiethanol, hydrazine hydrate, propylenediamine, butylenediamine, diethylenetriamine, triethylenetetramine or a combination thereof.
[0018] According to an embodiment of the first aspect of the present application, the volume ratio of the mass of the inorganic base and / or the organic base to the organic amine is 1:(1-100).
[0019] According to an embodiment of the first aspect of the present application, the resin of the pre-treated composite material is degraded using a catalytic solution, comprising:
[0020] The pretreated composite material is immersed in a catalytic solution and subjected to degradation treatment at 50° C. to 140° C. to obtain a degradation solution;
[0021] The degradation liquid is subjected to separation treatment to separate the carbon fibers in the degradation liquid from a mixed liquid containing the degraded resin, and the carbon fibers are recovered.
[0022] The method for recovering carbon fibers from carbon fiber composite materials according to the embodiment of the present application is based on the swelling pretreatment of the carbon fiber composite material with a first solvent, and the method of degrading the resin of the pretreated composite material that has undergone swelling pretreatment using a catalytic solution prepared with an inorganic base and / or an organic base and an organic amine. This can reduce the recovery temperature of the carbon fiber, improve the degradation efficiency of the resin per unit time at the same temperature, and achieve efficient recovery of carbon fiber and resin. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] In order to more clearly illustrate the technical solution of the embodiments of the present application, the following is a brief introduction to the drawings required for use in the embodiments of the present application. For ordinary technicians in this field, other drawings can be obtained based on these drawings without any creative work.
[0024] Figure 1 is a schematic flow chart of a method for recycling carbon fibers in carbon fiber composite materials provided in an embodiment of the present application;
[0025] Figure 2 This is a physical picture corresponding to the method for recycling carbon fiber in carbon fiber composite material provided in Example 1 of the present application. DETAILED DESCRIPTION
[0026] The features and exemplary embodiments of various aspects of the present application will be described in detail below. In order to make the purpose, technical solutions and advantages of the present application clearer, the present application will be further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the specific embodiments described herein are only intended to explain the present application, rather than to limit the present application. For those skilled in the art, the present application can be implemented without the need for some of these specific details. The following description of the embodiments is only to provide a better understanding of the present application by illustrating the examples of the present application.
[0027] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of further restrictions, the elements defined by the statement "include..." do not exclude the presence of other identical elements in the process, method, article or device including the elements.
[0028] The inventors of the present application have discovered that carbon fiber pultruded plates are usually made by pultruding a thermosetting resin containing an ester bond and carbon fiber. Using an amine base hydrolysis reaction, the epoxy resin can be degraded and the carbon fiber can be effectively recycled.
[0029] In order to solve the problems of the prior art, the embodiment of the present application provides a method for recycling carbon fibers in carbon fiber composite materials. The method for recycling carbon fibers in carbon fiber composite materials provided by the present application is introduced below.
[0030] Figure 1 A schematic flow chart of a method for recycling carbon fibers in carbon fiber composite materials provided in one embodiment of the present application is shown.
[0031] like Figure 1 As shown, the method for recycling carbon fibers in carbon fiber composite materials of the present application comprises:
[0032] S1, using a first solvent to perform swelling pretreatment on the carbon fiber composite material to swell the resin of the carbon fiber composite material to obtain a pretreated composite material;
[0033] S2. Degrading the resin of the pretreated composite material using a catalytic solution prepared with an inorganic base and / or an organic base and an organic amine to recover the carbon fiber.
[0034] The method for recovering carbon fibers from carbon fiber composite materials according to the embodiment of the present application uses a first solvent to perform swelling pretreatment on the carbon fiber composite material, and uses a catalytic solution prepared with an inorganic base and / or an organic base and an organic amine to degrade the resin of the pretreated composite material that has undergone swelling pretreatment. This can significantly reduce the recovery temperature, improve the degradation efficiency of the resin per unit time at the same temperature, achieve the degradation of the resin, and efficiently recover the carbon fibers and resin.
[0035] The method for recovering carbon fibers from carbon fiber composite materials in the embodiment of the present application can achieve effective recovery of carbon fibers from carbon fiber composite materials at a relatively low temperature through a method of combined recovery by swelling an amine with a first solvent and then hydrolyzing it with an alkali.
[0036] In the embodiments of the present application, the carbon fiber composite material can be cut into suitable sizes to ensure that it can be placed in a container for pre-swelling treatment, so as to recover carbon fibers with longer lengths as much as possible.
[0037] In some embodiments of the present application, the first solvent is selected from dichloromethane, dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetic acid or a combination thereof.
[0038] In some embodiments of the present application, the mass ratio of the carbon fiber composite material to the volume ratio of the first solvent is 1:(1-50). Optionally, the mass ratio of the carbon fiber composite material to the first solvent is 1:(1-10).
[0039] Exemplarily, the volume ratio of the mass of the carbon fiber composite material to the first solvent is 1:2, 1:3, 1:5, 1:7, 1:8, 1:9, 1:11, 1:13, 1:14, 1:15, 1:16, 1:18, 1:20, 1:21, 1:23, 1:25, 1:28, 1:30, 1:32, 1:35, 1:36, 1:39, 1:40, 1:42, 1:44, 1:46, 1:48, 1:49.
[0040] It should be noted that the mass-to-volume ratio of the carbon fiber composite material and the first solvent is calculated based on the corresponding dimensions. For example, when the mass unit of the carbon fiber composite material is gram, the corresponding volume unit is milliliter; when the mass unit of the carbon fiber composite material is kilogram, the corresponding volume unit is liter; when the mass unit of the carbon fiber composite material is ton, the corresponding volume unit is cubic meter.
[0041] In some embodiments of the present application, the first solvent is used to perform swelling pretreatment on the carbon fiber composite material, comprising: placing the carbon fiber composite material in the first solvent for swelling pretreatment, and the swelling pretreatment time is 12 hours to 300 hours. Optionally, the swelling pretreatment time is 72 hours to 144 hours.
[0042] In the embodiments of the present application, the first solvent is used to pretreat the carbon fiber composite material according to the principle of like dissolves like, so as to increase the specific surface area inside the carbon fiber composite material so that the subsequent catalytic solution can degrade the resin around the carbon fiber. The temperature at which the first solvent is used to perform swelling pretreatment on the carbon fiber composite material is not limited, and it can be performed at room temperature, or the first solvent can be heated to ≤50°C for treatment.
[0043] In some embodiments of the present application, the inorganic base is selected from alkali metal hydroxides, alkali metal organic compounds or combinations thereof. Exemplarily, the inorganic base is selected from sodium hydroxide, potassium hydroxide, lithium hydroxide or combinations thereof.
[0044] In some embodiments of the present application, the organic base is selected from alkyl compounds of lithium, sodium, and potassium. Exemplarily, the organic base is selected from butyl lithium, sodium tert-butoxide, potassium tert-butoxide, or a combination thereof.
[0045] In some embodiments of the present application, the organic amine is selected from 2-aminoethanol, iminodiethanol, hydrazine hydrate, propylenediamine, butylenediamine, diethylenetriamine, triethylenetetramine or a combination thereof.
[0046] In some embodiments of the present application, the mass ratio of the inorganic base and / or organic base to the volume ratio of the organic amine is 1: (1 to 100). For example, the inorganic base and the organic amine can be used to prepare a catalytic solution according to the aforementioned ratio, or the organic base and the organic amine can be used to prepare a catalytic solution, or a mixture of the inorganic base and the organic base and the organic amine can be used to prepare a catalytic solution. For example, the mass volume ratio of the inorganic base and the organic amine is 1g: (2ml to 10ml), 3g: (5ml to 20ml), 1g: (25ml to 50ml), 1g: (30ml to 80ml), 1g: 90ml. When the mass unit of the inorganic base and / or the organic base is replaced by kilograms or tons, the volume of the organic amine is liters or cubic meters accordingly.
[0047] In the embodiment of the present application, based on the hydrolysis reaction of the resin in the catalytic solution, the degradation of the pre-swelled resin in the pre-treated composite material is completed, thereby achieving effective recovery of the carbon fiber in the carbon fiber composite material. After the resin is hydrolyzed, it is dissolved in the degradation solution, and the resin and the carbon fiber can be separated by filtration. The catalyst solution for degrading the resin is neutralized and filtered to achieve effective recovery of the degraded resin.
[0048] In some embodiments of the present application, a catalytic solution is used to degrade the resin of the pre-treated composite material, comprising:
[0049] The pretreated composite material is immersed in a catalytic solution and subjected to degradation treatment at 50° C. to 140° C. to obtain a degradation solution;
[0050] The degradation liquid is subjected to separation treatment to separate the carbon fibers in the degradation liquid from a mixed liquid containing the degraded resin, and the carbon fibers are recovered.
[0051] In an embodiment of the present application, the temperature of using a catalytic solution to degrade the resin of the pretreated composite material is relatively low, the energy consumption is small, and there is no need to use a complex mechanical grinding pretreatment method, so that the recycled carbon fiber can retain an effective length. Exemplarily, the temperature at which the pretreated composite material is immersed in the catalytic solution for degradation treatment can be 55°C, 56°C, 58°C, 60°C, 65°C, 68°C, 70°C, 72°C, 75°C, 79°C, 80°C, 81°C, 83°C, 85°C, 88°C, 90°C, 2°C, 94°C, 96°C, 97°C, 100°C, 104°C, 105°C, 107°C, 110°C, 115°C, 18°C, 120°C, 125°C, 128°C, 130°C, 135°C, 136°C, 138°C.
[0052] In some embodiments of the present application, the degradation treatment time is 1 hour to 36 hours. Optionally, the degradation treatment time is 10 hours to 36 hours.
[0053] By using the method for recycling carbon fibers in carbon fiber composite materials according to the embodiment of the present application, carbon fibers with a length of 80 mm to 83 mm can be recycled. The recycling value of carbon fibers with such a length can be significantly increased.
[0054] Exemplarily, a method for recycling carbon fibers in carbon fiber composite materials comprises:
[0055] Weigh 10 g to 100 g of a carbon fiber pultruded plate sample and place it in a glass reactor, add dichloromethane as a first solvent to the glass reactor for sealing, perform swelling pretreatment on the carbon fiber pultruded plate sample, the mass ratio of the carbon fiber pultruded plate sample to the volume ratio of the first solvent is 1: (1 to 50), treat the sealed glass reactor at room temperature for 12 hours to 168 hours, take out the carbon fiber pultruded plate and place it in a vacuum drying oven for full drying to obtain a pretreated carbon fiber pultruded plate;
[0056] Sodium hydroxide and 2-aminoethanol are added to a glass reaction bottle to prepare a catalytic solution, wherein the mass ratio of sodium hydroxide to 2-aminoethanol is 1: (1-100), the dried pretreated carbon fiber pultruded board is placed in the catalytic solution of the glass reaction bottle and sealed, and the sealed glass reaction bottle is placed in an oil bath pot at 50°C to 140°C for degradation treatment, and the degradation time is 1 hour to 36 hours. After the degradation reaction is completed, the degradation liquid is separated to separate the carbon fiber in the degradation liquid and the mixed liquid containing the degraded resin, and the recovered carbon fiber is taken out, washed with anhydrous ethanol, and dried to recover the carbon fiber.
[0057] The method for recycling carbon fibers in carbon fiber composite materials according to the embodiment of the present application is applicable to the degradation and recycling of ester-bonded resins and carbon fiber composite materials, including but not limited to pultruded materials and vacuum infusion materials.
[0058] Test Section
[0059] Example 1
[0060] A method for recycling carbon fiber in carbon fiber composite materials comprises: weighing 10±1g of carbon fiber pultruded plate specimens and placing them in a glass reactor, such as Figure 2 As shown, 60 mL of dichloromethane was added to the glass reactor and sealed. In the initial state, dichloromethane was transparent and the carbon fiber pultruded plate was black. The glass reactor was placed in an oil bath at a constant temperature of 30°C for 72 hours for pre-swelling treatment to swell the resin of the carbon fiber pultruded plate. The carbon fiber pultruded plate specimen was taken out to wipe off the surface liquid and placed in a vacuum drying oven to fully dry to remove the solvent inside the carbon fiber pultruded plate specimen to obtain a pre-treated carbon fiber pultruded plate.
[0061] Add 75mL of ethanolamine and 1.35 of NaOH to the glass reaction bottle, soak the dried pretreated carbon fiber pultrusion plate in the fully mixed NaOH / ethanolamine solution, keep the oil bath at a constant temperature of 00℃, place the sealed glass reaction bottle in the oil bath for degradation treatment, and observe the degradation effect at different times. According to the degradation effect, the temperature of the oil bath can be adjusted to 100℃ for degradation for 32 hours, then adjusted to 120℃ for degradation for 2 hours, and finally cooled to 140℃ for continued degradation for 2 hours. After the degradation is completed, the following is obtained: Figure 2 The black degradation liquid containing degraded resin and carbon fiber is used to separate the carbon fiber in the degradation liquid from the mixed liquid containing the degraded resin, and the carbon fiber is taken out, washed with anhydrous ethanol, and dried to recover the carbon fiber. Among them, the yellow catalytic solution used for degradation can be directly recovered and reused without any treatment for the second degradation treatment.
[0062] Example 2
[0063] A method for recycling carbon fiber in carbon fiber composite materials, comprising: weighing 10±1g of a carbon fiber pultruded plate sample and placing it in a glass reactor, adding 60mL of dimethyl sulfoxide into the glass reactor and sealing it, wherein the dichloromethane is transparent and the carbon fiber pultruded plate is black in the initial state. The glass reactor is placed in an oil bath at a constant temperature of 30°C for 120 hours for pre-swelling treatment to swell the resin of the carbon fiber pultruded plate, taking out the carbon fiber pultruded plate sample and wiping off the surface liquid, placing it in a vacuum drying oven and fully drying it to remove the solvent inside the carbon fiber pultruded plate sample, and obtaining a pre-treated carbon fiber pultruded plate.
[0064] Add 75mL of ethanolamine and 1.35g of NaOH to a glass reaction bottle, soak the dried pretreated carbon fiber pultruded plate in a fully mixed NaOH / ethanolamine solution, keep the oil bath at a constant temperature of 00°C, place the sealed glass reaction bottle in an oil bath for degradation treatment, and observe the degradation effect at different times. According to the degradation effect, the temperature of the oil bath can be adjusted to 100°C for degradation for 32 hours, then adjusted to 120°C for degradation for 2 hours, and finally cooled to 140°C for continued degradation for 2 hours. After the degradation is completed, a black degradation liquid containing degraded resin and carbon fiber is obtained, and the carbon fiber in the degradation liquid and the mixed liquid containing the degraded resin are separated, and the carbon fiber is taken out, washed with anhydrous ethanol, and dried, that is, the carbon fiber is recovered. Among them, the yellow catalytic solution used for degradation can be recycled and reused.
[0065] Example 3
[0066] A method for recycling carbon fiber in carbon fiber composite materials, comprising: weighing 10±1g of a carbon fiber pultruded plate sample and placing it in a glass reactor, adding 60mL of dichloromethane to the glass reactor and sealing it, wherein the dichloromethane is transparent in the initial state and the carbon fiber pultruded plate is black. The glass reactor is placed in an oil bath at a constant temperature of 30°C for 72 hours for pre-swelling treatment to swell the resin of the carbon fiber pultruded plate, taking out the carbon fiber pultruded plate sample and wiping off the surface liquid, placing it in a vacuum drying oven and fully drying it to remove the solvent inside the carbon fiber pultruded plate sample, and obtaining a pre-treated carbon fiber pultruded plate.
[0067] Add 75mL of ethanolamine and 3.79g of sodium tert-butoxide to a glass reaction bottle, soak the dried pretreated carbon fiber pultrusion plate in a well-mixed sodium tert-butoxide / ethanolamine solution, keep the oil bath at a constant temperature of 100°C, place the sealed glass reaction bottle in an oil bath for degradation treatment, and observe the degradation effect at different times. According to the degradation effect, the temperature of the oil bath can be adjusted to 100°C for degradation for 32 hours, then adjusted to 120°C for degradation for 2 hours, and finally cooled to 140°C for continued degradation for 2 hours. After the degradation is completed, a black degradation solution containing degraded resin and carbon fiber is obtained, and the carbon fiber in the degradation solution and the mixed solution containing the degraded resin are separated, and the carbon fiber is taken out, washed with anhydrous ethanol, and dried, that is, the carbon fiber is recovered. Among them, the yellow catalytic solution used for degradation can be recycled and reused.
[0068] Example 4
[0069] A method for recycling carbon fiber in carbon fiber composite materials, comprising: weighing 10±1g of a carbon fiber pultruded plate sample and placing it in a glass reactor, adding 60mL of dichloromethane to the glass reactor and sealing it, wherein the dichloromethane is transparent in the initial state and the carbon fiber pultruded plate is black. The glass reactor is placed in an oil bath at a constant temperature of 30°C for 72 hours for pre-swelling treatment to swell the resin of the carbon fiber pultruded plate, taking out the carbon fiber pultruded plate sample and wiping off the surface liquid, placing it in a vacuum drying oven and fully drying it to remove the solvent inside the carbon fiber pultruded plate sample, and obtaining a pre-treated carbon fiber pultruded plate.
[0070] Add 129mL of iminodiethanol and 1.35g of NaOH to a glass reaction bottle, soak the dried pretreated carbon fiber pultrusion plate in a fully mixed NaOH / iminodiethanol solution, keep the oil bath at a constant temperature of 100°C, place the sealed glass reaction bottle in an oil bath for degradation treatment, and observe the degradation effect at different times. According to the degradation effect, the temperature of the oil bath can be adjusted to 100°C for degradation for 32 hours, then adjusted to 120°C for degradation for 2 hours, and finally cooled to 140°C for continued degradation for 2 hours. After the degradation is completed, a black degradation solution containing degraded resin and carbon fiber is obtained, and the carbon fiber in the degradation solution and the mixed solution containing the degraded resin are separated, and the carbon fiber is taken out, washed with anhydrous ethanol, and dried, that is, the carbon fiber is recovered. Among them, the yellow catalytic solution used for degradation can be recycled and reused.
[0071] Example 5
[0072] A method for recycling carbon fibers in carbon fiber composite materials, comprising:
[0073] Weigh 10±1g of carbon fiber pultruded sheet specimen and place it in a glass reactor. Figure 2 As shown, 60 mL of dichloromethane was added to the glass reactor and sealed. In the initial state, dichloromethane was transparent and the carbon fiber pultruded plate was black. The glass reactor was placed in an oil bath at a constant temperature of 30°C for 72 hours to allow the resin of the carbon fiber pultruded plate to swell. The carbon fiber pultruded plate specimen was taken out to wipe off the surface liquid, and was placed in a vacuum drying oven to be fully dried to remove the solvent inside the carbon fiber pultruded plate specimen to obtain a pretreated carbon fiber pultruded plate.
[0074] Add 129mL of iminodiethanol and 3.79g of sodium tert-butoxide to the glass reaction bottle, soak the dried pretreated carbon fiber pultrusion plate in the fully mixed sodium tert-butoxide / iminodiethanol solution, keep the oil bath at a constant temperature of 100°C, place the sealed glass reaction bottle in the oil bath for degradation treatment, and observe the degradation effect at different times. According to the degradation effect, the temperature of the oil bath can be adjusted to 100°C for degradation for 32 hours, then adjusted to 120°C for degradation for 2 hours, and finally cooled to 140°C for continued degradation for 2 hours. After the degradation is completed, the following is obtained: Figure 2 The black degradation liquid containing degraded resin and carbon fiber is used to separate the carbon fiber in the degradation liquid from the mixed liquid containing the degraded resin, and the carbon fiber is taken out, washed with anhydrous ethanol, and dried to recover the carbon fiber. Among them, the yellow catalytic solution used for degradation can be recovered and reused.
[0075] Comparative Example 1
[0076] A fresh CFRP composite material (13.9 g, size 5.5 cm x 7.5 cm x 3 cm) was placed in a beaker, and 150 ml of a 0.3 mol / L TBD-EG / NMP solution (EG and NMP accounted for 10% and 90% by volume, respectively) was added and heated at 170°C for 1.5 hours. The soaked product was washed with acetone and then dried. The carbon fiber was recovered with almost the same size and shape. Among them, TBD is 1,5,7-triazabicyclo[4.4.0]dec-5-ene, EG is ethylene glycol, NMP is N-methyl-2-pyrrolidone, and CFRP is a carbon fiber reinforced polymer.
[0077] The recovery efficiency of the fibers in the carbon fiber pultruded plates in Examples 1-5 is:
[0078] RG=WF1 / WF0*100%(1),
[0079] In formula (1), RG is the recovery efficiency of carbon fiber in the composite carbon fiber pultruded board, which is also the removal efficiency of resin in the carbon fiber pultruded board; WF1 is the mass (g) of the recycled carbon fiber after degradation; WF0 is the mass of carbon fiber in the carbon fiber pultruded board, which is calculated based on the mass content of the used carbon fiber in the carbon fiber pultruded board × the mass (g) of the carbon fiber pultruded board to be degraded.
[0080] The recovery efficiency of the carbon fiber in the carbon fiber pultruded plate of this embodiment is calculated according to formula (1), as shown in the following Table 1:
[0081] Table 1
[0082]
[0083] By comparing the above embodiments and comparative examples, it can be concluded that:
[0084] Although Comparative Example 1 can remove the resin of the CFRP composite material by using a TBD-EG / NMP (10 / 90) solution to obtain carbon fibers of suitable length, it needs to be processed at 170° C., which consumes a lot of energy.
[0085] Taking Example 1 as an example, as shown in Table 1, the mass of the carbon fiber calculated according to the carbon fiber content in the initial state of the carbon fiber pultruded plate is 8.4182g. After being treated by the method for recycling carbon fiber in carbon fiber composite materials according to the embodiment of the present application, the recovery efficiency of the carbon fiber is as high as 97.04%, and the length of the carbon fiber recovered by the method for recycling carbon fiber in carbon fiber composite materials according to the present application can reach 81.08mm. The carbon fiber recovery efficiency of Examples 2-5 is also as high as 97.71% to 98.29%, and the length of the recovered carbon fiber is 80.27mm to 81.59mm.
[0086] The above test results indicate that the method for recycling carbon fibers in carbon fiber composite materials according to the embodiment of the present application can efficiently recover carbon fibers from carbon fiber pultruded boards at a relatively low temperature, and the length of the recovered carbon fibers can reach more than 80 mm.
[0087] The above is only a specific implementation method of the present application. Those skilled in the art can clearly understand that for the convenience and simplicity of description, the specific working process described above can refer to the corresponding process in the aforementioned method embodiment, and will not be repeated here. It should be understood that the protection scope of the present application is not limited to this. Any technician familiar with the technical field can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the protection scope of the present application.
Claims
1. A method for recycling carbon fibers in carbon fiber composite materials, characterized in that: include: Using a first solvent to perform swelling pretreatment on the carbon fiber composite material to swell the resin of the carbon fiber composite material to obtain a pretreated composite material; The resin of the pretreated composite material is degraded by using a catalytic solution prepared with an inorganic base and / or an organic base and an organic amine to recover the carbon fiber.
2. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: The first solvent is selected from dichloromethane, dimethyl sulfoxide, N,N-dimethylformamide, acetone, acetic acid or a combination thereof.
3. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: The mass ratio of the carbon fiber composite material to the volume ratio of the first solvent is 1:(1-50).
4. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: The step of using the first solvent to perform swelling pretreatment on the carbon fiber composite material comprises: The carbon fiber composite material is placed in the first solvent for swelling pretreatment, and the swelling pretreatment time is 12 hours to 300 hours.
5. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: The inorganic base is selected from alkali metal hydroxides, and / or The organic base is selected from alkyl compounds of lithium, sodium and potassium.
6. The method for recycling carbon fibers in carbon fiber composite materials according to claim 5, characterized in that: The inorganic base is selected from sodium hydroxide, potassium hydroxide, lithium hydroxide or a combination thereof.
7. The method for recycling carbon fibers in carbon fiber composite materials according to claim 5, characterized in that: The organic base is selected from butyl lithium, sodium tert-butoxide, potassium tert-butoxide or a combination thereof.
8. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: The organic amine is selected from 2-aminoethanol, iminodiethanol, hydrazine hydrate, propylenediamine, butylenediamine, diethylenetriamine, triethylenetetramine or a combination thereof.
9. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: In the catalytic solution, the volume ratio of the inorganic base and / or organic base to the organic amine is 1:(1-100).
10. The method for recycling carbon fibers in carbon fiber composite materials according to claim 1, characterized in that: The method of using a catalytic solution to degrade the resin of the pretreated composite material comprises: Immersing the pretreated composite material in a catalytic solution at 50° C. to 140° C. for degradation treatment to obtain a degradation solution; The degradation liquid is subjected to separation treatment to separate the carbon fibers in the degradation liquid from a mixed liquid containing the degraded resin, and the carbon fibers are recovered.
Citation Information
Patent Citations
Pyrolysis catalyst for waste carbon fiber reinforced resin composite and carbon fiber recycling method
CN106807425A
Normal-pressure solvent recovery method of amine cured epoxy resin-based carbon fiber reinforced composite material
CN111793246A
Swelling dissociation recovery method for waste carbon fiber reinforced resin-based composite material
CN114539611A
Solvation crushing and recycling method of waste ester-group-containing thermosetting resin or composite material thereof
CN116355279A
Catalyst for thermal degradation of carbon-fiber-and-resin-based composite material and application method therefor
WO2021088123A1
Cited By
Method for efficiently decomposing and regenerating resin-based composite material
WO2026172576A1