Flame-retardant synthetic plastic and preparation method thereof

By grafting the phosphorus and boron flame retardants on the surface of magnesium hydroxide, forming a composite flame retardant, the problems of poor compatibility and low flame retardant efficiency of magnesium hydroxide and polypropylene matrix are solved, and excellent resistance of synthetic plastics is achieved Improved combustion and mechanical properties.

CN118978766AInactive Publication Date: 2024-11-19LINYI SANXIN PLASTIC PACKAGING PROD CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411119281.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-19
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Magnesium hydroxide has strong polarity, large surface energy, good hydrophilicity, easy to agglomerate, poor compatibility with polypropylene matrix, affecting the processing moldability and application performance of the product. At the same time, its flame retardant efficiency is not high, and more than 60% is required to be added. Only by achieving better flame retardant effect.

Method used

Graft the phosphorus and boron-based flame retardants on the surface of magnesium hydroxide to form a composite flame retardant, including three flame retardant elements: magnesium hydroxide, phosphorus and boron. Through the synergistic effect of different flame retardants, the flame retardant is improved. Its compatibility and flame retardant properties with polypropylene substrates and achieves excellent flame retardant effects at lower addition amounts.

Benefits of technology

By grafting the aliphatic hydrocarbon chain and carbon-carbon double bonds on the surface of magnesium hydroxide, the compatibility and cross-linking density of the composite flame retardant and the polypropylene matrix are improved, and the flame retardant and mechanical properties of synthetic plastics are significantly improved, achieving the following A good flame retardant effect is achieved at low addition amount.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004994554300000081
    Figure BDA0004994554300000081
  • Figure BDA0004994554300000091
    Figure BDA0004994554300000091
Patent Text Reader

Abstract

The invention relates to a flame-retardant synthetic plastic and a preparation method thereof, and belongs to the technical field of thermoplastic plastics, the flame-retardant synthetic plastic comprises the following components by weight: 80-92 parts of polypropylene resin, 12-28 parts of a composite flame retardant, 6-11 parts of a flexibilizer, and 0.6-1.2 parts of an antioxidant. According to the technical scheme, the phosphorus-based flame retardant and the boron-based flame retardant are grafted on the surface of magnesium hydroxide, so that the prepared composite flame retardant contains the inorganic flame retardant magnesium hydroxide and three flame-retardant elements of phosphorus, nitrogen and boron at the same time, and through the synergistic effect of different flame retardants, better flame-retardant performance can be achieved under the condition of lower additive amount. Besides, an aliphatic hydrocarbon chain and a carbon-carbon double bond are grafted on the surface of magnesium hydroxide, the aliphatic hydrocarbon chain and a polypropylene molecular chain have relatively high compatibility, and the carbon-carbon double bond can participate in a subsequent melt polymerization process of polypropylene plastic, so that the crosslinking density is improved, and meanwhile, the compatibility of the composite flame retardant and a polypropylene matrix can be further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of thermoplastic plastics, and in particular relates to a flame retardant synthetic plastic and a preparation method thereof. Background Art

[0002] Polypropylene is a thermoplastic with good heat resistance, low water absorption, and high comprehensive mechanical properties. It is widely used in electronic appliances, auto parts, modern office supplies, etc. However, due to the disadvantage of polypropylene being flammable, its application in some fields is limited.

[0003] Magnesium hydroxide is an inorganic additive flame retardant that can form a carbonized layer on the surface of the material to prevent the entry of oxygen and heat. At the same time, the magnesium hydroxide decomposes to generate magnesium oxide, which is a high-grade refractory material and has an excellent flame retardant effect. However, magnesium hydroxide has a strong polarity, a large surface energy, good hydrophilicity, is easy to agglomerate, and has poor compatibility with the polypropylene matrix, which affects the processing and application performance of the product. Moreover, the flame retardant efficiency of magnesium hydroxide as a flame retardant is not high, and more than 60% needs to be added to give the plastic substrate a better flame retardant effect. Therefore, it is necessary to modify magnesium hydroxide to improve the compatibility of magnesium hydroxide with the polypropylene matrix and at the same time improve the flame retardant properties of the plastic. Summary of the invention

[0004] The object of the present invention is to provide a flame-retardant synthetic plastic and a preparation method thereof, wherein phosphorus-based flame retardants and boron-based flame retardants are grafted onto the surface of magnesium hydroxide, so that the prepared composite flame retardant contains inorganic flame retardant magnesium hydroxide and three flame retardant elements of phosphorus, nitrogen and boron at the same time, and through the synergistic effect between different flame retardants, better flame retardant performance can be achieved at a lower addition amount. In addition, aliphatic hydrocarbon chains and carbon-carbon double bonds are grafted onto the surface of magnesium hydroxide, and the aliphatic hydrocarbon chains have high compatibility with polypropylene molecular chains, and the carbon-carbon double bonds can participate in the subsequent melt polymerization process of polypropylene plastics to increase the crosslinking density, and at the same time, the compatibility of the composite flame retardant with the polypropylene matrix can be further improved.

[0005] The technical problem to be solved by the present invention is that magnesium hydroxide has strong polarity, large surface energy, good hydrophilicity, easy agglomeration, and poor compatibility with the polypropylene matrix, thereby affecting the processing and application performance of the product. Moreover, the flame retardant efficiency of magnesium hydroxide as a flame retardant is not high, and more than 60% needs to be added to give the plastic substrate a good flame retardant effect.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A flame retardant synthetic plastic comprises the following components in parts by weight: 80-92 parts of polypropylene resin, 12-28 parts of composite flame retardant, 6-11 parts of toughening agent and 0.6-1.2 parts of antioxidant.

[0008] Furthermore, the toughening agent is at least one of ethylene-octene copolymer, ethylene propylene diene monomer rubber, and ethylene-vinyl acetate copolymer.

[0009] Furthermore, the antioxidant is at least one of antioxidant 1010 , antioxidant 168 , and antioxidant 264 .

[0010] Furthermore, the preparation method of the composite flame retardant comprises the following steps:

[0011] A1. Disperse magnesium hydroxide in an ethanol aqueous solution of epoxy group-containing silane coupling agent KH560, stir evenly, and then reflux for reaction at 60-70° C. for 3-5 hours. After the reaction is completed, centrifuge, wash, and dry to obtain epoxy group-modified magnesium hydroxide;

[0012] Furthermore, in step A1, the concentration of the ethanol aqueous solution of the epoxy group-containing silane coupling agent is 2-10%.

[0013] Furthermore, in step A1, the mass ratio of magnesium hydroxide to the epoxy group-containing silane coupling agent is 50:8-12.

[0014] A2, adding epoxy group-modified magnesium hydroxide, 3,5-diaminophenylboronic acid and a promoter into anhydrous ethanol, stirring and reacting at room temperature for 2-7 hours, filtering, washing and drying to obtain intermediate 1;

[0015] In the above preparation process, the epoxy group on the surface of magnesium hydroxide reacts with one of the amino groups on 3,5-diaminophenylboric acid, so that 3,5-diaminophenylboric acid is grafted onto the surface of magnesium hydroxide, and the molar ratio of the epoxy group on the surface of magnesium hydroxide and 3,5-diaminophenylboric acid is controlled to be close to 1:1.

[0016] Furthermore, in step A2, the mass ratio of epoxy group-modified magnesium hydroxide, 3,5-diaminophenylboric acid, accelerator and anhydrous ethanol is (7-9): (1-1.3): (0.05-0.08): (40-60).

[0017] Furthermore, in step A2, the accelerator is at least one of 1-methylimidazole, 2-methylimidazole, and 2-ethyl-4-methylimidazole.

[0018] A3, dispersing intermediate 1 in tetrahydrofuran, then adding a mixture of 6-chloro-1-hexene, sodium carbonate and tetrahydrofuran, stirring and reacting for 3-5 hours, filtering, washing and drying after the reaction to obtain intermediate 2;

[0019] In the above preparation process, the primary amino group and the secondary amino group on the intermediate 1 undergo a substitution reaction with the -Cl on the 6-chloro-1-hexene molecule, and the intermediate 2 molecule obtained also contains a secondary amino group. The molar ratio of the amino group on the intermediate 1 to the 6-chloro-1-hexene is controlled to be close to 1:2, so that a carbon-carbon double bond is grafted on the surface of the magnesium hydroxide.

[0020] Furthermore, in step A3, the mass ratio of the intermediate 1, 6-chloro-1-hexene and sodium carbonate is (5.2-6.8):(0.9-1.2):(0.42-0.48).

[0021] A4. Mix dimethyl phosphite, carbon tetrachloride and tetrahydrofuran, stir under ice bath conditions, then add triethylamine and a tetrahydrofuran mixture of intermediate 2, and react at room temperature for 12-15 hours. After the reaction is completed, filter, wash and dry to obtain a composite flame retardant.

[0022] In the above preparation process, -NH- contained in the intermediate 2 undergoes an Atherton-Todd reaction with dimethyl phosphite, and the molar ratio of -NH- contained in the intermediate 2 to dimethyl phosphite is controlled to be close to 1:1.

[0023] Furthermore, in step A4, the usage ratio of dimethyl phosphite, carbon tetrachloride, triethylamine and intermediate 2 is (11-12):(15.5-16.1):(10-10.8):(153-186).

[0024] The composite flame retardant prepared above contains the inorganic flame retardant magnesium hydroxide and three flame retardant elements of phosphorus, nitrogen and boron. Through the synergistic effect between different flame retardants, better flame retardant performance can be achieved at a lower addition amount.

[0025] A method for preparing a flame retardant synthetic plastic comprises the following steps:

[0026] The polypropylene resin, toughening agent, composite flame retardant and antioxidant are uniformly mixed, added into a twin-screw extruder, and subjected to melt extrusion granulation and drying treatment to obtain a flame retardant synthetic plastic.

[0027] Beneficial effects of the present invention:

[0028] (1) In the technical solution of the present invention, the prepared composite flame retardant contains the inorganic flame retardant magnesium hydroxide and three flame retardant elements of phosphorus, nitrogen and boron. Through the synergistic effect between different flame retardants, the prepared synthetic plastic has excellent flame retardant properties.

[0029] (2) In the technical solution of the present invention, aliphatic hydrocarbon chains and carbon-carbon double bonds are grafted on the surface of magnesium hydroxide. The aliphatic hydrocarbon chains have high compatibility with the polypropylene molecular chains. The carbon-carbon double bonds can participate in the subsequent melt polymerization process of the polypropylene plastic, thereby increasing the crosslinking density and thus improving the mechanical properties of the plastic. At the same time, the compatibility of the composite flame retardant with the polypropylene matrix can be further improved. DETAILED DESCRIPTION

[0030] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Example 1

[0032] This embodiment provides a method for preparing a composite flame retardant, comprising the following steps:

[0033] A1. Disperse 5 kg of magnesium hydroxide in 40 L of 2% KH560 ethanol aqueous solution, stir evenly, and then reflux at 60 ° C for 3 h. After the reaction, centrifuge, wash and dry to obtain epoxy group-modified magnesium hydroxide;

[0034] A2, adding 3.5 kg of epoxy group-modified magnesium hydroxide, 0.5 kg of 3,5-diaminophenylboronic acid and 25 g of 1-methylimidazole to 20 L of anhydrous ethanol, stirring and reacting at room temperature for 2 h, filtering, washing and drying to obtain intermediate 1;

[0035] A3, 2.6 kg of intermediate 1 was dispersed in 25 L of tetrahydrofuran, and then a mixture of 0.45 kg of 6-chloro-1-hexene, 0.21 kg of sodium carbonate and 1.9 L of tetrahydrofuran was added, and the mixture was stirred for 3 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2;

[0036] A4. Mix 110 g of dimethyl phosphite, 155 g of carbon tetrachloride and 100 mL of tetrahydrofuran, stir in an ice-water bath, then add 10 L of a tetrahydrofuran mixture containing 100 g of triethylamine and 1.53 kg of intermediate 2, and react at room temperature for 12 h. After the reaction is completed, filter, wash and dry to obtain a composite flame retardant.

[0037] Example 2

[0038] This embodiment provides a method for preparing a composite flame retardant, comprising the following steps:

[0039] A1. Disperse 5 kg of magnesium hydroxide in 20 L of 5% KH560 ethanol aqueous solution, stir evenly, and then reflux at 60 ° C for 5 hours. After the reaction, centrifuge, wash and dry to obtain epoxy group-modified magnesium hydroxide;

[0040] A2, adding 4.1 kg of epoxy group-modified magnesium hydroxide, 0.58 kg of 3,5-diaminophenylboronic acid and 29 g of 2-methylimidazole to 25 L of anhydrous ethanol, stirring and reacting at room temperature for 5 h, filtering, washing and drying to obtain intermediate 1;

[0041] A3, 3.2 kg of intermediate 1 was dispersed in 25 L of tetrahydrofuran, and then a mixture of 0.55 kg of 6-chloro-1-hexene, 0.22 kg of sodium carbonate and 2 L of tetrahydrofuran was added, and the mixture was stirred for 4 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2;

[0042] A4. Mix 115 g of dimethyl phosphite, 158 g of carbon tetrachloride and 100 mL of tetrahydrofuran, stir in an ice-water bath, then add 10 L of a tetrahydrofuran mixture containing 103 g of triethylamine and 1.66 kg of intermediate 2, and react at room temperature for 13 h. After the reaction is completed, filter, wash and dry to obtain a composite flame retardant.

[0043] Example 3

[0044] This embodiment provides a method for preparing a composite flame retardant, comprising the following steps:

[0045] A1. Disperse 5 kg of magnesium hydroxide in 15 L of 8% KH560 ethanol aqueous solution, stir evenly, and then reflux for reaction at 70° C. for 3 h. After the reaction, centrifuge, wash, and dry to obtain epoxy group-modified magnesium hydroxide.

[0046] A2, adding 4.5 kg of epoxy group-modified magnesium hydroxide, 0.65 kg of 3,5-diaminophenylboric acid and 40 g of 2-ethyl-4-methylimidazole to 30 L of anhydrous ethanol, stirring and reacting at room temperature for 7 h, filtering, washing and drying to obtain intermediate 1;

[0047] A3, 3.4 kg of intermediate 1 was dispersed in 25 L of tetrahydrofuran, and then a mixture of 0.6 kg of 6-chloro-1-hexene, 0.24 kg of sodium carbonate and 2 L of tetrahydrofuran was added, and the mixture was stirred for 5 h. After the reaction was completed, the mixture was filtered, washed and dried to obtain intermediate 2;

[0048] A4. Mix 120 g of dimethyl phosphite, 161 g of carbon tetrachloride and 100 mL of tetrahydrofuran, stir in an ice-water bath, then add 10 L of a tetrahydrofuran mixture containing 108 g of triethylamine and 1.86 kg of intermediate 2, and react at room temperature for 15 h. After the reaction is completed, filter, wash and dry to obtain a composite flame retardant.

[0049] Example 4

[0050] A flame retardant synthetic plastic comprises the following components in parts by weight: 80 parts of polypropylene resin, 12 parts of the composite flame retardant prepared in Example 2, 6 parts of ethylene-octene copolymer, and 0.6 parts of antioxidant 1010.

[0051] The method for preparing a flame retardant synthetic plastic comprises the following steps:

[0052] Weigh the above-mentioned components in parts by weight, mix the polypropylene resin, ethylene-octene copolymer, the composite flame retardant prepared in Example 2 and the antioxidant 1010 evenly, add them into a twin-screw extruder, and after melt extrusion granulation and drying, a flame-retardant synthetic plastic is obtained. In the twin-screw extruder, the three-stage temperatures are 150°C, 180°C and 200°C respectively.

[0053] Example 5

[0054] A flame retardant synthetic plastic comprises the following components in parts by weight: 85 parts of polypropylene resin, 16 parts of the composite flame retardant prepared in Example 2, 9 parts of EPDM rubber, and 0.9 parts of antioxidant 1010.

[0055] The method for preparing a flame retardant synthetic plastic comprises the following steps:

[0056] Weigh the above-mentioned components in parts by weight, mix the polypropylene resin, EPDM rubber, the composite flame retardant prepared in Example 2 and the antioxidant 1010 evenly, add them into a twin-screw extruder, and perform melt extrusion granulation and drying to obtain a flame-retardant synthetic plastic. In the twin-screw extruder, the three-stage temperatures are 150°C, 180°C and 200°C respectively.

[0057] Example 6

[0058] A flame retardant synthetic plastic comprises the following components in parts by weight: 89 parts of polypropylene resin, 28 parts of the composite flame retardant prepared in Example 2, 10 parts of EPDM rubber, and 1 part of antioxidant 168.

[0059] The method for preparing a flame retardant synthetic plastic comprises the following steps:

[0060] Weigh the above-mentioned components in parts by weight, mix the polypropylene resin, EPDM rubber, the composite flame retardant prepared in Example 2 and the antioxidant 168 evenly, add them into a twin-screw extruder, and perform melt extrusion granulation and drying to obtain a flame-retardant synthetic plastic. In the twin-screw extruder, the three-stage temperatures are 150°C, 180°C and 200°C respectively.

[0061] Example 7

[0062] A flame retardant synthetic plastic comprises the following components in parts by weight: 92 parts of polypropylene resin, 25 parts of the composite flame retardant prepared in Example 2, 9 parts of ethylene-vinyl acetate copolymer, and 1.1 parts of antioxidant 168.

[0063] The method for preparing a flame retardant synthetic plastic comprises the following steps:

[0064] Weigh the above-mentioned components in parts by weight, mix the polypropylene resin, ethylene-vinyl acetate copolymer, the composite flame retardant prepared in Example 2 and the antioxidant 168 evenly, add them into a twin-screw extruder, and perform melt extrusion granulation and drying to obtain a flame-retardant synthetic plastic. In the twin-screw extruder, the three-stage temperatures are 150°C, 180°C and 200°C respectively.

[0065] Example 8

[0066] A flame retardant synthetic plastic comprises the following components in parts by weight: 92 parts of polypropylene resin, 22 parts of the composite flame retardant prepared in Example 2, 11 parts of ethylene-vinyl acetate copolymer, and 1.2 parts of antioxidant 264.

[0067] The method for preparing a flame retardant synthetic plastic comprises the following steps:

[0068] Weigh the above-mentioned components in parts by weight, mix the polypropylene resin, ethylene-vinyl acetate copolymer, the composite flame retardant prepared in Example 2 and the antioxidant 264 evenly, add them into a twin-screw extruder, and after melt extrusion granulation and drying, a flame-retardant synthetic plastic is obtained. In the twin-screw extruder, the three-stage temperatures are 150°C, 180°C and 200°C respectively.

[0069] Comparative Example 1

[0070] Compared with Example 6, the composite flame retardant in Comparative Example 1 did not undergo step A4, that is, it did not contain a phosphorus-based flame retardant, and the other steps and raw materials were the same as those in Examples 2 and 6.

[0071] Comparative Example 2

[0072] Compared with Example 6, the composite flame retardant in Comparative Example 2 did not undergo step A3, that is, it did not contain an aliphatic hydrocarbon chain containing a carbon-carbon double bond, and the other steps and raw materials were the same as those of Examples 2 and 6.

[0073] Comparative Example 3

[0074] Compared with Example 6, the composite flame retardant in Comparative Example 3 did not undergo step A2, i.e., it did not contain a boron-based flame retardant. The surface of the magnesium hydroxide was first grafted with a silane coupling agent containing an amino group, and then reacted with 6-chloro-1-hexene and dimethyl phosphite in sequence. The other steps and raw materials were the same as those of Examples 2 and 6.

[0075] Performance Testing

[0076] (1) Mechanical properties: The tensile strength was tested according to GB / T 1040.2-2022 standard. The specimen size was 150 mm × 20 mm × 4 mm and the running speed was 50 mm / min. The results are shown in Table 1.

[0077] (2) Flame retardant properties: The oxygen index was tested using an XZT-100A oxygen index tester in accordance with GB / T2406.2-2009. The vertical burning test (UL-94) was tested in accordance with GB / T 2408-2021. The results are shown in Table 1.

[0078] Table 1

[0079]

[0080]

[0081] It can be seen from the data in Table 1 that the synthetic plastic prepared by the present invention has excellent mechanical properties and flame retardant properties. It can be seen from the data of Example 6 and Comparative Examples 1 and 3 that the addition of phosphorus flame retardant and boron flame retardant significantly improves the flame retardant properties of the synthetic plastic. It can be seen from the data of Example 6 and Comparative Example 2 that the tensile strength of the synthetic plastic is significantly improved due to the presence of carbon-carbon double bonds and aliphatic hydrocarbon chains.

[0082] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0083] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A flame retardant synthetic plastic, characterized in that: The invention comprises the following components in parts by weight: 80-92 parts of polypropylene resin, 12-28 parts of composite flame retardant, 6-11 parts of toughening agent, and 0.6-1.2 parts of antioxidant; The preparation method of the composite flame retardant comprises the following steps: A1. Disperse magnesium hydroxide in an ethanol aqueous solution of epoxy group-containing silane coupling agent KH560, stir evenly, and then reflux for reaction at 60-70° C. for 3-5 hours. After the reaction is completed, centrifuge, wash, and dry to obtain epoxy group-modified magnesium hydroxide; A2, adding epoxy group-modified magnesium hydroxide, 3,5-diaminophenylboronic acid and a promoter into anhydrous ethanol, stirring and reacting at room temperature for 2-7 hours, filtering, washing and drying to obtain intermediate 1; A3, dispersing intermediate 1 in tetrahydrofuran, then adding a mixture of 6-chloro-1-hexene, sodium carbonate and tetrahydrofuran, stirring and reacting for 3-5 hours, filtering, washing and drying after the reaction to obtain intermediate 2; A4. Mix dimethyl phosphite, carbon tetrachloride and tetrahydrofuran, stir under ice bath conditions, then add triethylamine and a tetrahydrofuran mixture of intermediate 2, and react at room temperature for 12-15 hours. After the reaction is completed, filter, wash and dry to obtain a composite flame retardant.

2. The flame retardant synthetic plastic according to claim 1, characterized in that: In the step A1, the concentration of the ethanol aqueous solution of the epoxy group-containing silane coupling agent is 2-10%.

3. The flame retardant synthetic plastic according to claim 1, characterized in that: In the step A1, the mass ratio of magnesium hydroxide to the epoxy group-containing silane coupling agent is 50:8-12.

4. The flame retardant synthetic plastic according to claim 1, characterized in that: In the step A2, the mass ratio of epoxy group-modified magnesium hydroxide, 3,5-diaminophenylboric acid, accelerator and anhydrous ethanol is (7-9): (1-1.3): (0.05-0.08): (40-60).

5. The flame retardant synthetic plastic according to claim 1, characterized in that: In the step A2, the accelerator is at least one of 1-methylimidazole, 2-methylimidazole, and 2-ethyl-4-methylimidazole.

6. The flame retardant synthetic plastic according to claim 1, characterized in that: In the step A3, the mass ratio of the intermediate 1, 6-chloro-1-hexene and sodium carbonate is (5.2-6.8):(0.9-1.2):(0.42-0.48).

7. The flame retardant synthetic plastic according to claim 1, characterized in that: In the step A4, the usage ratio of dimethyl phosphite, carbon tetrachloride, triethylamine and intermediate 2 is (11-12): (15.5-16.1): (10-10.8): (153-186).

8. The flame retardant synthetic plastic according to claim 1, characterized in that: The toughening agent is at least one of ethylene-octene copolymer, ethylene propylene diene monomer rubber and ethylene-vinyl acetate copolymer.

9. The flame retardant synthetic plastic according to claim 1, characterized in that: The antioxidant is at least one of antioxidant 1010 , antioxidant 168 , and antioxidant 264 .

10. A method for preparing the flame retardant synthetic plastic according to any one of claims 1 to 9, characterized in that: The following steps are involved: The polypropylene resin, toughening agent, composite flame retardant and antioxidant are uniformly mixed, added into a twin-screw extruder, and subjected to melt extrusion granulation and drying treatment to obtain a flame retardant synthetic plastic.