ABS (Acrylonitrile Butadiene Styrene) resin, preparation method thereof and resin product
By optimizing the ratio and structure of ABS resin and combining anionic emulsifiers, the problems of insufficient heat resistance and electroplating performance of ABS resin are solved, and high-performance ABS resin preparation is achieved, with good heat resistance, electroplating performance and plating binding strength. .
Patent Information
- Application Number
- CN202411167667.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-23
AI Technical Summary
Existing ABS resins cannot take into account both good heat resistance and electroplating properties, resulting in easy deformation when heated, unqualified electroplating properties of the foundation, or insufficient binding force of the coating.
ABS graft copolymer and styrene-acrylonitrile copolymer are prepared by using specific ratio poly(butadiene-acrylonitrile) latex, styrene monomer, acrylonitrile monomer and initiator to control acrylonitrile The nitrile content is between 25% and 34%, combined with anionic emulsifiers such as 1.18-octadecanediate soap, the composition and structure of ABS resin are optimized.
It realizes good heat resistance, electroplating performance and comprehensive performance of ABS resin, improves the coating bonding force, ensures the basic electroplating and high temperature stability of the electroplating parts, and enhances the peel strength and fluidity of the injection molded parts.
Smart Images

Figure CN118978771A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of polymer material preparation, and in particular to ABS resin, a preparation method thereof and a resin product. Background Art
[0002] Butadiene-styrene-acrylonitrile copolymer (ABS) resin is a thermoplastic engineering plastic widely used in the industrial field. Usually, ABS resin is prepared by emulsion polymerization of ABS grafted with bulk styrene-acrylonitrile copolymer (SAN) blending method. This method first uses emulsion polymerization to synthesize polybutadiene (PB) latex, uses it as a seed emulsion to carry out graft polymerization reaction of styrene (St) and acrylonitrile (AN) to obtain ABS graft copolymer, and then melt blends it with SAN resin prepared by bulk method to obtain ABS resin.
[0003] The market demand for ABS is increasing day by day, and at the same time, the requirements for ABS performance are also increasing, and higher requirements are also put forward for the heat resistance and electroplating performance of electroplating grade ABS. Existing ABS resin has problems such as easy deformation under heat, unqualified basic electroplating performance or insufficient bonding strength of the coating. Summary of the invention
[0004] Therefore, the technical problem to be solved by the present invention is to overcome the defect of ABS resin in the prior art that it cannot have both good heat resistance and electroplating performance, thus leading to the problems of easy deformation under heat, unqualified basic electroplating properties or insufficient coating bonding strength.
[0005] The invention provides an ABS resin, comprising an ABS graft copolymer and a styrene-acrylonitrile copolymer. The raw materials of the ABS graft copolymer include, by weight, 20-30 parts of poly(butadiene-acrylonitrile) latex, 4-18 parts of styrene monomers, 1-10 parts of acrylonitrile monomers, 0.001-2 parts of an initiator and 5-65 parts of water. The acrylonitrile content in the styrene-acrylonitrile copolymer is less than 34% and greater than 25%.
[0006] The term acrylonitrile content refers to the mass percentage of acrylonitrile in the styrene-acrylonitrile copolymer. The test is carried out by the method of determining the N element content in the styrene-acrylonitrile copolymer by elemental analysis.
[0007] The term styrene monomer refers to styrene and its derivatives, and the styrene derivatives may include but are not limited to styrene substituted with 1 to 6 alkyl groups.
[0008] The term acrylonitrile monomer refers to acrylonitrile and its derivatives, and the acrylonitrile derivatives may include but are not limited to acrylonitrile substituted with 1 to 6 alkyl groups.
[0009] Further, the styrene monomer is selected from one or more of styrene, α-methylstyrene and p-methylstyrene; and / or, the acrylonitrile monomer is selected from one or more of acrylonitrile, methacrylonitrile and ethacrylonitrile; and / or, the initiator comprises an organic peroxide initiator; and / or, the particle size of the poly(butadiene-acrylonitrile) latex is 280-400nm.
[0010] The organic peroxide initiator comprises one or more of cumene hydroperoxide, benzoyl peroxide, tert-butyl benzoyl peroxide, and methyl ethyl ketone peroxide.
[0011] Furthermore, the raw materials of the ABS graft copolymer also include one or more of an activator, a molecular weight regulator and an emulsifier; Preferably, the activator comprises one or more of sodium pyrophosphite, ferrous sulfate and glucose; Preferably, the molecular weight regulator comprises an alkyl mercaptan containing 1 to 25 carbon atoms; Preferably, the emulsifier comprises an anionic emulsifier, more preferably, the anionic emulsifier is selected from one or more of alkylbenzene sulfonates with an alkyl carbon number between 6 and 22, alkyl sulfates with an alkyl carbon number between 6 and 22, fatty acid salts with an alkyl carbon number between 6 and 22, and disproportionated rosin acid soap; Preferably, based on 100 parts by weight of the raw material of the ABS graft copolymer, the activator accounts for 0.001-2 parts; Preferably, based on 100 parts by weight of the raw material of the ABS graft copolymer, the molecular weight regulator accounts for 0.05-0.1 parts; Preferably, based on 100 parts by weight of the raw material of the ABS graft copolymer, the emulsifier accounts for 0.05-0.2 parts.
[0012] Wherein, the alkyl mercaptan containing 1 to 25 carbon atoms comprises one or more of methyl mercaptan, n-dodecyl mercaptan, and n-hexadecyl mercaptan.
[0013] Alkyl sulfates having an alkyl carbon number between 6 and 22 include sodium lauryl sulfate.
[0014] The alkylbenzene sulfonate having an alkyl carbon number between 6 and 22 includes sodium dodecylbenzene sulfonate.
[0015] The fatty acid salts with an alkyl carbon number between 6 and 22 include oleate and / or octadecane dioic acid soap.
[0016] In certain preferred embodiments, the emulsifier comprises one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, oleate, disproportionated rosin acid soap, and octadecane dioic acid soap.
[0017] The above-mentioned oleate may be potassium salt and / or sodium salt. The disproportionated rosin acid soap comprises disproportionated rosin acid potassium soap and / or disproportionated rosin acid sodium soap. The octadecane dioic acid soap comprises 1,18-octadecane dioic acid potassium soap and / or 1,18-octadecane dioic acid sodium soap. More preferably, the emulsifier is 1,18-octadecane dioic acid soap.
[0018] Further, the mass ratio of the ABS graft copolymer to the styrene-acrylonitrile copolymer is 70:30-30:70; and / or the acrylonitrile content in the styrene-acrylonitrile copolymer is 27-30%.
[0019] Further, the raw materials of the poly (butadiene - acrylonitrile) latex include 30-55 parts of butadiene, 2-10 parts of acrylonitrile, 0.05-0.5 parts of initiator and 40-110 parts of water in parts by weight; Optionally, the initiator is an inorganic peroxide initiator.
[0020] The inorganic peroxide initiator includes one or more of a persulfate initiator and a perphosphate initiator. The persulfate initiator includes one or more of potassium persulfate and sodium persulfate. The superphosphate includes one or more of potassium superphosphate and sodium superphosphate.
[0021] Furthermore, the raw materials of the poly(butadiene-acrylonitrile) latex also include one or more of a cross-linking agent, a molecular weight regulator, an emulsifier, and an electrolyte; Preferably, the cross-linking agent comprises an ester cross-linking agent and / or a divinyl cross-linking agent; Preferably, the molecular weight regulator comprises an alkyl mercaptan containing 1 to 25 carbon atoms; Preferably, the emulsifier comprises an anionic emulsifier, more preferably, the anionic emulsifier is selected from one or more of alkylbenzene sulfonates with an alkyl carbon number between 6 and 22, alkyl sulfates with an alkyl carbon number between 6 and 22, fatty acid salts with an alkyl carbon number between 6 and 22, and disproportionated rosin acid soaps, more preferably, the emulsifier is 1.18-octadecane dioic acid soap; Preferably, the electrolyte comprises potassium salt and / or sodium salt; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the cross-linking agent accounts for 0.01-0.3 parts; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the molecular weight regulator accounts for 0.01-0.3 parts; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the emulsifier accounts for 0.05-2.5 parts; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the electrolyte accounts for 0.1-1 part.
[0022] The ester crosslinking agent includes one or more of triethylene glycol dimethacrylate, ethylene glycol dimethacrylate, 1,4-butanediol dimethacrylate, hexanediol dimethacrylate, and trimethylolpropane trimethacrylate.
[0023] The divinyl crosslinking agent includes divinylbenzene.
[0024] The alkyl mercaptan containing 1 to 25 carbon atoms includes one or more of methyl mercaptan, n-dodecyl mercaptan, and n-hexadecyl mercaptan.
[0025] Alkyl sulfates having an alkyl carbon number between 6 and 22 include sodium lauryl sulfate.
[0026] The alkylbenzene sulfonate having an alkyl carbon number between 6 and 22 includes sodium dodecylbenzene sulfonate.
[0027] The fatty acid salts with an alkyl carbon number between 6 and 22 include oleate and / or octadecane dioic acid soap.
[0028] In certain preferred embodiments, the emulsifier comprises one or more of sodium dodecyl sulfate, sodium dodecylbenzene sulfonate, oleate, octadecane dioic acid soap, and disproportionated rosin acid soap.
[0029] The above-mentioned oleate may be potassium salt and / or sodium salt. The disproportionated rosin acid soap comprises disproportionated rosin acid potassium soap and / or disproportionated rosin acid sodium soap. The octadecane dioic acid soap comprises 1,18-octadecane dioic acid potassium soap and / or 1,18-octadecane dioic acid sodium soap.
[0030] Wherein, the potassium salt is selected from one or more of potassium carbonate, potassium chloride, potassium nitrate and potassium sulfate.
[0031] The sodium salt is selected from one or more of sodium carbonate, sodium chloride, sodium nitrate and sodium sulfate.
[0032] Furthermore, the mass ratio of butadiene to acrylonitrile is 80-95:20-5.
[0033] On the other hand, the present invention also provides a method for preparing ABS resin, comprising: mixing an ABS graft copolymer and a styrene-acrylonitrile copolymer to prepare the ABS resin; Optionally, the mixing is carried out at a temperature of 180-250°C.
[0034] For example, the conventional twin-screw extruder can be used for mixing, and then the mixture is water-cooled and granulated.
[0035] Furthermore, the preparation method of the ABS graft copolymer includes mixing poly(butadiene-acrylonitrile) latex, styrene monomer, acrylonitrile monomer, initiator and water, heating and polymerizing, and condensing to obtain the ABS graft copolymer; Optionally, the temperature of the heating polymerization is 50-90° C. and the time is 2-8 hours; Optionally, the coagulation process uses a coagulant, wherein the coagulant comprises an acid solution.
[0036] The coagulant may be a magnesium sulfate solution, for example, a magnesium sulfate aqueous solution with a concentration of 3-8 wt %.
[0037] Furthermore, the preparation method of the poly(butadiene-acrylonitrile) latex includes mixing butadiene, acrylonitrile, an initiator and water, heating and polymerizing to obtain the poly(butadiene-acrylonitrile) latex; Optionally, the reaction temperature of the heating polymerization is not more than 85° C., the reaction pressure is not more than 0.9 MPa, and the heating polymerization time is 10-40 hours; Optionally, the step of chemical agglomeration is further included after the thermal polymerization, for example, acetic acid is added for chemical agglomeration to increase the particle size of the latex to 350nm-400nm, and then alkali is added to pH=8-11.
[0038] The present invention also provides a resin product, which is an ABS resin prepared from the above ABS resin or the ABS resin preparation method described above.
[0039] The resin product of the present invention can be produced by conventional technical means, for example, ABS resin can be injection molded into various types of resin products by injection molding process.
[0040] The technical solution of the present invention has the following advantages: 1. The ABS resin provided by the present invention comprises an ABS graft copolymer and a styrene-acrylonitrile copolymer. The raw materials of the ABS graft copolymer include, by weight, 20-30 parts of poly(butadiene-acrylonitrile) latex, 4-18 parts of styrene monomers, 1-10 parts of acrylonitrile monomers, 0.001-2 parts of initiators and 5-65 parts of water. The acrylonitrile content in the styrene-acrylonitrile copolymer is less than 34% and greater than 25%. The electroplating-grade ABS resin is obtained by mixing an ABS graft copolymer obtained by using a specific ratio of poly(butadiene-acrylonitrile) latex, a styrene monomer, an acrylonitrile monomer, an initiator and water with the styrene-acrylonitrile copolymer and controlling the acrylonitrile content in the styrene-acrylonitrile copolymer to be less than 34% and greater than 25%. The ABS resin has good compatibility, good heat resistance and electroplating performance, and excellent comprehensive performance.
[0041] Among them, poly (butadiene - acrylonitrile) latex replaces polybutadiene latex, increasing the polarity of the rubber phase, which is beneficial to the grafting of styrene-acrylonitrile with acrylonitrile content less than 34% and greater than 25% on the one hand, and on the other hand, it enhances the corrosion resistance of the rubber phase. By controlling the acrylonitrile content of styrene-acrylonitrile copolymer to be less than 34% and greater than 25%, the chemical resistance can be improved, and the transitional etching of ABS by chromic acid during the roughening process can be prevented, thereby improving the bonding strength of the coating and improving the heat resistance and electroplating performance of ABS resin. After testing, the ABS resin has high flexibility, qualified basic electroplating performance, and no appearance defects such as dents and bulges on the surface after a high temperature test at 100°C.
[0042] In addition, the fluidity of the ABS resin prepared by the present invention is higher than that of the general ABS resin. High fluidity is conducive to stress release during molding of parts, can improve the phenomenon of plating leakage, help to improve the bonding force of the electroplating layer, and significantly improve the peeling strength of the injection molded parts.
[0043] 2. The ABS resin provided by the present invention has higher adsorption, emulsification stability and solubility than the emulsifiers commonly used in the polymerization of butadiene latex, such as disproportionate rosin soap or sodium dodecyl sulfate, by using an anionic emulsifier, especially 1.18-octadecane dioic acid soap as an emulsifier, so that the polymerization of nitrile latex and the graft polymerization of nitrile latex can be smoothly realized. The hydrophobic group of the emulsifier is a long-chain alkyl group, and the low concentration of the colloid formation reduces the usage amount, and the low molecular occupation area can achieve effective adsorption, thereby improving dispersion stabilization. The hydrophilic group introduces two carboxyl bases, the dispersion stabilization effect is increased, and the solubility is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0044] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0045] Figure 1 This is a particle size distribution diagram of the nitrile latex before adding acetic acid in Example 1 of the present invention; Figure 2 This is a particle size distribution diagram of the nitrile latex after adding acetic acid in Example 1 of the present invention; Figure 3 This is a particle size distribution diagram of the nitrile latex before adding acetic acid in Example 2 of the present invention; Figure 4 This is a particle size distribution diagram of the nitrile latex after adding acetic acid in Example 2 of the present invention; Figure 5This is a particle size distribution diagram of the nitrile latex before adding acetic acid in Example 3 of the present invention; Figure 6 This is a particle size distribution diagram of the nitrile latex after adding acetic acid in Example 3 of the present invention; in Figure 1-6 In the figure, the horizontal axis Size is the particle size, and the vertical axis Intensity (Percent) is the intensity (percent). DETAILED DESCRIPTION
[0046] The following examples are provided for a better understanding of the present invention, but are not intended to limit the best mode of implementation, nor to limit the content and protection scope of the present invention. Any product identical or similar to the present invention obtained by anyone under the inspiration of the present invention or by combining the features of the present invention with other prior arts shall fall within the protection scope of the present invention.
[0047] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in the field can be used. If no manufacturer is specified for the reagents or instruments used, they are all conventional reagent products that can be obtained commercially. Among them, TSC is the total solid content, which is determined according to GB∕T8298-2017.
[0048] Example 1 Poly(butadiene-acrylonitrile) latex A This embodiment provides a method for synthesizing poly(butadiene-acrylonitrile) latex A, which is carried out in a 10L high-pressure polymerization reactor, and the reaction process is carried out under nitrogen protection.
[0049] Add deionized water: 4400g, 1.18-octadecane dioic acid soap (purchased from Latemul ASK): 95g, potassium persulfate: 10.276g, potassium carbonate: 25.69g into the reactor, stir and mix evenly, then add butadiene: 2487.48g, acrylonitrile: 130.92g, divinylbenzene: 5.24g, and dodecyl mercaptan: 12.8g.
[0050] Start heating. Heat to 65°C in 1 hour. Adiabatically react at 65°C, control the reaction temperature not to exceed 85°C, and the reaction pressure not to exceed 0.9MPa. React for about 25 hours until the conversion rate reaches 98%, then terminate the reaction to obtain nitrile latex. Use a laser particle size analyzer (Zetasizer Nano ZS90, Malvern, UK) to measure the particle size. Figure 1 As shown, the average particle size is 106.5 nm and the PDI is 0.251.
[0051] The nitrile latex (pH = 10.5, particle size in the range of 106.5 nm) prepared above was gradually added with 10% acetic acid for chemical agglomeration. When the particle size was measured to be 350-400 nm, 10 wt % potassium hydroxide aqueous solution was added to pH = 10.5, and deionized water was added to adjust TSC = 30% to obtain poly (butadiene-acrylonitrile) latex A. Particle size was measured, see Figure 2 As shown, the average particle size is 352.4 nm, the PDI is 0.170, and the particle size distribution is uniform.
[0052] Example 2 Poly(butadiene-acrylonitrile) latex B This embodiment provides a method for synthesizing poly(butadiene-acrylonitrile) latex B, which is carried out in a 10L high-pressure polymerization reactor, and the reaction process is carried out under nitrogen protection.
[0053] Add deionized water: 4400g, 1.18-octadecane dioic acid soap: 95g, potassium persulfate: 10.276g, potassium carbonate: 25.69g into the reactor, stir and mix evenly, then add butadiene: 2356.56g, acrylonitrile 261.84g, divinylbenzene 7.7g, and dodecyl mercaptan 10.5g.
[0054] Start heating. When the temperature reaches 65℃ in 1 hour, conduct adiabatic reaction at 65℃, control the reaction temperature not to exceed 85℃, and the reaction pressure not to exceed 0.9MPa. React for about 25 hours until the conversion rate reaches 98%, then terminate the reaction to obtain nitrile latex. Measure the particle size, see Figure 3 As shown, the average particle size is 96.09 nm and the PDI is 0.192.
[0055] The nitrile latex (pH = 10, particle size 96.09 nm) prepared above was gradually added with 10% acetic acid for chemical agglomeration. When the particle size was measured to be 350-400 nm, 10 wt % potassium hydroxide aqueous solution was added to pH = 10, and deionized water was added to adjust TSC = 30% to obtain poly (butadiene-acrylonitrile) latex B. The particle size was measured, see Figure 4 As shown, the average particle size is 361.9 nm, the PDI is 0.229, and the particle size distribution is uniform.
[0056] Example 3 Poly(butadiene-acrylonitrile) latex C This embodiment provides a method for synthesizing poly(butadiene-acrylonitrile) latex C, which is carried out in a 10L high-pressure polymerization reactor, and the reaction process is carried out under nitrogen protection.
[0057] Add deionized water: 4400g, 1.18-octadecane dioic acid soap: 95g, potassium persulfate: 10.276g, potassium carbonate: 25.69g into the reactor, stir and mix evenly, then add butadiene: 2225.64g, acrylonitrile: 392.76g, divinylbenzene: 10.47g, and dodecyl mercaptan: 6.55g.
[0058] Start heating. When the temperature reaches 65℃ in 1 hour, conduct adiabatic reaction at 65℃, control the reaction temperature not to exceed 85℃, and the reaction pressure not to exceed 0.9MPa. React for about 25 hours until the conversion rate reaches 98%, then terminate the reaction to obtain nitrile latex. Measure the particle size, see Figure 5 As shown, the average particle size is 89.27 nm and the PDI is 0.131.
[0059] The nitrile latex (pH = 9.7, particle size 89.27nm) prepared above was gradually added with 10% acetic acid for chemical agglomeration. When the particle size was measured to be 350-400nm, 10wt% potassium hydroxide aqueous solution was added to pH = 10, and deionized water was added to adjust TSC = 30% to obtain poly (butadiene-acrylonitrile) latex C. The particle size was measured, see Figure 6 As shown, the average particle size is 377.2 nm, the PDI is 0.256, and the particle size distribution is uniform.
[0060] Example 4 Synthesis of ABS-2 This embodiment provides an ABS resin, including SAN (purchased from Kumho, South Korea, brand SAN-300NA, molecular weight M) with a mass ratio of 70:30. W 12.5×10 4 , 28% acrylonitrile content) and ABS graft copolymer. The raw materials of the ABS graft copolymer include: TSC=30% poly(butadiene-acrylonitrile) latex A prepared in Example 1: 1188g, styrene 171.072g, acrylonitrile 66.528g, cumene hydroperoxide 1.9g, deionized water 260g, dodecanethiol 2.376g, 1.18-octadecane dioic acid soap 4.2g, sodium pyrophosphite: 1.9008g, anhydrous glucose: 3.564g, ferrous sulfate: 0.0476g.
[0061] The preparation method comprises the following steps: S1. Polymerization reaction: Place poly (butadiene-acrylonitrile) latex in a polymerization kettle and pass nitrogen. Add 1.18-octadecane dioic acid soap and 200g deionized water and stir for 30 minutes. Mix sodium pyrophosphite, anhydrous glucose and ferrous sulfate, dissolve in 60g deionized water to prepare an activator solution. Mix dodecanethiol, cumene hydroperoxide, styrene and acrylonitrile to obtain a mixed monomer. Add the above activator solution into the polymerization kettle at one time and heat to 70°C. Add the mixed monomer dropwise for 4 hours, react for 2 hours, stop the reaction when the conversion rate reaches more than 98%, and obtain an emulsion.
[0062] S2, coagulation and drying: dilute the above emulsion with deionized water to about TSC=25%, and control the temperature at 50°C. Gradually add about 60g of 20% magnesium sulfate solution by mass, stirring while adding, until the polymer is completely coagulated. Wash the coagulated polymer with deionized water until the pH of the washing solution is 6-7. Dry in an oven at 80°C to obtain an ABS graft copolymer.
[0063] S3. Mixing: Add SAN and ABS graft copolymers in a mass ratio of 70:30 into the main feeder of a twin-screw extruder. The process conditions of the twin-screw extrusion are shown in Table 1. After extrusion, the ABS resin (denoted as ABS-2) is obtained by water cooling and granulation.
[0064] Table 1 Process conditions of twin-screw extrusion
[0065] The test specimens were prepared by injection molding machine and the performance tests were carried out. The results are shown in Tables 4 and 5.
[0066] Example 5 Synthesis of ABS-5 This embodiment provides an ABS resin, which is basically the same as Example 4, except that the type of poly(butadiene-acrylonitrile) latex is different. In this embodiment, the same mass of TSC=30% poly(butadiene-acrylonitrile) latex B prepared in Example 2 is used to replace poly(butadiene-acrylonitrile) latex A, and the remaining raw material amounts and processes are the same as those in Example 4.
[0067] Example 6 Synthesis of ABS-8 This embodiment provides an ABS resin, which is basically the same as Example 4, except that the type of poly(butadiene-acrylonitrile) latex is different. This embodiment uses the same mass of TSC=30% poly(butadiene-acrylonitrile) latex C prepared in Example 3 instead of poly(butadiene-acrylonitrile) latex A, and the remaining raw material amounts and processes are the same as those in Example 4.
[0068] Comparative Example 1 Synthesis of ABS-1 This comparative example provides an ABS resin, including SAN (purchased from Kumho, South Korea, brand SAN-326NA, molecular weight M) with a mass ratio of 70:30. W 12.6×10 4 , 25% acrylonitrile content) and ABS graft copolymer. The raw materials of ABS graft copolymer include: TSC=30% poly(butadiene-acrylonitrile) latex A: 1188g, styrene 178.2g, acrylonitrile 59.4g, cumene hydroperoxide 1.42g, deionized water 260g, dodecanethiol 2.376g, 1.18-octadecane dioic acid soap 4.2g, sodium pyrophosphite: 1.9008g, anhydrous glucose: 3.564g, ferrous sulfate: 0.0476g.
[0069] The preparation method comprises the following steps: S1. Polymerization reaction: Place poly (butadiene-acrylonitrile) latex in a polymerization kettle and pass nitrogen. Add 1.18-octadecane dioic acid soap and 200g deionized water and stir for 30 minutes. Mix sodium pyrophosphite, anhydrous glucose and ferrous sulfate, dissolve in 60g deionized water to prepare an activator solution. Mix dodecanethiol, cumene hydroperoxide, styrene and acrylonitrile to obtain a mixed monomer. Add the above activator solution into the polymerization kettle at one time and heat to 70°C. Add the mixed monomer dropwise for 4 hours, react for 2 hours, stop the reaction when the conversion rate reaches more than 98%, and obtain an emulsion.
[0070] S2, coagulation and drying: dilute the above emulsion with deionized water to about TSC=25%, and control the temperature at 50°C. Gradually add about 60g of 20% magnesium sulfate solution by mass, stirring while adding, until the polymer is completely coagulated. Wash the coagulated polymer with deionized water until the pH of the washing solution is 6-7. Dry in an oven at 80°C to obtain an ABS graft copolymer.
[0071] S3. Mixing: Add SAN and ABS graft copolymers in a mass ratio of 70:30 into the main feeder of a twin-screw extruder. The process conditions of the twin-screw extrusion are shown in Table 2. After extrusion, the ABS resin (denoted as ABS-1) is obtained by water cooling and granulation.
[0072] Table 2 Process conditions of twin-screw extrusion
[0073] The test specimens were prepared by injection molding machine and the performance test was carried out. The results are shown in Table 4.
[0074] Comparative Example 2 Synthesis of ABS-3 This comparative example provides an ABS resin, including SAN (purchased from Kumho, South Korea, brand SAN-350N HM, molecular weight M) with a mass ratio of 70:30. W 15.5×10 4 , 34% acrylonitrile content) and ABS graft copolymer. The raw materials of ABS graft copolymer include: TSC = 30% poly (butadiene-acrylonitrile) latex A: 1188g, styrene 156.816g, acrylonitrile 80.784g, cumene hydroperoxide 2.85g, deionized water 260g, dodecanethiol 2.376g, 1.18-octadecane dioic acid soap 4.2g, sodium pyrophosphite: 1.9008g, anhydrous glucose: 3.564g, ferrous sulfate: 0.0476g.
[0075] The preparation method comprises the following steps: S1. Polymerization reaction: Place poly (butadiene-acrylonitrile) latex in a polymerization kettle and pass nitrogen. Add 1.18-octadecane dioic acid soap and 200g deionized water and stir for 30 minutes. Mix sodium pyrophosphite, anhydrous glucose and ferrous sulfate, dissolve in 60g deionized water to prepare an activator solution. Mix dodecanethiol, cumene hydroperoxide, styrene and acrylonitrile to obtain a mixed monomer. Add the above activator solution into the polymerization kettle at one time and heat to 70°C. Add the mixed monomer dropwise for 4 hours, react for 2 hours, stop the reaction when the conversion rate reaches more than 98%, and obtain an emulsion.
[0076] S2, coagulation and drying: dilute the above emulsion with deionized water to about TSC=25%, and control the temperature at 50°C. Gradually add about 60g of 20% magnesium sulfate solution by mass, stirring while adding, until the polymer is completely coagulated. Wash the coagulated polymer with deionized water until the pH of the washing solution is 6-7. Dry in an oven at 80°C to obtain an ABS graft copolymer.
[0077] S3. Mixing: SAN and ABS graft copolymers were added into the main feeder of a twin-screw extruder according to a mass ratio of 70:30. The process conditions of the twin-screw extrusion are shown in Table 3. After extrusion, ABS resin (denoted as ABS-3) was obtained by water cooling and granulation.
[0078] Table 3 Process conditions of twin-screw extrusion
[0079] The test specimens were prepared by injection molding machine and the performance test was carried out. The results are shown in Table 4.
[0080] Comparative Example 3 Synthesis of ABS-4 This comparative example provides an ABS resin, which is basically the same as comparative example 1, except that the type of poly(butadiene-acrylonitrile) latex is different. This comparative example uses poly(butadiene-acrylonitrile) latex B of the same mass instead of poly(butadiene-acrylonitrile) latex A, and the remaining raw material amounts and processes are the same as those in comparative example 1.
[0081] Comparative Example 4 Synthesis of ABS-6 This comparative example provides an ABS resin, which is basically the same as comparative example 2, except that the type of poly(butadiene-acrylonitrile) latex is different. This comparative example uses poly(butadiene-acrylonitrile) latex B of the same mass instead of poly(butadiene-acrylonitrile) latex A, and the remaining raw material amounts and processes are the same as those in comparative example 2.
[0082] Comparative Example 5 Synthesis of ABS-7 This comparative example provides an ABS resin, which is basically the same as comparative example 1, except that the type of poly(butadiene-acrylonitrile) latex is different. This comparative example uses poly(butadiene-acrylonitrile) latex C of the same mass instead of poly(butadiene-acrylonitrile) latex A, and the remaining raw material amounts and processes are the same as those in comparative example 1.
[0083] Comparative Example 6 Synthesis of ABS-9 This comparative example provides an ABS resin, which is basically the same as comparative example 2, except that the type of poly(butadiene-acrylonitrile) latex is different. This comparative example uses poly(butadiene-acrylonitrile) latex C of the same mass instead of poly(butadiene-acrylonitrile) latex A, and the remaining raw material amounts and processes are the same as those in comparative example 2.
[0084] Comparative Example 7 Synthesis of ABS-10 This comparative example provides an ABS resin, which is basically the same as comparative example 1, except that the type of ABS graft copolymer is different. This comparative example uses commercially available Korean Kumho ABS-181 of the same quality to replace the ABS graft copolymer in comparative example 1.
[0085] Comparative Example 8 Synthesis of ABS-11 This comparative example provides an ABS resin, which is basically the same as Example 4, except that the type of ABS graft copolymer is different. This comparative example uses commercially available Korean Kumho ABS-181 of the same quality to replace the ABS graft copolymer in Example 4.
[0086] Comparative Example 9 Synthesis of ABS-12 This comparative example provides an ABS resin, which is basically the same as comparative example 2, except that the type of ABS graft copolymer is different. This comparative example uses commercially available Korean Kumho ABS-181 of the same quality to replace the ABS graft copolymer in comparative example 2.
[0087] Experimental Example 1 The ABS resins prepared in the embodiments and comparative examples were electroplated, and the basic electroplating performance, high temperature resistance and electroplating bonding strength of the electroplated parts were tested.
[0088] Basic electroplating performance (appearance): If there are no obvious defects and pitting on the surface of the electroplated parts, the basic electroplating performance is qualified, otherwise it is unqualified. If the basic electroplating performance is unqualified, the next test experiment will not be carried out.
[0089] High temperature resistance: Place the electroplated parts in a 100℃ high temperature test box for 6 hours, then take them out and cool them to room temperature. If there are no dents, bulges or other appearance defects on the surface of the product, the high temperature resistance is qualified, otherwise it is unqualified.
[0090] Electroplating bonding strength: The electroplated thermoplastic resin test piece was cut into 100mm*25mm specimens, and the electroplated specimen was subjected to a 90° peel strength test on a universal tensile testing machine according to ASTM B533 standard.
[0091] The results are shown in the following table: Table 4 Electroplating performance test results
[0092] Appendix: Products with unqualified basic electroplating performance will not be tested for electroplating bonding strength As shown in Table 4, the basic electroplating performance of Comparative Examples 1-7 and Comparative Example 9 is unqualified, and the surface of the electroplated parts has obvious defects and / or pitting. The bonding strength of Comparative Example 8 is poor. The ABS resins prepared in Examples 4-6 of the present invention have good basic electroplating performance and high temperature resistance and significantly improved peel strength, especially Examples 4 and 5 have significantly improved bonding strength of the coating.
[0093] Experimental Example 2 The ABS resin prepared in each embodiment was tested as follows: The melt index was tested by melt flow rate tester (model: GT-7100-MI) of High-speed Railway Inspection Company; impact strength test: measured according to GB / T1043.1-2008; notched impact strength was tested by cantilever beam impact tester (model: GT-HV2000A-C6W) of High-speed Railway Inspection Company; tensile strength test: tested according to GB / T1040.2-2006; bending performance test: tested according to GB / T9341-2008; tensile and bending tests were tested by universal testing machine (model: GT-TCS-2000) of High-speed Railway Inspection Company; Vicat softening point was tested by Vicat deformation tester (model: GTHV2000A-C5W) of High-speed Railway Inspection Company; dielectric constant and dissipation factor were tested by dielectric impedance spectrometer at 100 Hz according to IEC 6231-2-1, and the sample was a 20 mm×2 mm disc; volume resistivity and surface resistivity were tested by high resistance meter according to IEC 6231-3-1 Testing.
[0094] Comparative samples with unqualified electroplating performance will no longer be subject to basic performance testing.
[0095] Table 5 Basic performance test results
[0096] As can be seen from Table 5, the ABS resin prepared in each embodiment of the present invention has high Izod notched impact strength, tensile strength, flexural strength, and elongation at break, and has excellent mechanical properties; the melt index result is between 15 and 30 g / 10 min, and the fluidity is good; the dielectric constant is between 3 and 4, and the lower dielectric constant makes it have excellent insulation performance and reduce signal loss and interference; the soft point, dissipation factor, dielectric constant and resistivity also meet the basic performance requirements of electroplating.
[0097] Obviously, the above embodiments are merely examples for the purpose of clear explanation, and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived therefrom are still within the scope of protection of the invention.
Claims
1. An ABS resin, characterized in that: The invention comprises an ABS graft copolymer and a styrene-acrylonitrile copolymer. The raw materials of the ABS graft copolymer include, by weight, 20-30 parts of poly(butadiene-acrylonitrile) latex, 4-18 parts of styrene monomers, 1-10 parts of acrylonitrile monomers, 0.001-2 parts of an initiator and 5-65 parts of water. The acrylonitrile content in the styrene-acrylonitrile copolymer is less than 34% and greater than 25%.
2. The ABS resin according to claim 1, characterized in that The styrene monomer is selected from one or more of styrene, α-methylstyrene and p-methylstyrene; and / or, the acrylonitrile monomer is selected from one or more of acrylonitrile, methacrylonitrile and ethacrylonitrile; and / or, the initiator comprises an organic peroxide initiator; and / or, the particle size of the poly(butadiene-acrylonitrile) latex is 280-400nm.
3. The ABS resin according to claim 1 or 2, characterized in that: The raw materials of the ABS graft copolymer also include one or more of an activator, a molecular weight regulator and an emulsifier; Preferably, the activator comprises one or more of sodium pyrophosphite, ferrous sulfate and glucose; Preferably, the molecular weight regulator comprises an alkyl mercaptan containing 1 to 25 carbon atoms; Preferably, the emulsifier comprises an anionic emulsifier, more preferably, the anionic emulsifier is selected from one or more of alkylbenzene sulfonates with an alkyl carbon number between 6 and 22, alkyl sulfates with an alkyl carbon number between 6 and 22, fatty acid salts with an alkyl carbon number between 6 and 22, and disproportionated rosin acid soaps, more preferably, the emulsifier is 1.18-octadecane dioic acid soap; Preferably, based on 100 parts by weight of the raw material of the ABS graft copolymer, the activator accounts for 0.001-2 parts; Preferably, based on 100 parts by weight of the raw material of the ABS graft copolymer, the molecular weight regulator accounts for 0.05-0.1 parts; Preferably, based on 100 parts by weight of the raw material of the ABS graft copolymer, the emulsifier accounts for 0.05-0.2 parts.
4. The ABS resin according to any one of claims 1 to 3, characterized in that: The mass ratio of the ABS graft copolymer to the styrene-acrylonitrile copolymer is 70:30-30:70; and / or the acrylonitrile content in the styrene-acrylonitrile copolymer is 27-30%.
5. The ABS resin according to any one of claims 1 to 4, characterized in that: The raw materials of the poly (butadiene-acrylonitrile) latex include 30-55 parts of butadiene, 2-10 parts of acrylonitrile, 0.05-0.5 parts of initiator and 40-110 parts of water in parts by weight; Optionally, the initiator is an inorganic peroxide initiator.
6. The ABS resin according to claim 5, characterized in that The raw materials of the poly (butadiene-acrylonitrile) latex also include one or more of a cross-linking agent, a molecular weight regulator, an emulsifier, and an electrolyte; Preferably, the cross-linking agent comprises an ester cross-linking agent and / or a divinyl cross-linking agent; Preferably, the molecular weight regulator comprises an alkyl mercaptan containing 1 to 25 carbon atoms; Preferably, the emulsifier comprises an anionic emulsifier, more preferably, the anionic emulsifier is selected from one or more of alkylbenzene sulfonates with an alkyl carbon number between 6 and 22, alkyl sulfates with an alkyl carbon number between 6 and 22, fatty acid salts with an alkyl carbon number between 6 and 22, and disproportionated rosin acid soaps, more preferably, the emulsifier is 1.18-octadecane dioic acid soap; Preferably, the electrolyte comprises potassium salt and / or sodium salt; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the cross-linking agent accounts for 0.01-0.3 parts; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the molecular weight regulator accounts for 0.01-0.3 parts; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the emulsifier accounts for 0.05-2.5 parts; Preferably, based on 100 parts by weight of the raw material of the poly(butadiene-acrylonitrile) latex, the electrolyte accounts for 0.1-1 part.
7. The ABS resin according to claim 5, characterized in that The mass ratio of butadiene to acrylonitrile is 80-95:20-5.
8. A method for preparing the ABS resin according to any one of claims 1 to 7, characterized in that: The ABS graft copolymer and the styrene-acrylonitrile copolymer are mixed to prepare the ABS resin; Optionally, the mixing is carried out at a temperature of 180-250°C.
9. The method for preparing ABS resin according to claim 8, characterized in that: The preparation method of the ABS graft copolymer comprises: mixing poly(butadiene-acrylonitrile) latex, styrene monomer, acrylonitrile monomer, initiator and water, heating and polymerizing, and condensing to obtain the ABS graft copolymer; Optionally, the temperature of the heating polymerization is 50-90° C. and the time is 2-8 hours; Optionally, the coagulation process uses a coagulant, wherein the coagulant comprises an acid solution.
10. The method for preparing ABS resin according to claim 9, characterized in that: The preparation method of the poly (butadiene - acrylonitrile) latex comprises: taking butadiene, acrylonitrile, an initiator and water, mixing, heating and polymerizing, and preparing the poly (butadiene - acrylonitrile) latex; Optionally, the reaction temperature of the heating polymerization is not more than 85° C., the reaction pressure is not more than 0.9 MPa, and the heating polymerization time is 10-40 hours; Optionally, the thermal polymerization further comprises a chemical agglomeration step.
11. A resin product, characterized in that: An ABS resin prepared by the ABS resin described in any one of claims 1 to 7 or the method for preparing the ABS resin described in any one of claims 8 to 10.
Citation Information
Patent Citations
Heat-resisting ABS (Acrylonitrile-Butadiene-Styrene) resin applicable to electroplating and preparation method thereof
CN103342874A
ABS resin composition suitable for coating part
CN105733119A
Polybutadiene latex, preparation method thereof and ABS (Acrylonitrile Butadiene Styrene) resin
CN113024728A
High-toughness and high-rigidity ABS composite material dedicated to storage battery casings, preparation method therefor and application thereof