Light-weight high-strength epoxy foaming material and tablet computer rear cover prepared from same
By combining three foaming agents and using a three-stage foaming process, the foam structure is optimized, solving the problem of lightweight and high-strength epoxy foam materials, making it suitable for tablet computer back covers.
Patent Information
- Application Number
- CN202411065321.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-05
AI Technical Summary
Existing epoxy foam materials cannot simultaneously achieve the characteristics of being lightweight and high-strength. The cell structure has a significant impact on the strength and density of the material, making the selection of foaming agent and foaming method particularly important.
Three foaming agents are used in combination: foaming agent A is OBSH supported on porous silica, foaming agent B is low-boiling-point alkane coated with organic copolymer, and foaming agent C is a composite of modified filler high-hydrogen-content silicone oil and hollow glass microspheres. The foam morphology is optimized through a three-stage foaming process.
A lightweight and high-strength epoxy foam material has been developed, suitable for tablet computer back covers, improving the material's mechanical strength and corrosion resistance.
Smart Images

Figure BDA0004979187190000081
Abstract
Description
Technical Field
[0001] The invention relates to the field of epoxy foaming materials, and specifically discloses a lightweight and high-strength epoxy foaming material and a tablet computer back cover prepared therefrom. Background Art
[0002] The materials of mobile phone back covers are mainly metal or plastic. In recent years, plastic mobile phone back covers have attracted more and more attention due to their light weight, good wear resistance and easy processing. Epoxy foaming material is a commonly used material for making plastic mobile phone back covers. The epoxy resin foaming methods include physical foaming method, chemical foaming method and hollow microsphere method. The foaming process reduces the material density and also changes the medium state of the continuous distribution of the epoxy resin matrix. Therefore, the structural morphology of the pores has a great influence on the strength and density of the epoxy foam material.
[0003] The back cover of a mobile phone requires an epoxy foam material that has both light weight and high strength. Therefore, the selection of foaming agent and foaming method is particularly important. Therefore, it is of great significance to study a lightweight and high-strength epoxy foam material and a tablet computer back cover prepared therefrom. Summary of the invention
[0004] The object of the present invention is to provide a lightweight and high-strength epoxy foam material and a tablet computer back cover prepared therefrom, so as to solve the problems raised in the above-mentioned background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A lightweight and high-strength epoxy foam material, characterized in that it comprises the following raw materials, by mass: 100 parts of epoxy resin, 15 to 25 parts of curing agent, 2 to 3 parts of foaming agent A, 2 to 3 parts of foaming agent B, and 3 to 5 parts of foaming agent C;
[0006] The preparation of the foaming agent A comprises the following steps: supporting 4,4'-oxybisbenzenesulfonylhydrazide with porous silica to obtain the foaming agent A;
[0007] The preparation of the foaming agent B comprises the following steps: coating low boiling point alkane with an organic copolymer to obtain the foaming agent B;
[0008] The preparation of the foaming agent C comprises the following steps: taking hollow glass microspheres containing vinyl, bismaleimide, allyl glycidyl ether, and a solvent, stirring evenly, adding an initiator, heating and stirring to obtain a modified filler; taking high hydrogen-containing silicone oil and a modified filler, heating, adding chloroplatinic acid as a catalyst, reacting, and obtaining the foaming agent C.
[0009] More preferably, the curing agent includes one or two of triethylenetetramine and N-aminoethylpiperazine.
[0010] More optimally, the preparation of the foaming agent C comprises the following steps: Step 1: taking hollow glass microspheres, adding ethanol, water, and a vinyl silane coupling agent, stirring at 50-60° C. for 3-4 hours, filtering, washing, and drying to obtain hollow glass microspheres containing vinyl groups;
[0011] Step 2: Take hollow glass microspheres containing vinyl, bismaleimide, allyl glycidyl ether, azobisisobutyronitrile, and solvent, stir evenly, and stir at 75-85° C. for 2-3 hours to obtain a modified filler;
[0012] Step 3: Take high hydrogen silicone oil and modified filler, heat up, add chloroplatinic acid as a catalyst, heat to 155-160°C and react for 6-7h, heat to 175-180°C and keep under vacuum for 1-2h, and distill under reduced pressure to obtain foaming agent C.
[0013] More optimally, the hollow glass microspheres containing vinyl groups include the following raw materials, calculated by weight: 8 to 12 parts of hollow glass microspheres, 60 to 80 parts of ethanol, 60 to 80 parts of water, and 2 to 3 parts of vinyl silane coupling agent;
[0014] The modified filler comprises the following raw materials, calculated by weight: 10 to 15 parts of hollow glass microspheres containing vinyl groups, 3 to 5 parts of bismaleimide, 3 to 5 parts of allyl glycidyl ether, 30 to 50 parts of solvent (water and DMF in a volume ratio of 1:1), and an initiator in an amount of 0.02 to 0.03% by weight of bismaleimide;
[0015] The foaming agent C comprises the following raw materials, calculated by weight: 15 to 20 parts of high hydrogen-containing silicone oil, 2 to 3 parts of modified filler, and 0.01% of chloroplatinic acid catalyst by weight of the high hydrogen-containing silicone oil.
[0016] More optimally, the preparation of the foaming agent A includes the following steps: taking porous silica, ethanol, aminosilane coupling agent (KH550), and water, stirring evenly, stirring at 60-70° C. for 3-5 hours, filtering, and drying to obtain modified microspheres; taking an N,N-dimethylformamide solution of 4,4'-oxybisbenzenesulfonylhydrazine (DMF solution of OBSH), adding the modified microspheres, stirring at 40-50° C. for 10-12 hours, filtering, washing, and drying to obtain the foaming agent A.
[0017] More optimally, the modified microspheres include the following raw materials, calculated by mass: 0.2-0.4 parts of porous silica, 1-2 parts of ethanol, 0.8-1.2 parts of aminosilane coupling agent, and 1-2 parts of water; the foaming agent A includes the following raw materials, calculated by mass: 8-12 parts of N,N-dimethylformamide solution of 4,4'-oxybisbenzenesulfonylhydrazine, and 0.2-0.4 parts of modified microspheres; the concentration of the N,N-dimethylformamide solution of 4,4'-oxybisbenzenesulfonylhydrazine is 1-2 mol / L.
[0018] Preferably, the concentration of the N,N-dimethylformamide solution of 4,4'-oxybisbenzenesulfonylhydrazide is 1.8 mol / L.
[0019] More optimally, the preparation of the foaming agent B refers to the prior art, and includes the following steps: Step 1: adding sodium malate to the magnesium chloride ethanol solution, stirring, slowly adding ammonia water to precipitate, aging, washing, drying, adding water to disperse, and obtaining a nano magnesium hydroxide suspension; adding the nano magnesium hydroxide suspension, polyvinyl pyrrolidone, and sodium dodecyl sulfate into water, heating and stirring, and obtaining an aqueous phase;
[0020] Step 2: uniformly mix the polymer monomer, azobisisobutyronitrile, low boiling point alkane and trimethylolpropane trimethacrylate, and perform ultrasonic treatment to obtain an oil phase;
[0021] Step 3: Mix the oil phase and the water phase evenly, add epoxy resin and sodium hydroxymethyl cellulose, mix and emulsify to obtain a suspension; introduce nitrogen to pressurize, slowly heat to 42-45°C and keep warm for 25-30 minutes, keep warm at 48-52°C for 23-24 hours, heat to 56-60°C and keep warm for 4-5 hours, cool, wash, and dry to obtain foaming agent B.
[0022] More optimally, the polymer monomer includes one or more of acrylonitrile, ethylene glycol dimethacrylate, methyl methacrylate, and hydroxypropyl acrylate; and the low-boiling-point alkane is isopentane.
[0023] More optimally, the preparation method of the foaming agent B is as follows: Step 1: adding 5 parts of nano magnesium hydroxide suspension, 3 parts of polyvinyl pyrrolidone, and 6 parts of sodium dodecyl sulfate into water, heating to 45° C., stirring evenly, to obtain an aqueous phase;
[0024] The amount of deionized water added is 1.4 times the mass of the nano magnesium hydroxide suspension;
[0025] Step 2: 22 parts of polymer monomer, 5 parts of azobisisobutyronitrile, 6 parts of isopentane, and 2 parts of trimethylolpropane trimethacrylate were mixed evenly, and ultrasonicated at 30° C. for 5 minutes to obtain an oil phase;
[0026] Step 3: Mix the oil phase and the water phase evenly, add 13 parts of epoxy resin and 15 parts of sodium hydroxymethyl cellulose, mix and emulsify at 20°C and 4000r / min for 10 minutes to obtain a suspension;
[0027] Nitrogen was introduced to pressurize to 13 KPa, the temperature was slowly raised to 42°C and kept for 30 min, then kept at 48°C for 24 h, then raised to 58°C and kept for 5 h, then cooled, washed and dried to obtain foaming agent B;
[0028] The polymer monomers include the following raw materials, by mass percentage: 60% acrylonitrile, 2% ethylene glycol dimethacrylate, 30% methyl methacrylate, and 8% hydroxypropyl acrylate;
[0029] The preparation method of nano magnesium hydroxide suspension comprises the following steps: adding sodium malate to a 0.225 mol / L magnesium chloride ethanol solution, stirring at 43°C for 30 minutes, slowly dropping ammonia water for precipitation, aging at 8°C for 24 hours after the dropping is completed, washing with water until no chloride ions are detected, drying, and adding water to disperse into a nano magnesium hydroxide suspension with a mass concentration of 50%;
[0030] The amount of sodium malate added is 0.6% of the mass of the magnesium chloride ethanol solution; and the amount of ammonia water added is 18% of the mass of the magnesium chloride ethanol solution.
[0031] More optimally, the preparation of a tablet computer back cover made of any one of the above-mentioned lightweight and high-strength epoxy foam materials includes the following steps: taking epoxy resin, curing agent, foaming agent A, foaming agent B, and foaming agent C, mixing them evenly, injecting them into a mold, foaming at room temperature for 1 to 2 hours, heating to 65 to 75°C, and foaming for 1 to 2 hours; heating to 155 to 160°C, and foaming for 1 to 2 hours to obtain an epoxy foam material.
[0032] More optimally, the surface of the epoxy foam material is coated with a metal film layer to obtain a tablet computer back cover.
[0033] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: the present invention uses three foaming agents: the foaming agent A is OBSH supported by porous silica, and because the porous silica is used as a carrier, the mechanical strength and corrosion resistance of the foaming material can be effectively improved, but it should not be added too much, otherwise it will lead to an increase in density and the foam material will not be light enough; the foaming agent B is a low-boiling-point alkane coated with an organic copolymer, and compared with the foaming agent A, the unit mass is lighter, but the improvement of the mechanical strength is not as good as the foaming agent A, and the two are mixed in a certain proportion to obtain a lightweight and high-strength foaming material;
[0034] The raw materials of the foaming agent C include high-hydrogen silicone oil and modified filler. The modified filler is hollow glass microspheres modified by bismaleimide and allyl glycidyl ether. The hollow glass microspheres themselves help to improve the strength of epoxy resin and reduce its density. The addition of bismaleimide improves the mechanical properties and heat resistance of epoxy resin. The addition of allyl glycidyl ether improves the compatibility of hollow glass microspheres with epoxy resin matrix. The high-hydrogen silicone oil and the modified filler are compounded to further improve the compatibility. The silicone oil can improve the toughness of epoxy resin, thereby improving the compressive strength of epoxy foaming material after foaming. At the same time, the silicon hydrogen group participates in the reaction to generate hydrogen when the epoxy resin is cured, and foaming can be carried out at room temperature.
[0035] The foaming agents A, B and C are mixed in a certain proportion and foamed in three stages: the foaming agent C can foam at room temperature, the foaming agents B and C begin to foam at 65-75°C and 155-160°C respectively. The multi-stage foaming method is used to optimize the shape, size and distribution uniformity of the foam, and finally a lightweight and high-strength epoxy foaming material is obtained. DETAILED DESCRIPTION
[0036] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0037] The following parts are by mass unless otherwise specified;
[0038] Example 1: S1: Take 0.3 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water, stir evenly, stir at 65°C for 4 hours, filter, and dry to obtain modified microspheres; take 10 parts of OBSH DMF solution, add 0.3 parts of modified microspheres, stir at 45°C for 12 hours, filter, wash, and dry to obtain foaming agent A;
[0039] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0040] S3: Take 10 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 3 parts of vinyl silane coupling agent, stir at 55°C for 4h, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; take 12 parts of hollow glass microspheres containing vinyl, 4 parts of bismaleimide, 4 parts of allyl glycidyl ether, and 50 parts of solvent, stir evenly, add 0.02% of the mass of bismaleimide as initiator azobisisobutyronitrile, stir at 85°C for 3h to obtain modified filler; take 18 parts of high hydrogen silicone oil and 3 parts of modified filler, heat to 90°C, add 0.01% of the mass of high hydrogen silicone oil as chloroplatinic acid as catalyst, heat to 160°C for reaction for 6h, heat to 180°C and keep vacuum -0.1MPa for 1h, and distill under reduced pressure to obtain foaming agent C;
[0041] S4: Take 100 parts of epoxy resin, add 12 parts of triethylenetetramine, 8 parts of N-aminoethylpiperazine, 3 parts of foaming agent A, 2 parts of foaming agent B, and 4 parts of foaming agent C, mix well, foam at room temperature for 1.5 hours, heat to 70°C, foam for 1.5 hours; heat to 158°C, foam for 1 hour, and obtain epoxy foaming material.
[0042] Example 2: S1: Take 0.4 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water, stir evenly, stir at 65°C for 4 hours, filter, and dry to obtain modified microspheres; take 12 parts of OBSH DMF solution, add 0.4 parts of modified microspheres, stir at 45°C for 12 hours, filter, wash, and dry to obtain foaming agent A;
[0043] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0044] S3: Take 12 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 3 parts of vinyl silane coupling agent, stir at 55°C for 4h, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; take 15 parts of hollow glass microspheres containing vinyl, 5 parts of bismaleimide, 3 parts of allyl glycidyl ether, and 50 parts of solvent, stir evenly, add 0.02% of the mass of bismaleimide as initiator azobisisobutyronitrile, stir at 85°C for 3h to obtain modified filler; take 20 parts of high hydrogen silicone oil and 3 parts of modified filler, heat to 90°C, add 0.01% of the mass of high hydrogen silicone oil as chloroplatinic acid as catalyst, heat to 160°C for reaction for 6h, heat to 180°C and keep vacuum -0.1MPa for 1h, and distill under reduced pressure to obtain foaming agent C;
[0045] S4: Take 100 parts of epoxy resin, add 15 parts of triethylenetetramine, 5 parts of N-aminoethylpiperazine, 2 parts of foaming agent A, 2 parts of foaming agent B, and 5 parts of foaming agent C, mix well, foam at room temperature for 2 hours, heat to 75°C, foam for 1 hour; heat to 155°C, foam for 1 hour, and obtain epoxy foam material.
[0046] Example 3: S1: Take 0.2 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water, stir evenly, stir at 65°C for 4 hours, filter, and dry to obtain modified microspheres; take 8 parts of OBSH DMF solution, add 0.2 parts of modified microspheres, stir at 45°C for 12 hours, filter, wash, and dry to obtain foaming agent A;
[0047] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0048] S3: Take 8 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 2 parts of vinyl silane coupling agent, stir at 55°C for 4h, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; take 10 parts of hollow glass microspheres containing vinyl, 3 parts of bismaleimide, 3 parts of allyl glycidyl ether, and 50 parts of solvent, stir evenly, add 0.02% of the mass of bismaleimide as initiator azobisisobutyronitrile, stir at 85°C for 3h to obtain modified filler; take 15 parts of high hydrogen silicone oil and 3 parts of modified filler, heat to 90°C, add 0.01% of the mass of high hydrogen silicone oil as chloroplatinic acid as catalyst, heat to 160°C for reaction for 6h, heat to 180°C and keep vacuum -0.1MPa for 1h, and distill under reduced pressure to obtain foaming agent C;
[0049] S4: Take 100 parts of epoxy resin, add 10 parts of triethylenetetramine, 10 parts of N-aminoethylpiperazine, 2 parts of foaming agent A, 3 parts of foaming agent B, and 3 parts of foaming agent C, mix well, foam at room temperature for 1 hour, heat to 75°C, foam for 2 hours; heat to 160°C, foam for 1 hour, and obtain epoxy foam material.
[0050] Comparative Example 1 (the addition amount of the three foaming agents was changed, and the other method steps were consistent with Example 1): S1: 0.3 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water were taken, stirred evenly, stirred at 65° C. for 4 hours, filtered, and dried to obtain modified microspheres; 10 parts of OBSH DMF solution were taken, 0.3 parts of modified microspheres were added, stirred at 45° C. for 12 hours, filtered, washed, and dried to obtain foaming agent A;
[0051] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0052] S3: Take 10 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 3 parts of vinyl silane coupling agent, stir at 55°C for 4h, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; take 12 parts of hollow glass microspheres containing vinyl, 4 parts of bismaleimide, 4 parts of allyl glycidyl ether, and 50 parts of solvent, stir evenly, add 0.02% of the mass of bismaleimide as initiator azobisisobutyronitrile, stir at 85°C for 3h to obtain modified filler; take 18 parts of high hydrogen silicone oil and 3 parts of modified filler, heat to 90°C, add 0.01% of the mass of high hydrogen silicone oil as chloroplatinic acid as catalyst, heat to 160°C for reaction for 6h, heat to 180°C and keep vacuum -0.1MPa for 1h, and distill under reduced pressure to obtain foaming agent C;
[0053] S4: Take 100 parts of epoxy resin, add 12 parts of triethylenetetramine, 8 parts of N-aminoethylpiperazine, 1 part of foaming agent A, 5 parts of foaming agent B, and 2 parts of foaming agent C, mix well, foam at room temperature for 1.5 hours, heat to 70°C, foam for 1.5 hours; heat to 158°C, foam for 1 hour, and obtain epoxy foam material.
[0054] Comparative Example 2 (changing the foaming process, the remaining method steps are consistent with Example 1): S1: Take 0.3 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water, stir evenly, stir at 65°C for 4 hours, filter, and dry to obtain modified microspheres; take 10 parts of OBSH DMF solution, add 0.3 parts of modified microspheres, stir at 45°C for 12 hours, filter, wash, and dry to obtain foaming agent A;
[0055] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0056] S3: Take 10 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 3 parts of vinyl silane coupling agent, stir at 55°C for 4h, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; take 12 parts of hollow glass microspheres containing vinyl, 4 parts of bismaleimide, 4 parts of allyl glycidyl ether, and 50 parts of solvent, stir evenly, add 0.02% of the mass of bismaleimide as initiator azobisisobutyronitrile, stir at 85°C for 3h to obtain modified filler; take 18 parts of high hydrogen silicone oil and 3 parts of modified filler, heat to 90°C, add 0.01% of the mass of high hydrogen silicone oil as chloroplatinic acid as catalyst, heat to 160°C for reaction for 6h, heat to 180°C and keep vacuum -0.1MPa for 1h, and distill under reduced pressure to obtain foaming agent C;
[0057] S4: Take 100 parts of epoxy resin, add 12 parts of triethylenetetramine, 8 parts of N-aminoethylpiperazine, 3 parts of foaming agent A, 2 parts of foaming agent B, and 4 parts of foaming agent C, mix well, heat to 158°C, and foam for 4 hours to obtain epoxy foaming material.
[0058] Comparative Example 3 (modified filler and high hydrogen silicone oil are added directly, and the remaining steps are consistent with Example 1): S1: Take 0.3 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water, stir evenly, stir at 65° C. for 4 hours, filter, and dry to obtain modified microspheres; take 10 parts of OBSH DMF solution, add 0.3 parts of modified microspheres, stir at 45° C. for 12 hours, filter, wash, and dry to obtain foaming agent A;
[0059] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0060] S3: Take 10 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 3 parts of vinyl silane coupling agent, stir at 55°C for 4 hours, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; take 12 parts of hollow glass microspheres containing vinyl, 4 parts of bismaleimide, 4 parts of allyl glycidyl ether, and 50 parts of solvent, stir evenly, add 0.02% of the mass of bismaleimide as initiator azobisisobutyronitrile, stir at 85°C for 3 hours to obtain modified filler;
[0061] Take high hydrogen content silicone oil and name it as foaming agent C;
[0062] S4: Take 100 parts of epoxy resin, add 12 parts of triethylenetetramine, 8 parts of N-aminoethylpiperazine, 3 parts of foaming agent A, 2 parts of foaming agent B, 4 parts of foaming agent C, and 0.7 parts of modified filler, mix well, foam at room temperature for 1.5 hours, heat to 70°C, foam for 1.5 hours; heat to 158°C, foam for 1 hour, and obtain epoxy foam material.
[0063] Comparative Example 4 (the preparation method of the modified filler was changed, and the other method steps were consistent with Example 1): S1: 0.3 parts of porous silica, 2 parts of ethanol, 1 part of KH550, and 1 part of water were taken, stirred evenly, stirred at 65° C. for 4 hours, filtered, and dried to obtain modified microspheres; 10 parts of OBSH DMF solution were taken, 0.3 parts of modified microspheres were added, stirred at 45° C. for 12 hours, filtered, washed, and dried to obtain foaming agent A;
[0064] S2: low boiling point alkane is coated with an organic copolymer to prepare a foaming agent B;
[0065] S3: Take 10 parts of hollow glass microspheres, add 80 parts of ethanol, 80 parts of water, and 3 parts of vinyl silane coupling agent, stir at 55°C for 4 hours, filter, wash, and dry to obtain a modified filler; take 18 parts of high hydrogen silicone oil and 3 parts of modified filler, heat to 90°C, add 0.01% chloroplatinic acid by mass of high hydrogen silicone oil as a catalyst, heat to 160°C and react for 6 hours, heat to 180°C and keep vacuum -0.1MPa for 1 hour, and distill under reduced pressure to obtain a foaming agent C;
[0066] S4: Take 100 parts of epoxy resin, add 12 parts of triethylenetetramine, 8 parts of N-aminoethylpiperazine, 3 parts of foaming agent A, 2 parts of foaming agent B, and 4 parts of foaming agent C, mix well, foam at room temperature for 1.5 hours, heat to 70°C, foam for 1.5 hours; heat to 158°C, foam for 1 hour, and obtain epoxy foaming material.
[0067] In the above embodiments, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: epoxy resin (E51, Gadal); ethanol (CAS: 64-17-5); porous silica (AM-SiO2-K-01, Yamei Nano); KH550 (CAS: 919-30-2); OBSH (CAS: 80-51-3); DMF (CAS: 68-12-2); polyvinyl pyrrolidone (S30268, Shanghai Yuanye); sodium dodecyl sulfate (S15012, Shanghai Yuanye); azobisisobutyronitrile (CAS: 78-67-1); isopentane (CAS: 78-78-4); trimethylolpropane trimethacrylate (CAS: 3290-92-4); sodium hydroxymethylcellulose (CAS: 9085-26-1); acrylonitrile (CAS: 10 7-13-1); ethylene glycol dimethacrylate (CAS: 97-90-5); methyl methacrylate (CAS: 80-62-6); hydroxypropyl acrylate (CAS: 25584-83-2); magnesium chloride (S50664, Shanghai Yuanye); sodium malate (S11103, Shanghai Yuanye); ammonia (25%, Sigma-Aldrich); hollow glass microspheres (HN20, Shanxi Hainuo Technology Co., Ltd.); vinyl Silane coupling agent (CAS: 2768-02-7); bismaleimide (CAS: 35325-39-4); allyl glycidyl ether (CAS: 106-92-3); high hydrogen silicone oil (IOTA202, Anhui IOTA Silicone Oil Co., Ltd.); chloroplatinic acid (CAS: 16941-12-1); triethylenetetramine (CAS: 112-24-3); N-aminoethylpiperazine (CAS: 140-31-8).
[0068] Experiment: Take the epoxy foam materials prepared in Examples 1 to 3 and Comparative Examples 1 to 4; (1) refer to GB / T 6343-1995 to measure the apparent density; (2) refer to GB / T 8813-2008 to measure the compressive strength; see the table below for specific data;
[0069]
[0070] Conclusion: In comparative example 1, by changing the addition amount of the three foaming agents, the density of the epoxy foam material increased and the compression strength decreased, from which it can be seen that the addition amount of the three foaming agents needs to be controlled; in comparative example 2, the foaming process was changed, and the stepped multi-stage foaming was not used, which also led to a decrease in performance. From this, it can be seen that the three foaming agents used in the present invention cooperate with the three-stage foaming process to obtain a lightweight epoxy foam material with the best performance; in comparative example 3, the modified filler and the high hydrogen silicone oil were directly added, and the performance decreased due to compatibility problems; in comparative example 4, the preparation method of the modified filler was changed, and bismaleimide and allyl glycidyl ether were not added, and the performance was not as good as the embodiment; in summary, the epoxy foam material prepared by the present invention has the advantages of light weight and high strength, and is suitable for preparing the back cover of a tablet computer.
[0071] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A lightweight and high-strength epoxy foam material, characterized in that: The epoxy foaming material comprises the following raw materials, calculated by weight: 100 parts of epoxy resin, 15-25 parts of curing agent, 2-3 parts of foaming agent A, 2-3 parts of foaming agent B, and 3-5 parts of foaming agent C; The foaming agent A is obtained by loading 4,4'-oxybisbenzenesulfonyl hydrazide on porous silica; the foaming agent B is obtained by coating low-boiling-point alkane with an organic copolymer; and the foaming agent C includes hollow glass microspheres.
2. A lightweight and high-strength epoxy foam material according to claim 1, characterized in that: The preparation of the foaming agent A comprises the following steps: Step 1: Take porous silica, ethanol, aminosilane coupling agent and water, stir evenly, stir at 60-70°C for 3-5h, filter and dry to obtain modified microspheres; Step 2: Take a solution of 4,4'-oxybisbenzenesulfonyl hydrazide in N,N-dimethylformamide, add the modified microspheres, stir at 40-50°C for 10-12h, filter, wash, and dry to obtain a foaming agent A.
3. A lightweight and high-strength epoxy foam material according to claim 2, characterized in that: The modified microspheres include the following raw materials, calculated by weight: 0.2-0.4 parts of porous silica, 1-2 parts of ethanol, 0.8-1.2 parts of aminosilane coupling agent, and 1-2 parts of water; The foaming agent A comprises the following raw materials, calculated by mass: 8-12 parts of 4,4'-oxybisbenzenesulfonylhydrazine N,N-dimethylformamide solution, 0.2-0.4 parts of modified microspheres; the concentration of the 4,4'-oxybisbenzenesulfonylhydrazine N,N-dimethylformamide solution is 1-2 mol / L.
4. The lightweight and high-strength epoxy foam material according to claim 1, characterized in that: The preparation of the foaming agent B comprises the following steps: Step 1: adding sodium malate to the magnesium chloride ethanol solution, stirring, slowly dropping ammonia water for precipitation, aging, washing, drying, and dispersing with water to obtain a nano magnesium hydroxide suspension; adding the nano magnesium hydroxide suspension, polyvinyl pyrrolidone, and sodium dodecyl sulfate into water, heating and stirring to obtain an aqueous phase; Step 2: uniformly mix the polymer monomer, azobisisobutyronitrile, low boiling point alkane and trimethylolpropane trimethacrylate, and perform ultrasonic treatment to obtain an oil phase; Step 3: Evenly mix the oil phase and the water phase, add epoxy resin and sodium hydroxymethyl cellulose, mix and emulsify to obtain a suspension; introduce nitrogen to pressurize, slowly heat to 42-45°C and keep warm for 25-30 minutes, keep warm at 48-52°C for 23-24 hours, heat to 56-60°C and keep warm for 4-5 hours, cool, wash, and dry to obtain a foaming agent B; The polymer monomers include one or more of acrylonitrile, ethylene glycol dimethacrylate, methyl methacrylate, and hydroxypropyl acrylate; and the low-boiling-point alkane is isopentane.
5. The lightweight and high-strength epoxy foam material according to claim 1, characterized in that: The preparation of the foaming agent C comprises the following steps: taking high hydrogen silicone oil and modified filler, heating, adding chloroplatinic acid as a catalyst, heating to 155-160° C. and reacting for 6-7 hours, heating to 175-180° C. and maintaining vacuum for 1-2 hours, and distilling under reduced pressure to obtain the foaming agent C.
6. A lightweight and high-strength epoxy foam material according to claim 5, characterized in that: The foaming agent C comprises the following raw materials, calculated by weight: 15 to 20 parts of high hydrogen-containing silicone oil, 2 to 3 parts of modified filler, and 0.01% of chloroplatinic acid by weight of the high hydrogen-containing silicone oil.
7. The lightweight and high-strength epoxy foam material according to claim 5, characterized in that: The preparation of the modified filler comprises the following steps: Step 1: Take hollow glass microspheres, add ethanol, water, and vinyl silane coupling agent, stir at 50-60°C for 3-4 hours, filter, wash, and dry to obtain hollow glass microspheres containing vinyl; Step 2: Take hollow glass microspheres containing vinyl, bismaleimide, allyl glycidyl ether, initiator azobisisobutyronitrile, and solvent, stir evenly, and stir at 75-85° C. for 2-3 hours to obtain a modified filler.
8. The lightweight and high-strength epoxy foam material according to claim 7, characterized in that: The hollow glass microspheres containing vinyl groups include the following raw materials, calculated by weight: 8 to 12 parts of hollow glass microspheres, 60 to 80 parts of ethanol, 60 to 80 parts of water, and 2 to 3 parts of vinyl silane coupling agents; The modified filler comprises the following raw materials, calculated by weight: 10-15 parts of hollow glass microspheres containing vinyl, 3-5 parts of bismaleimide, 3-5 parts of allyl glycidyl ether, 30-50 parts of solvent, and an initiator with a weight percentage of 0.02-0.03% of bismaleimide.
9. The method for preparing a lightweight and high-strength epoxy foam material according to any one of claims 1 to 8, characterized in that: The following steps are involved: Take epoxy resin, curing agent, foaming agent A, foaming agent B, and foaming agent C, mix them evenly, inject them into the mold, foam them at room temperature for 1 to 2 hours, heat them to 65 to 75°C, foam them for 1 to 2 hours; heat them to 155 to 160°C, foam them for 1 to 2 hours, and obtain epoxy foaming material.
10. A method for preparing a tablet computer back cover, characterized in that: The following steps are involved: The surface of the epoxy foam material prepared in claim 9 is plated with a metal film layer to obtain a tablet computer back cover.
Citation Information
Patent Citations
Light-high-strength epoxy foam material and preparation method thereof
CN101319085A
A conductive composition for low frequency EMI shielding
CN108476604A
Environment-friendly special heavy-duty anti-corrosion finishing coat and preparation method thereof
CN109401549A
Flame-retardant epoxy resin foam material as well as preparation method and application thereof
CN113045862A
Thermal expansion type foaming microsphere and preparation method thereof
CN114369281A