Epoxy resin for motor encapsulation and preparation method thereof
By modifying the epoxy resin composite system combining boron nitride nanosheets and allylcholestyrene liquid crystal monomers, the problem of poor thermal conductivity of traditional epoxy resins is solved, and good thermal conductivity and mechanics of motor potting materials are achieved. Performance improves the thermal stability and toughness of the motor.
Patent Information
- Application Number
- CN202411315429.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional epoxy resins have poor thermal conductivity in motor potting, making it difficult to have both good thermal conductivity and mechanical properties, which affects the motor's heat dissipation ability and working efficiency.
The modified boron nitride nanosheets were prepared by using bisphenol A type epoxy resin and E-39D epoxy resin composite system, and enhanced by modified boron nitride nanosheets through Michael addition reaction and liquid phase ultrasonic peeling technology. Combining allylcholestyrene liquid crystal monomers, a three-dimensional thermal conductivity network is formed to improve thermal conductivity and mechanical properties.
It significantly improves the thermal conductivity and mechanical properties of composite materials, improves the thermal stability and toughness of the motor, and effectively protects the performance of the motor during operation.
Smart Images

Figure BDA0005052053410000091
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of epoxy resins, and in particular relates to an epoxy resin for motor potting and a preparation method thereof. Background Art
[0002] New energy vehicles are more energy-efficient and environmentally friendly, so they have become the main popular trend at present. As the power executor of new energy vehicles, motors are related to the safe driving and riding quality of the car. However, due to their small installation space and harsh operating environment, in order to ensure their stable operation, they need to be encapsulated with epoxy resin potting glue to enhance the overall resistance of the motor.
[0003] As motor equipment develops towards large capacity, high power density, and small and lightweight, the heat generated per unit volume during operation and working increases significantly. The continuous accumulation of heat and the resulting rapid temperature rise will accelerate the aging and failure of dielectric materials, greatly reducing the working efficiency and reliability of the equipment. However, the traditional epoxy resin has poor bulk thermal conductivity, which seriously restricts its heat dissipation capacity in electrical equipment. Generally, the thermal conductivity of epoxy resin is improved by introducing thermal conductive fillers (such as Al2O3, Si3N4, Al N, BN, etc.). However, relevant studies have shown that when the thermal conductivity absorption of the filler is greater than 100 times the thermal conductivity of the matrix, even if the filler content is high, the increase in the filler has little effect on improving the thermal absorption of the composite material. In addition, the introduction of too much thermal conductive filler will also affect the mechanical properties of the epoxy resin potting compound. Therefore, seeking an epoxy resin for motor potting with good thermal conductivity and mechanical properties is a technical problem that needs to be solved at present. Summary of the invention
[0004] The object of the present invention is to provide an epoxy resin for motor potting and a preparation method thereof, so as to solve the problem that the existing epoxy resin is difficult to have both good thermal conductivity and mechanical properties.
[0005] The purpose of the present invention can be achieved through the following technical solutions:
[0006] An epoxy resin for motor potting, comprising component A and component B, wherein the mass ratio of component A to component B is 1:1, and the component A comprises the following components in parts by weight: 100 parts of bisphenol A epoxy resin, 25 parts of E-39D epoxy resin, 20-30 parts of active diluent, and 18.75-37.5 parts of modified boron nitride nanosheets;
[0007] The B component includes the following components: 25-35 parts of a curing agent and 1 part of an accelerator.
[0008] Further, the modified boron nitride nanosheets are prepared by the following steps:
[0009] Aminated boron nitride nanosheets are ultrasonically dispersed in toluene, and then allyl cholesteric liquid crystal monomers are added, reacted at 60-100° C. for 8-10 hours, cooled to room temperature, filtered, and the filter cake is washed with anhydrous ethanol for 3-5 times and then dried to obtain modified boron nitride nanosheets.
[0010] Aminated boron nitride nanosheets and allyl cholesteric liquid crystal monomers are used as raw materials, and the aminated boron nitride nanosheets and allyl cholesteric liquid crystal monomers are chemically bonded through Michael addition reaction to obtain modified boron nitride nanosheets.
[0011] Furthermore, the usage ratio of the amino boron nitride nanosheets, toluene and allyl cholesteric liquid crystal monomer is 3.5-4.8 g: 50-100 mL: 0.5-1.2 g.
[0012] Further, the amination boron nitride nanosheets are prepared by the following steps:
[0013] The branched polyethyleneimine and deionized water were stirred and mixed for 0.5 h, hexagonal boron nitride powder was added, and stirring was continued for 0.5 h. Then, ultrasonic treatment was performed for 1.5 h and mechanical stirring was performed for 0.5 h. The steps of ultrasonic treatment for 1.5 h and mechanical stirring for 0.5 h were repeated 5 times. The mixture was centrifuged at a speed of 1500 r / min for 10 min, and the supernatant was retained. The supernatant was centrifuged at 10000 r / min for 20 min. The obtained precipitate was washed three times with deionized water, and finally dried at 60°C for 48 h to obtain amino boron nitride nanosheets.
[0014] The hexagonal boron nitride powder is subjected to liquid phase ultrasonic exfoliation using a branched polyethyleneimine aqueous solution, so that the hexagonal boron nitride powder becomes hexagonal boron nitride nanosheets with fewer layers, and part of the amino groups of the branched polyethyleneimine are combined with the hydroxyl groups on the surface of the hexagonal boron nitride through hydrogen bonds, thereby increasing the surface activity of the hexagonal boron nitride nanosheets.
[0015] Furthermore, the usage ratio of branched polyethyleneimine, deionized water and hexagonal boron nitride powder is 8g:392mL:1.6g, the stirring speed is 50-200r / min, and the ultrasonic power is 200-300W.
[0016] Furthermore, the particle size of the hexagonal boron nitride powder is 1-2 um, and the molecular weight of the branched polyethyleneimine is 1800-25000.
[0017] Further, the allyl cholesteric liquid crystal monomer is prepared by the following steps:
[0018] Dissolve 4-allyloxybenzoyl chloride in chloroform to obtain a mixed solution a, add cholesterol, pyridine and chloroform into a flask, stir for 5-10 minutes, add the mixed solution a dropwise into the flask, and after the addition is complete, stir and react at 50°C for 12 hours. After the reaction is complete, filter, add the filter cake into anhydrous ethanol for recrystallization, and obtain an allyl cholesteric liquid crystal monomer.
[0019] Furthermore, the usage ratio of 4-allyloxybenzoyl chloride, cholesterol and pyridine is 0.1 mol:0.1 mol:8 mL.
[0020] Furthermore, the bisphenol A epoxy resin is bisphenol A epoxy resin E-51.
[0021] Furthermore, the active diluent is trimethylolpropane triglycidyl ether.
[0022] Furthermore, the curing agent is any one or more of methyltetrahydrophthalic anhydride, diethylenetriamine and maleic anhydride.
[0023] Furthermore, the accelerator is any one or more of 2,4,6-tris(dimethylaminomethyl)phenol, dimethylacrylamide, and triethylamine.
[0024] The preparation method of the above-mentioned epoxy resin for motor potting comprises the following steps:
[0025] (2) adding bisphenol A epoxy resin, E-39D epoxy resin and active diluent into a stirring kettle, stirring and dispersing at a temperature of 40-50° C. and a speed of 800-1200 r / min for 15-20 min, adding modified boron nitride nanosheets, continuing to stir for 45-60 min, and then degassing at a vacuum degree of -0.098 to -0.1 MPa for 2-3 h to obtain component A;
[0026] (2) Add the curing agent and accelerator into a stirring tank, stir and disperse at a speed of 800-1200 r / min for 15-20 min to obtain component B.
[0027] Beneficial effects of the present invention:
[0028] The present invention provides an epoxy resin for motor potting, wherein the main resin is a compound system of bisphenol A epoxy resin E-51 and E-39D epoxy resin, wherein the bisphenol A epoxy resin E-51 has excellent adhesion and chemical resistance, and the epoxy resin E-39D has low viscosity, which is conducive to potting and defoaming. After compounding, the ultraviolet radiation resistance of the potting material can be guaranteed, and the requirement of chemical corrosion resistance can be met;
[0029] Component A contains self-made modified boron nitride nanosheets, which are allyl cholesteric liquid crystal monomers grafted with amino boron nitride nanosheets. They not only have good dispersibility in the epoxy resin matrix, but also have good interface compatibility with the epoxy resin. The introduction of cholesteric liquid crystal monomers also promotes the orderly and uniform distribution of amino boron nitride nanosheets in the epoxy resin group, forming a three-dimensional thermal conductive network in the epoxy resin matrix, which significantly improves the thermal conductivity of the composite material.
[0030] The good interfacial bonding between the modified boron nitride nanosheets and the epoxy resin restricts the movement of the epoxy resin chain segments, thereby increasing the glass transition temperature (Tg) of the composite material and improving the thermal stability of the composite material;
[0031] When the composite material is subjected to external force, the modified boron nitride nanosheets can also effectively absorb the crack damage energy, prevent the further expansion of the crack, and improve the mechanical properties of the composite material. Compared with the existing amino-modified boron nitride nanosheets, the introduction of branched polyethyleneimine not only improves the dispersibility of the boron nitride nanosheets, but also effectively improves the toughness of the composite material due to the introduction of the branched structure. The introduction of cholesteric liquid crystal monomers further improves the mechanical properties and heat resistance of the composite material.
[0032] In summary, the epoxy resin for motor potting prepared by the present invention has good thermal conductivity and mechanical properties, can play a good protective role when the motor is running, and has high application value. DETAILED DESCRIPTION
[0033] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0034] Bisphenol A epoxy resin E-51, industrial grade, epoxy value 0.51-0.52, Jiangsu Sanmu Chemical Co., Ltd.;
[0035] Branched polyethyleneimine (PE I, 99%, Mw 25000, purchased from Shanghai Yien Chemical Technology Co., Ltd.).
[0036] Example 1
[0037] Modified boron nitride nanosheets are prepared by the following steps:
[0038] 3.5 g of amino-modified boron nitride nanosheets were ultrasonically dispersed in 50 mL of toluene, and then 0.5 g of allyl cholesteric liquid crystal monomer was added, reacted at 60° C. for 8 h, cooled to room temperature, filtered, and the filter cake was washed three times with anhydrous ethanol and dried to obtain modified boron nitride nanosheets.
[0039] Aminated boron nitride nanosheets were prepared by the following steps:
[0040] 8 g of branched polyethyleneimine particles (1-2 um) and 392 mL of deionized water were stirred and mixed for 0.5 h, 1.6 g of hexagonal boron nitride powder was added, and the mixture was stirred at 50 r / min for 0.5 h. Then, ultrasonic treatment was performed at a power of 200 W for 1.5 h and mechanical stirring was performed for 0.5 h. The ultrasonic treatment was repeated for 1.5 h and mechanical stirring was performed for 0.5 h for 5 times. The mixture was centrifuged at a speed of 1500 r / min for 10 min, and the supernatant was retained. The supernatant was centrifuged at 10000 r / min for 20 min. The obtained precipitate was washed three times with deionized water, and finally dried at 60°C for 48 h to obtain amino boron nitride nanosheets.
[0041] Allyl cholesteric liquid crystal monomers are prepared by the following steps:
[0042] Dissolve 0.1 mol 4-allyloxybenzoyl chloride in 100 mL chloroform to obtain a mixed solution a, add 0.1 mol cholesterol, 8 mL pyridine and 150 mL chloroform into a flask, stir for 5 min, add the mixed solution a dropwise into the flask, after the addition is complete, stir and react at 50°C for 12 h, after the reaction is complete, filter, add the filter cake into anhydrous ethanol for recrystallization, and obtain an allyl cholesteric liquid crystal monomer.
[0043] Example 2
[0044] Modified boron nitride nanosheets are prepared by the following steps:
[0045] 4.8 g of amino-modified boron nitride nanosheets were ultrasonically dispersed in 100 mL of toluene, and then 1.2 g of allyl cholesteric liquid crystal monomer was added, reacted at 100° C. for 10 h, cooled to room temperature, filtered, and the filter cake was washed 5 times with anhydrous ethanol and dried to obtain modified boron nitride nanosheets.
[0046] Aminated boron nitride nanosheets were prepared by the following steps:
[0047] 8 g of branched polyethyleneimine particles (1-2 um) and 392 mL of deionized water were stirred and mixed for 0.5 h, 1.6 g of hexagonal boron nitride powder was added, and the mixture was stirred at 200 r / min for 0.5 h. Then, ultrasonic treatment was performed at a power of 300 W for 1.5 h and mechanical stirring was performed for 0.5 h. The ultrasonic treatment was repeated for 1.5 h and mechanical stirring was performed for 0.5 h for 5 times. The mixture was centrifuged at a speed of 1500 r / min for 10 min, and the supernatant was retained. The supernatant was centrifuged at 10000 r / min for 20 min. The obtained precipitate was washed three times with deionized water, and finally dried at 60°C for 48 h to obtain amino boron nitride nanosheets.
[0048] Allyl cholesteric liquid crystal monomers are prepared by the following steps:
[0049] Dissolve 0.1 mol 4-allyloxybenzoyl chloride in 100 mL chloroform to obtain a mixed solution a, add 0.1 mol cholesterol, 8 mL pyridine and 150 mL chloroform into a flask, stir for 10 min, add the mixed solution a dropwise into the flask, after the addition is complete, stir and react at 50°C for 12 h, after the reaction is complete, filter, add the filter cake into anhydrous ethanol for recrystallization, and obtain an allyl cholesteric liquid crystal monomer.
[0050] Comparative Example 1
[0051] Modified boron nitride nanosheets are prepared by the following steps:
[0052] Aminated boron nitride nanosheets and allyl cholesteric liquid crystal monomers were added into a stirring tank at a mass ratio of 3.5:0.5, and stirred and mixed at 200 r / min for 20 minutes to obtain modified boron nitride nanosheets. The preparation process of aminated boron nitride nanosheets and allyl cholesteric liquid crystal monomers was the same as that in Example 1.
[0053] Comparative Example 2
[0054] Modified boron nitride nanosheets are prepared by the following steps:
[0055] 8 g of branched polyethyleneimine particles (1-2 um) and 392 mL of deionized water were stirred and mixed for 0.5 h, 1.6 g of hexagonal boron nitride powder was added, and the mixture was stirred at 200 r / min for 0.5 h. Then, ultrasonic treatment was performed at a power of 300 W for 1.5 h and mechanical stirring was performed for 0.5 h. The ultrasonic treatment was repeated for 1.5 h and mechanical stirring was performed for 0.5 h for 5 times. The mixture was centrifuged at a speed of 1500 r / min for 10 min, and the supernatant was retained. The supernatant was centrifuged at 10000 r / min for 20 min. The obtained precipitate was washed three times with deionized water, and finally dried at 60°C for 48 h to obtain modified boron nitride nanosheets.
[0056] Comparative Example 3
[0057] This comparative example provides surface-modified h-BN nanosheets (BN-NH2 particle size is about 500 nm) with amino groups as terminal groups, with a purity of 99.0%, purchased from Beijing Deke Shimadzu Co., Ltd.
[0058] Example 3
[0059] An epoxy resin for motor potting, comprising component A and component B, wherein the mass ratio of component A to component B is 1:1, and the component A comprises the following components in parts by weight: 1100 parts of bisphenol A epoxy resin E-51, 25 parts of E-39D epoxy resin, 20 parts of trimethylolpropane triglycidyl ether, and 18.75 parts of modified boron nitride nanosheets of Example 1;
[0060] The B component includes the following components: 25 parts of maleic anhydride and 1 part of accelerator.
[0061] The preparation method of the above-mentioned epoxy resin for motor potting comprises the following steps:
[0062] (1) adding bisphenol A epoxy resin E-51 and trimethylolpropane triglycidyl ether into a stirring kettle, stirring and dispersing at a temperature of 40° C. and a speed of 800 r / min for 15 min, adding modified boron nitride nanosheets, continuing to stir for 45 min, and then degassing at a vacuum degree of -0.098 MPa for 2 h to obtain component A;
[0063] (2) Add maleic anhydride and dimethylacrylamide into a stirring tank and stir and disperse them at a speed of 800 r / min for 15 minutes to obtain component B.
[0064] Example 4
[0065] An epoxy resin for motor potting, comprising component A and component B, wherein the mass ratio of component A to component B is 1:1, and the component A comprises the following components in parts by weight: 1100 parts of bisphenol A epoxy resin E-51, 25 parts of E-39D epoxy resin, 20-30 parts of trimethylolpropane triglycidyl ether, and 28.75 parts of modified boron nitride nanosheets of Example 2;
[0066] The B component includes the following components: 30 parts of methyltetrahydrophthalic anhydride and 1 part of 2,4,6-tris(dimethylaminomethyl)phenol.
[0067] The preparation method of the above-mentioned epoxy resin for motor potting comprises the following steps:
[0068] (1) adding polypropylene glycol diglycidyl ether, bisphenol A epoxy resin E-51 and trimethylolpropane triglycidyl ether into a stirring kettle, stirring and dispersing for 18 min at a temperature of 45° C. and a speed of 1000 r / min, adding modified boron nitride nanosheets, continuing to stir for 52 min, and then degassing for 2.5 h at a vacuum degree of -0.1 MPa to obtain component A;
[0069] (2) Methyltetrahydrophthalic anhydride and 2,4,6-tris(dimethylaminomethyl)phenol were added into a stirring tank and stirred and dispersed at a speed of 1000 r / min for 18 min to obtain component B.
[0070] Example 5
[0071] An epoxy resin for motor potting, comprising component A and component B, wherein the mass ratio of component A to component B is 1:1, and the component A comprises the following components in parts by weight: 1100 parts of bisphenol A epoxy resin E-51, 25 parts of E-39D epoxy resin, 30 parts of trimethylolpropane triglycidyl ether, and 37.5 parts of modified boron nitride nanosheets of Example 2;
[0072] The B component includes the following components: 35 parts of methyltetrahydrophthalic anhydride and 1 part of 2,4,6-tris(dimethylaminomethyl)phenol.
[0073] The preparation method of the above-mentioned epoxy resin for motor potting comprises the following steps:
[0074] (1) adding bisphenol A epoxy resin, E-39D epoxy resin and active diluent into a stirring kettle, stirring and dispersing at a temperature of 50° C. and a speed of 1200 r / min for 20 min, adding modified boron nitride nanosheets, continuing to stir for 60 min, and then degassing at a vacuum degree of -0.1 MPa for 3 h to obtain component A;
[0075] (2) Add methyltetrahydrophthalic anhydride and 2,4,6-tris(dimethylaminomethyl)phenol into a stirring tank, stir and disperse at a speed of 1200 r / min for 20 min to obtain component B.
[0076] Comparative Example 4
[0077] An epoxy resin for motor potting is prepared based on Example 3, wherein the modified boron nitride nanosheets in Example 3 are replaced by the material prepared in Comparative Example 1, and the remaining raw materials, parameters and steps are the same as those in Example 3.
[0078] Comparative Example 5
[0079] An epoxy resin for motor potting is prepared in Example 3, wherein the modified boron nitride nanosheets in Example 3 are replaced by the material prepared in Comparative Example 2, and the remaining raw materials, parameters and steps are the same as those in Example 3.
[0080] Comparative Example 6
[0081] An epoxy resin for motor potting is provided. Based on Example 3, the modified boron nitride nanosheets in Example 3 are replaced by the material in Comparative Example 3, and the remaining raw materials, parameters and steps are the same as those in Example 3.
[0082] Component A and component B of the epoxy resin for motor potting prepared in Examples 3 to 5 and Comparative Examples 4 to 6 were added to a mixing barrel, stirred at 500 r / min for 30 min, vacuum degree -0.1 MPa, temperature 60°C, deaerated for 15 min, then cast in a polytetrafluoroethylene mold, pre-cured at 80°C for 2 h, cured at 120°C for 4 h, and cured at 160°C for 4 h, and performance tested:
[0083] 1. The thermal conductivity of composite materials of different components was measured using a laser flash thermal conductivity analyzer (NETZSCH, LFA467). The test sample size was 10 mm × 10 mm × 1 mm.
[0084] 2. Test the glass transition temperature of the material according to GB / T 22567-2008;
[0085] 3. Test the tensile strength and bending strength of the material according to GB / T 2567-2008;
[0086] The results are shown in Table 1:
[0087] Table 1
[0088]
[0089] It can be seen from Table 1 that, compared with Comparative Examples 4-6, the epoxy resin for motor potting obtained in Examples 3-5 has both good thermal conductivity and mechanical properties, can play a good protective role when the motor is running, and has a high application value.
[0090] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.
[0091] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. An epoxy resin for motor potting, comprising component A and component B, characterized in that: The mass ratio of component A to component B is 1:
1. Component A comprises the following components in parts by weight: 100 parts of bisphenol A epoxy resin, 25 parts of E-39D epoxy resin, 20-30 parts of reactive diluent, and 18.75-37.5 parts of modified boron nitride nanosheets; The B component includes the following components: 25-35 parts of curing agent and 1 part of accelerator.
2. The epoxy resin for motor potting according to claim 1, characterized in that: Modified boron nitride nanosheets are prepared by the following steps: Aminated boron nitride nanosheets are ultrasonically dispersed in toluene, and then allyl cholesteric liquid crystal monomers are added. The mixture is reacted at 60-100° C. for 8-10 hours, cooled to room temperature, filtered, and the filter cake is washed with anhydrous ethanol for 3-5 times and then dried to obtain modified boron nitride nanosheets.
3. The epoxy resin for motor potting according to claim 2, characterized in that: The usage ratio of the amino-bonded boron nitride nanosheets, toluene and allyl cholesteric liquid crystal monomer is 3.5-4.8 g: 50-100 mL: 0.5-1.2 g.
4. The epoxy resin for motor potting according to claim 2, characterized in that: Amination-modified boron nitride nanosheets are prepared by the following steps: The branched polyethyleneimine and deionized water were stirred and mixed for 0.5 h, hexagonal boron nitride powder was added, and stirring was continued for 0.5 h. After ultrasonic treatment for 1.5 h, mechanical stirring was performed for 0.5 h. The ultrasonic treatment for 1.5 h and mechanical stirring for 0.5 h were repeated 5 times. The mixture was centrifuged at a speed of 1500 r / min for 10 min, and the supernatant was retained. The supernatant was centrifuged at 10000 r / min for 20 min. The obtained precipitate was washed three times with deionized water and finally dried at 60°C for 48 h to obtain amino boron nitride nanosheets.
5. The epoxy resin for motor potting according to claim 4, characterized in that: The usage ratio of branched polyethyleneimine, deionized water and hexagonal boron nitride powder is 8 g:392 mL:1.6 g.
6. The epoxy resin for motor potting according to claim 2, characterized in that: Allyl cholesteric liquid crystal monomers are prepared by the following steps: 4-Allyloxybenzoyl chloride was dissolved in chloroform to obtain a mixture a. Cholesterol, pyridine and chloroform were added to a flask and stirred for 5-10 minutes. The mixture a was added dropwise to the flask. After the addition was completed, the mixture was stirred at 50°C for 12 hours. After the reaction was completed, the mixture was filtered and the filter cake was added to anhydrous ethanol for recrystallization to obtain an allyl cholesteric liquid crystal monomer.
7. The epoxy resin for motor potting according to claim 6, characterized in that: The usage ratio of 4-allyloxybenzoyl chloride, cholesterol and pyridine is 0.1 mol:0.1 mol:8 mL.
8. A method for preparing the epoxy resin for motor potting according to any one of claims 1 to 7, characterized in that: The following steps are involved: (1) Add bisphenol A epoxy resin, E-39D epoxy resin and reactive diluent into a stirred tank, stir and disperse at a temperature of 40-50°C and a speed of 800-1200 r / min for 15-20 minutes, add modified boron nitride nanosheets, continue stirring for 45-60 minutes, and then degas at a vacuum degree of -0.098 to -0.1 MPa for 2-3 hours to obtain component A; (2) Add the curing agent and accelerator into a stirring tank, stir and disperse at a speed of 800-1200 r / min for 15-20 minutes to obtain component B.
Citation Information
Cited By
High-flexibility energy storage cable and preparation method thereof
CN119286077A