Seedling raising cup capable of being used for household compost degradation
The seedling cup prepared by using polylactic acid, polyhydroxy fatty acid ester and other materials has solved the problem of poor damage and degradation of seedling roots, achieved degradation and release of nutrients under home composting conditions, and promoted plants Grow healthy.
Patent Information
- Application Number
- CN202411272635.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-05-17
- Filing Date
- 2024-09-11
- Publication Date
- 2024-11-19
AI Technical Summary
Existing seedling cup materials (such as PVC/PET/PS) are susceptible to injury when the seedling roots are removed and cannot provide effective nutrition and moisture absorption and breathability, resulting in root rot and difficult to degrade.
A household fertilization can be prepared by ultrasonic mixing, acid chloride reaction, melt plasticization and blister forming processes using polylactic acid, polyhydroxy fatty acid ester, modified diatomaceous earth, ZIF-8-OH, lignin and other materials. The degraded seedling cup has good degradability and mechanical properties.
The degradation time of the seedling cup in the home composting conditions is 6 to 15 months, providing suitable structural support and moisture regulation, promoting healthy growth of plant roots, and releasing nutrients during the degradation process, improving soil permeability and water retention. .
Smart Images

Figure BDA0005039153050000061 
Figure BDA0005039153050000071 
Figure BDA0005039153050000072
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of seedling cup degradation, in particular to a seedling cup that can be degraded by household composting. Background Art
[0002] Currently, most seedling cups are made of PVC / PET / PS as the base material. After the seedlings are grown, they need to be taken out of the seedling cups and recycled for continued use. However, the roots of the seedlings are easily injured during the removal process, which is not conducive to the growth of the seedlings. In addition, PVC / PET / PS seedling cups cannot provide nutrients to the seedlings during their growth stage, have poor moisture absorption and air permeability, and are prone to cause root rot of the seedlings. They are also difficult to degrade.
[0003] In summary, in order to solve the above problems, it is of great significance to prepare a seedling cup that can be degraded by household composting. Summary of the invention
[0004] The object of the present invention is to provide a seedling raising cup which can be degraded by household composting, so as to solve the problems raised in the above-mentioned background technology.
[0005] A seedling growing cup capable of being degraded by household composting comprises the following steps:
[0006] S1: 4-Hydroxyethylimidazole, 2-methylimidazole and dinotefuran are added to deionized water and ultrasonically mixed for 1 to 2 hours to obtain solution A. Zinc phosphate is added to deionized water to obtain solution B. Solution A is added to solution B under ultrasonic conditions and purified to obtain ZIF-8-OH; (2) Polylactic acid is added to chloroform to completely dissolve it, and SOCl2 is added dropwise and reacted for 3 to 4 hours to obtain chlorinated polylactic acid; (3) Lignin and ZIF-8-OH are added to anhydrous pyridine and stirred at 115 to 125°C for 20 to 30 minutes, and chlorinated polylactic acid is added and reacted for 4 to 6 hours to obtain a composite material.
[0007] S2: (1) placing diatomaceous earth in a ZnCl2 aqueous solution, stirring for 12 to 14 hours, adjusting the pH to 7.5 to 8.8, reacting for 1 to 2 hours, centrifuging, and drying to obtain modified diatomaceous earth A; uniformly mixing the modified diatomaceous earth A with heavy calcium carbonate, calcining at 500 to 700°C for 2 to 3.5 hours to obtain modified diatomaceous earth B; (2) adding the modified diatomaceous earth B to deionized water and ultrasonically dispersing it for 30 to 40 minutes to obtain a suspension A; adding chitosan to a 4 to 5 wt% glacial acetic acid aqueous solution to obtain a mixed solution B; uniformly mixing the mixed solution B with the suspension A, reacting at 65 to 78°C for 1.5 to 3 hours, and purifying to obtain modified diatomaceous earth.
[0008] S3: weigh the raw materials of the seedling cup according to the mass fraction, mix them evenly, and obtain a mixed material;
[0009] S4: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled, pulled, cooled and shaped to obtain a sheet;
[0010] S5: The sheet is formed by vacuum forming to obtain a seedling cup.
[0011] More optimally, the raw materials of the seedling cup include the following components: by weight, 25 to 35 parts of polylactic acid, 45 to 60 parts of polyhydroxyalkanoate, 0.3 to 0.8 parts of nucleating agent, 5 to 15 parts of modified diatomaceous earth, 0.2 to 1 parts of composite material, 2 to 5 parts of toughening agent, 0.5 to 1.5 parts of coupling agent, and 1 to 5 parts of lubricant.
[0012] Preferably, the polyhydroxyalkanoic acid ester includes one or more of polytrihydroxyalkanoic acid ester, polytrihydroxybutyrate, tetrahydroxybutyrate, 3-hydroxybutyric acid, and 3-hydroxyhexanoic acid.
[0013] More optimally, the toughening agent includes one or two of polybutylene adipate / terephthalate and polycaprolactone; the coupling agent includes one or more of silanes, titanates and aluminate compounds.
[0014] Preferably, the lubricant includes one or more of stearic acid, erucic acid, and polyethylene wax.
[0015] More optimally, the nucleating agent is ethylene bisstearamide.
[0016] The parameters of the twin-screw sheet drawing machine are as follows: the screw temperature is 150-195°C, the screw speed is 60-150rpm; the sheet specifications are as follows: the sheet thickness is 0.2-0.4mm, and the width is 660-710mm;
[0017] The parameters of the blister molding are more optimized as follows: the baking temperature is 135-160°C, the baking time is 3-7 seconds, the blister molding time is 15-25 seconds, and the cooling temperature is 10-25°C.
[0018] More optimally, the mass ratio of the diatomite to ZnCl2 in the ZnCl2 aqueous solution is (4-5.5):3; the mass ratio of the modified diatomite A to heavy calcium carbonate is 1:(0.8:1.2).
[0019] More optimally, the mass fraction of modified diatomaceous earth B in the suspension A is 40-55% of deionized water; the mass fraction of chitosan in the mixed solution B is 4-5wt% and the mass fraction of glacial acetic acid aqueous solution is 4-8%; the mass ratio of suspension A to mixed solution B is 1:(1-2).
[0020] More optimally, the raw materials of the ZIF-8-OH include the following components: by weight, 3 to 4 parts of 2-methylimidazole, 0.1 to 0.2 parts of 4-hydroxyethylimidazole, 0.4 to 0.6 parts of dinotefuran, and 0.8 to 0.12 parts of zinc phosphate; the volume ratio of solution A to solution B is (1 to 1.2):1; the mass ratio of polylactic acid to thionyl chloride is 1:(1 to 2); the raw materials of the composite material include the following components: by weight, 3.5 to 5 parts of lignin, 2 to 4 parts of ZIF-8-OH, and 8 to 9 parts of polylactic acid chloride.
[0021] The seedling cup prepared by the present invention has good degradability, and the degradation time is 6 to 15 months under household composting conditions; the density of the seedling cup is 1.1 to 1.25 g / cubic centimeter, and the density within this range can provide sufficient structural support and stability for the seedling cup. The elongation rate of the seedling cup is 70 to 140%, and the tensile strength is 31 to 55 MPa, so that the seedling cup has good ductility and is conducive to the development of plant roots.
[0022] In the scheme, polylactic acid and polyhydroxyalkanoate are used as basic materials. The polyhydroxyalkanoate and polylactic acid blending system has good compatibility, and polyhydroxyalkanoate can effectively improve the toughness of polylactic acid materials.
[0023] Diatomaceous earth can provide basic structure and support for the seedling cup, promote water regulation, help maintain appropriate soil moisture, and provide space for root growth, so that plants can grow healthily. Among them, heavy calcium carbonate can increase the stability of the composite material, making the seedling cup more durable. Heavy calcium carbonate can also adjust the pH value of the soil inside the seedling cup to provide a more suitable growth environment for the seedlings. During the degradation process of the seedling cup, heavy calcium carbonate can also release calcium, providing the necessary nutrients for plant growth, promoting root growth and plant health. Zinc oxide has antibacterial, antifungal and anti-corrosion properties, which can keep the internal environment of the seedling cup clean and hygienic.
[0024] As a biodegradable polymer, chitosan can provide some nutrients for plants and promote their growth. At the same time, it has good water retention properties, which helps to keep the soil moist, provide water and nutrients to plants, and thus promote seed germination and seedling growth. In addition, chitosan itself has gelling and adhesive properties, which can form glue bridges between diatomaceous earth particles, enhance the binding force between particles, and further improve the overall mechanical properties of the seedling cup.
[0025] In the scheme, the ZIF-8 in the composite material contains a pore structure composed of metal ions and organic ligands. These pores can absorb oxygen molecules and stabilize them in the lattice, making ZIF-8 antioxidant. Hydroxylated ZIF-8 can form more elastic support structures in the material and increase the mechanical properties of the material. Dinotefuran is added during the production of ZIF-8 to prevent it from being released too early. During the slow degradation of the seedling cup, dinotefuran is also released, providing a good growth environment for the seedlings.
[0026] Lignin is a natural polymer with a high molecular structure. The aromatic ring and active functional group in lignin are conjugated, which makes lignin anti-ultraviolet. Adding lignin to the seedling cup forms a porous structure in the seedling cup, thereby increasing the mechanical properties of the seedling cup and facilitating the respiration and growth of the root system. Degraded lignin can increase the organic matter content of the soil, improve the structure and texture of the soil, increase the permeability and water retention of the soil, and release organic carbon after degradation, which can provide a carbon source for plants.
[0027] The degradation performance of lignin can be improved by reacting polylactic acid with hydroxylated ZIF-8 and lignin after chlorination, and the compatibility between lignin and ZIF-8 and polylactic acid and polyhydroxyalkanoates can be improved, thereby improving the dispersibility of ZIF-8 and lignin in the seedling cup. DETAILED DESCRIPTION
[0028] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0029] In the following specific embodiments, parts are by weight. In the present embodiment, it should be noted that the purchase manufacturers of all raw materials involved in the present invention include, without any special restrictions, exemplarily: the diatomaceous earth has a CAS number of BD0506, the ZnCl2 has a CAS number of 7646-85-7, the heavy calcium carbonate has a CAS number of HC2080, the chitosan model is food grade, the CAS number of glacial acetic acid is 64-19-7, the CAS number of 4-hydroxyethylimidazole is 872-82-2, the CAS number of 2-methylimidazole is 693-98-1, the CAS number of dinotefuran is 165252-70-0, the CAS number of zinc phosphate is 7779-90-0, and the CAS number of polylactic acid is S3078 9-1g, the CAS number of thionyl chloride is 7719-09-7, the CAS number of chloroform is 67-66-3, the CAS number of pyridine is 110-86-1, the product number of polyhydroxyalkanoate is H2200, the CAS number of KH-570 silane coupling agent is 2530-85-0, the product number of polybutylene adipate / terephthalate is JS1934, the CAS number of erucamide is 112-84-5, the CAS number of ethylene bisstearamide is 110-30-5, the product number of lignin is 8068-05-1, the model of butylated hydroxytoluene (antioxidant) is food grade, and the product number of anti-ultraviolet agent is 051.
[0030] The preparation method of modified diatomite is as follows: (1) diatomite and ZnCl2 are weighed in a mass ratio of 5:3; diatomite is added to deionized water, ultrasonically dispersed for 25 minutes, ZnCl2 is added, stirred for 18 hours, the pH is adjusted to 8.2, the reaction is continued for 1.5 hours, centrifuged, and dried to obtain modified diatomite A; modified diatomite A and heavy calcium carbonate are uniformly mixed in a mass ratio of 1:1, and calcined at 620°C for 3.5 hours to obtain modified diatomite B; (2) modified diatomite B The mixture was added into deionized water for ultrasonic dispersion for 30 minutes to obtain suspension A; the mass fraction of modified diatomaceous earth B in the suspension A to deionized water was 48%; chitosan was added into a 4.5wt% glacial acetic acid aqueous solution to obtain a mixed solution B; the mass fraction of chitosan in the mixed solution B to the 4.5wt% glacial acetic acid aqueous solution was 6.5%; the mixed solution B and the suspension A were uniformly mixed, reacted at 75°C for 2 hours, purified, and modified diatomaceous earth was obtained; the mass ratio of suspension A to mixed solution B was 1:1.6.
[0031] The preparation method of the composite material is as follows: (1) adding 0.17 parts of 4-hydroxyethylimidazole, 4 parts of 2-methylimidazole and 0.4 parts of dinotefuran to deionized water, and ultrasonically mixing for 1 hour to obtain solution A, adding 0.8 parts of zinc phosphate to deionized water to obtain solution B, and mixing solution A and solution B at a volume ratio of 1:1 under ultrasonic conditions, centrifuging, and washing with water for 3 times to obtain ZIF-8-OH; (2) weighing polylactic acid and thionyl chloride at a mass ratio of 1:1.2; adding polylactic acid to chloroform to completely dissolve it, adding SOCl2 dropwise, and reacting for 4 hours to obtain chlorinated polylactic acid; (3) adding 5 parts of lignin and 2 parts of ZIF-8-OH to anhydrous pyridine, stirring and reacting at 120°C for 30 minutes, adding 8.5 parts of chlorinated polylactic acid, and reacting for 5 hours to obtain a composite material.
[0032] Example 1: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 7 parts of diatomaceous earth, 0.4 parts of ethylene bis stearamide, 0.5 parts of antioxidant, 0.5 parts of anti-ultraviolet agent, 2 parts of polybutylene adipate / terephthalate, 0.5 parts of KH-570 silane coupling agent, and 1 part of erucamide were uniformly mixed for 20 to 30 minutes to obtain a mixed product;
[0033] S2: The mixed material is put into a twin-screw extruder, and is subjected to melt plasticization, extrusion, rolling and pulling, and cooling and shaping to obtain a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0034] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0035] Example 2: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 7 parts of modified diatomaceous earth, 0.4 parts of ethylene bisstearamide, 1 part of composite material, 3 parts of polybutylene adipate / terephthalate, 1 part of KH-570 silane coupling agent, and 1.5 parts of erucamide were uniformly mixed for 30 minutes to obtain a mixed material;
[0036] S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled and drawn, and cooled to form a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0037] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0038] Example 3: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 5 parts of modified diatomaceous earth, 0.4 parts of ethylene bisstearamide, 0.6 parts of composite material, 3 parts of polybutylene adipate / terephthalate, 1 part of KH-570 silane coupling agent, and 1.5 parts of erucamide were uniformly mixed for 30 minutes to obtain a mixed material;
[0039] S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled and drawn, and cooled to form a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0040] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0041] Example 4: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 9.5 parts of modified diatomaceous earth, 0.4 parts of ethylene bisstearamide, 1 part of composite material, 3 parts of polybutylene adipate / terephthalate, 1 part of KH-570 silane coupling agent, and 1.5 parts of erucamide were uniformly mixed for 30 minutes to obtain a mixed material;
[0042] S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled and drawn, and cooled to form a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0043] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0044] Comparative Example 1 is based on Example 2, but the diatomaceous earth is not modified.
[0045] Comparative Example 1: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 7 parts of diatomaceous earth, 0.4 parts of ethylene bisstearamide, 1 part of composite material, 3 parts of polybutylene adipate / terephthalate, 1 part of KH-570 silane coupling agent, and 1.5 parts of erucamide were uniformly mixed for 30 minutes to obtain a mixed product;
[0046] S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled and drawn, and cooled to form a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0047] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0048] Comparative Example 2 is based on Example 2, except that ZIF-8-OH is not added to the composite material.
[0049] Comparative Example 2: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 7 parts of modified diatomaceous earth, 0.4 parts of ethylene bisstearamide, 1 part of composite material, 3 parts of polybutylene adipate / terephthalate, 1 part of KH-570 silane coupling agent, and 1.5 parts of erucamide were uniformly mixed for 30 minutes to obtain a mixed material;
[0050] S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled and drawn, and cooled to form a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0051] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0052] Comparative Example 3 is based on Example 2, but no lignin is added to the composite material.
[0053] Comparative Example 3: S1: 25 parts of polylactic acid, 45 parts of polyhydroxyalkanoate, 7 parts of modified diatomaceous earth, 0.4 parts of ethylene bisstearamide, 1 part of composite material, 3 parts of polybutylene adipate / terephthalate, 1 part of KH-570 silane coupling agent, and 1.5 parts of erucamide were uniformly mixed for 30 minutes to obtain a mixed material;
[0054] S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled and drawn, and cooled to form a sheet; the parameters of the twin-screw extruder are: screw temperature is 175°C, screw speed is 90rpm; the specifications of the sheet are: sheet thickness is 0.2mm, width is 660mm;
[0055] S3: forming the sheet material by vacuum forming to obtain a seedling cup; the parameters of the vacuum forming are: a baking temperature of 135° C., a baking time of 5 seconds, a vacuum forming time of 20 seconds, and a cooling temperature of 23° C.
[0056] Test experiment 1: Examples 1 to 4 and comparative examples 1 to 3 were cut into 5 cm×5 cm pieces, and mechanical properties of Examples 1 to 3 and comparative examples 1 to 3 were tested using a universal mechanical testing machine at a tensile speed of 30 mm / min.
[0057]
[0058]
[0059] Conclusion: Comparative Example 1 is based on Example 2, and the diatomaceous earth is not modified, thereby reducing the elongation and tensile strength of the seedling cup. Heavy calcium carbonate can increase the stability of the composite material, making the seedling cup more sturdy and durable. Chitosan can increase the strength of the material in the composite material, because chitosan itself has gelling and adhesion properties, which can enhance the binding force between particles and further improve the overall mechanical properties of the seedling cup. Comparative Example 2 is based on Example 2, and ZIF-8-OH is not added to the composite material. ZIF-8, as a porous material, can adjust the pore structure of the seedling cup to make it more suitable for the growth and development of plant roots. Hydroxylated ZIF-8 can form more elastic support structures in the material, thereby enhancing the mechanical properties of the seedling cup. Comparative Example 3 is based on Example 2, and lignin is not added to the composite material. Lignin is a natural polymer with a high molecular structure. Lignin is added to the seedling cup to form a porous structure in the seedling cup, thereby increasing the mechanical properties of the seedling cup.
[0060] Test experiment 2: 100 sowing peanuts were taken from Examples 1 to 4 and Comparative Examples 1 to 3 respectively, and the results were observed and recorded.
[0061]
[0062] Conclusion: Comparative Example 1 is based on Example 2, and diatomaceous earth is not modified. Because chitosan itself is biodegradable, it is modified to form a composite made of diatomaceous earth, heavy calcium carbonate and zinc oxide, which has a slow release effect on the trace elements in heavy calcium carbonate and zinc oxide, thereby promoting the growth of seedlings. Comparative Example 2 is based on Example 2, and ZIF-8-OH is not added to the composite material. During the slow degradation of the seedling cup, the dimethoate insecticide and nitrogen element in ZIF-8 are slowly released, providing a good growth environment for the seedlings. Comparative Example 3 is based on Example 2, and lignin is not added to the composite material, resulting in a decrease in the structural stability of Comparative Example 3, which improves the degradation of the seedling cup and promotes the release of nutrients in the seedling cup. However, the seedling height becomes lower after 100 days, because compared with other materials containing lignin, the degraded lignin can increase the organic matter content of the soil, improve the structure and texture of the soil, increase the permeability and water retention of the soil, and release organic carbon after lignin degradation, which can provide a carbon source for plants.
[0063] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A seedling cup that can be degraded by home composting, characterized in that: The raw materials of the seedling cup include the following components: by weight, 25 to 35 parts of polylactic acid, 45 to 60 parts of polyhydroxyalkanoate, 0.3 to 0.8 parts of nucleating agent, 5 to 15 parts of diatomaceous earth, 0.1 to 0.5 parts of antioxidant, 0.1 to 0.5 parts of anti-ultraviolet agent, 2 to 5 parts of toughening agent, 0.5 to 1.5 parts of coupling agent, and 1 to 5 parts of lubricant.
2. A home compostable seedling cup according to claim 1, characterized in that: The polyhydroxyalkanoic acid ester includes one or more of polytrihydroxyalkanoic acid ester, polytrihydroxybutyrate tetrahydroxybutyrate, 3-hydroxybutyric acid, and 3-hydroxyhexanoic acid; The toughening agent includes one or two of polybutylene adipate / terephthalate and polycaprolactone; the coupling agent includes one or more of silanes, titanates and aluminate compounds.
3. The home compostable seedling cup according to claim 1, characterized in that: The lubricant includes one or more of stearic acid, erucic acid, and polyethylene wax.
4. The home compostable seedling cup according to claim 1, characterized in that: The preparation method of the seedling cup comprises the following steps: S1: Weigh the raw materials of the seedling cup according to the mass fraction, mix them evenly, and obtain a mixed material; S2: The mixed material is placed in a twin-screw extruder, melt-plasticized, extruded, rolled, pulled, cooled and shaped to obtain a sheet; S3: The sheet is formed by vacuum forming to obtain a seedling cup.
5. The home compostable seedling cup according to claim 4, characterized in that: The parameters of the twin-screw sheet drawing machine are: screw temperature is 150-195°C, screw speed is 60-150rpm; the specifications of the sheet are: sheet thickness is 0.2-0.4mm, width is 660-710mm; The parameters of the blister molding are: baking temperature is 135-160°C, baking time is 3-7 seconds, blister molding time is 15-25 seconds, and cooling temperature is 10-25°C.
6. A home compostable seedling cup according to claim 5, characterized in that: The diatom is modified diatomaceous earth; Using composite materials as antioxidants and UV inhibitors; The raw materials of the seedling cup include the following components: by weight, 25 to 35 parts of polylactic acid, 45 to 60 parts of polyhydroxyalkanoate, 0.3 to 0.8 parts of nucleating agent, 5 to 15 parts of modified diatomaceous earth, 0.2 to 1 parts of composite material, 2 to 5 parts of toughening agent, 0.5 to 1.5 parts of coupling agent, and 1 to 5 parts of lubricant.
7. The home compostable seedling cup according to claim 6, characterized in that: The preparation method of the modified diatomite is as follows: (1) placing diatomite in a ZnCl2 aqueous solution, stirring for 12 to 14 hours, adjusting the pH to 7.5 to 8.8, reacting for 1 to 2 hours, centrifuging, and drying to obtain modified diatomite A; uniformly mixing the modified diatomite A with heavy calcium carbonate, calcining at 500 to 700° C. for 2 to 3.5 hours to obtain modified diatomite B; (2) adding the modified diatomite B to deionized water for ultrasonic dispersion for 30 to 40 minutes to obtain a suspension A; adding chitosan to a 4 to 5 wt% glacial acetic acid aqueous solution to obtain a mixed solution B; uniformly mixing the mixed solution B with the suspension A, placing at 65 to 78° C. for reaction for 1.5 to 3 hours, purifying, and obtaining the modified diatomite.
8. The home compostable seedling cup according to claim 7, characterized in that: The mass ratio of diatomite to ZnCl2 in ZnCl2 aqueous solution is (4-5.5):3; the mass ratio of modified diatomite A to heavy calcium carbonate is 1:(0.8:1.2); The mass fraction of modified diatomite B in the suspension A to deionized water is 40-55%; the mass fraction of chitosan in the mixed solution B to 4-5wt% glacial acetic acid aqueous solution is 4-8%; the mass ratio of suspension A to mixed solution B is 1:(1-2).
9. The home compostable seedling cup according to claim 6, characterized in that: The preparation method of the composite material is as follows: (1) preparing ZIF-8-OH: adding 4-hydroxyethylimidazole, 2-methylimidazole and dinotefuran to deionized water, ultrasonically mixing for 1 to 2 hours to obtain solution A, adding zinc phosphate to deionized water to obtain solution B, adding solution A to solution B under ultrasonic conditions, purifying, and obtaining ZIF-8-OH; (2) adding polylactic acid to chloroform to completely dissolve it, adding SOCl2 dropwise, reacting for 3 to 4 hours, and obtaining chlorinated polylactic acid; (3) adding lignin and ZIF-8-OH to anhydrous pyridine, stirring at 115 to 125° C. for 20 to 30 minutes, adding chlorinated polylactic acid, and reacting for 4 to 6 hours to obtain a composite material.
10. The home compostable seedling cup according to claim 6, characterized in that: The raw materials of ZIF-8-OH include the following components: by weight, 3 to 4 parts of 2-methylimidazole, 0.1 to 0.2 parts of 4-hydroxyethylimidazole, 0.4 to 0.6 parts of dinotefuran, and 0.8 to 0.12 parts of zinc phosphate; the volume ratio of solution A to solution B is (1 to 1.2):1; the mass ratio of polylactic acid to thionyl chloride is 1:(1 to 2); the raw materials of the composite material include the following components: by weight, 3.5 to 5 parts of lignin, 2 to 4 parts of ZIF-8-OH, and 8 to 9 parts of polylactic acid chloride.