Composition and application thereof
By using cationic polymerizable resins, cationic initiators and polymerization inhibitors in the semiconductor field, the wire breakage and warping problems caused by high-temperature curing are solved, the bonding strength and stability are improved, and the bonding effect is reliable. and storage stability.
Patent Information
- Application Number
- CN202310526555.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-10
- Publication Date
- 2024-11-19
AI Technical Summary
In the semiconductor field, wire breakage, warping and wiring dislocation caused by high-temperature curing adhesive compositions, and the bonding strength of the cationic initiator conflicts with storage stability, resulting in unstable bonding effect.
Provided is a composition including a cationic polymerizable resin, a cationic initiator and a polymerization inhibitor. The polymerization inhibitor is a hindered amine or hindered phenol, with a PKa greater than 7.0, which improves storage stability and bond strength by defining the composition and reduces the temperature. and humidity requirements for storage and transportation, and achieve high bond strength at lower curing temperatures.
It improves the stability and reliability of the bonding effect, reduces storage and transportation costs, improves the structural accuracy and production yield of the product, and avoids side reactions affecting the bonding effect.
Smart Images

Figure CN118978884A_ABST
Abstract
Description
Technical Field
[0001] The embodiments of the present application particularly relate to a composition and application thereof, belonging to the technical field of electronic equipment. Background Art
[0002] In the semiconductor field, adhesives are usually used to fix electronic parts and connect circuits. For example, anisotropic conductive film (ACF) dispersed with conductive particles is used as a circuit connection material to achieve the connection between a liquid crystal display and a tape carrier package (TCP), the connection between a flexible printed circuit (FPC) and TCP, and the connection between an FPC and a printed circuit board. In this field, as the density and clarity of electronic circuits increase, adhesives are required to have high bonding strength.
[0003] In recent years, in the field of precision electronic equipment, circuits have become more dense, and electrode widths and electrode spacings have become extremely narrow. Therefore, when using adhesive compositions with high curing temperatures for connection, high temperatures often lead to undesirable phenomena such as disconnection, warping, and wiring dislocation. Among them, the expansion and peeling of chips and substrates caused by warping are very serious, making it difficult to meet the requirements in terms of bonding strength and product precision.
[0004] Adhesive compositions including cationic initiators are often able to achieve high bonding strength at lower curing temperatures. However, there is a conflict between the bonding strength and storage stability of such adhesive compositions, which often decompose and denature during storage before curing and bonding applications, resulting in unstable bonding effects, weakening, or even failure. Summary of the invention
[0005] The embodiments of the present application provide a composition and application thereof, and by limiting the composition of the composition, the storage stability of the composition is improved, thereby ensuring the reliability and stability of the bonding strength of the composition after curing.
[0006] In one aspect, an embodiment of the present application provides a composition, including a cationic polymerizable resin, a cationic initiator, and an inhibitor;
[0007] The polymerization inhibitor is a hindered amine compound and / or a hindered phenol compound, and the PKa of the polymerization inhibitor is greater than 7.0.
[0008] The composition satisfying the above composition has a certain degree of reaction inertness. Therefore, even if the temperature and humidity of the external environment are high, the composition can stably exist, avoiding the bonding effect being affected due to the occurrence of side reactions, and improving the stability and reliability of the bonding effect of the composition after curing application. At the same time, the reaction inertness can also reduce the temperature and humidity requirements of the composition during storage and transportation, so that the cost of storage and transportation is controlled. In addition, the combination of cationic polymerizable resin and cationic initiator has the advantage of achieving high bonding strength at a lower curing temperature, so the bonding effect is guaranteed, especially the structural accuracy and production yield of products in the semiconductor field can be improved.
[0009] In a possible implementation, the mass ratio of the polymerization inhibitor to the cationic initiator is (0.01-20):100.
[0010] This ratio can further balance the reaction inertness of the composition and improve the reaction controllability of the composition.
[0011] In a possible implementation, the mass ratio of the polymerization inhibitor to the cationic polymerizable resin is not less than 1:10.
[0012] In a possible implementation, the cationic polymerizable resin includes an epoxy compound.
[0013] In a possible implementation, the cationic polymerizable resin further includes an oxetane compound.
[0014] In a possible implementation, the polymerization inhibitor has a structure shown in either Formula 1 or Formula 2.
[0015]
[0016] wherein R1 and R2 each independently represent a hydrogen atom, a single bond, or a monovalent organic group, R4, R5, R6, and R7 each independently represent a hydrogen atom, a single bond, an alkyl group or an alkylene group having 1 to 5 carbon atoms, and at most one of R4 and R5 is a hydrogen atom, and at most one of R6 and R7 is a hydrogen atom;
[0017] R 12 represents a hydrogen atom, a single bond or a monovalent organic group, R 13 , R 14 Each independently represents a single bond, an alkyl group or an alkylene group having 1 to 8 carbon atoms.
[0018] In a possible implementation, an auxiliary agent is further included, and the auxiliary agent is selected from at least one of a conductive agent, a solvent, a film former, a toughening agent, a filler, a reinforcing agent, a stabilizer, a coupling agent and a colorant.
[0019] An embodiment of the present application also provides a polymer, which is obtained by curing any one of the aforementioned compositions; the polymer includes a cross-linking unit formed by the cationic polymerizable resin as a cross-linking monomer and the inhibitor.
[0020] The above-mentioned polymer is obtained by curing the above-mentioned composition as a raw material. During the curing process, the cationic polymerizable resin is cross-linked to form a cross-linking unit, and the polymerization inhibitor is dispersed in the cross-linking unit. The polymer can improve the structural accuracy and production yield of the product through its own performance in terms of adhesion and mechanical properties.
[0021] The present application also provides a method for preparing a polymer, wherein the composition is subjected to a curing treatment to obtain the polymer; the curing treatment includes light treatment or heating treatment.
[0022] The light treatment and the heating treatment are both used to induce the cationic initiator in the initiator composition to release cations, thereby initiating the cross-linking of the cationic polymerizable resin.
[0023] An embodiment of the present application further provides a display screen, comprising a first structural member, an adhesive layer, and a second structural member, wherein the first structural member and the second structural member are bonded via the adhesive layer, and the adhesive layer comprises the polymer described above.
[0024] By connecting the first structural member and the second structural member using an adhesive layer including a polymer, the high adhesive strength and reliability of the adhesive layer enable the display screen to have excellent performance in terms of structural accuracy and manufacturing yield, thus having a positive driving effect on the development of the semiconductor field.
[0025] In a possible implementation manner, the first structural member and the second structural member are each independently selected from one of a chip, a screen, a flexible printed circuit, and a packaging member.
[0026] The embodiment of the present application also provides an electronic device, which at least includes a housing and a display screen as described in any one of the above items. The display screen is connected to the housing. By including the display screen, the reliability of use and life of the electronic device can be guaranteed. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 A three-dimensional diagram of an electronic device provided for this application;
[0028] Figure 2 An exploded diagram of an electronic device provided for this application;
[0029] Figure 3 is a schematic diagram of the structure of the film-like composition in Example 9 of the present application;
[0030] Figure 4This is a schematic diagram of the application of the film-like composition of the embodiment of the present application. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solutions and advantages of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0032] A first aspect of an embodiment of the present application provides a composition comprising a cationic polymerizable resin, a cationic initiator, and an inhibitor; the inhibitor is a hindered amine compound and / or a hindered phenol compound, and the PKa of the inhibitor is greater than 7.0.
[0033] The composition of the embodiment of the present application refers to a composition that can undergo curing (polymerization cross-linking reaction) under certain induction initiation conditions.
[0034] In the above composition, cationic polymerizable resin refers to a compound that can undergo polymerization and crosslinking to solidify in the presence of cations (generally referring to hydrogen ions); cationic initiator refers to a compound that can release cations (generally referring to hydrogen ions) under certain induced initiation conditions, wherein the induced initiation conditions include thermal initiation or photoinitiation; inhibitor refers to a compound that can prevent the cationic polymerizable resin from undergoing polymerization and crosslinking to a certain extent, wherein the inhibitor is specifically at least one of a hindered amine compound and a hindered phenol compound, and the acidity dissociation constant PKa is greater than 7.0.
[0035] The present invention does not limit the specific selection of the cationic polymerizable resin, cationic initiator and polymerization inhibitor, as long as the above requirements are met. The composition comprising the cationic polymerizable resin and the cationic initiator can be cured at a relatively low temperature and in a short time, and the obtained polymer has excellent bonding strength.
[0036] In addition, according to the above scheme provided by the present invention, the composition also has excellent storage stability. On the one hand, even if the composition has a long storage or transportation period from preparation to actual curing application, the composition will not have side reactions, thereby ensuring that it still has excellent curing effect when it is actually cured and applied. Specifically, even if it is stored or transported for a long time before curing application, it can still show stable and excellent bonding strength after curing, and the rate of change of bonding strength does not exceed 20%; on the other hand, the advantage of strong stability can reduce the stringency of requirements for storage environment parameters and transportation environment parameters, which not only broadens the application range of the composition, but also controls the high cost of transportation and storage.
[0037] Based on this phenomenon, the inventor analyzed the stability principle and believed that it might be that as an electron-rich compound, a hindered amine or hindered phenol inhibitor with a pKa greater than 7 can efficiently capture cations (especially hydrogen ions) in the environment, avoiding the side reactions or premature curing of the cationic polymerizable resin under the initiation of cations; and when the composition is given the conditions for achieving the curing reaction (high temperature or light), the electron cloud in the hindered amine or hindered phenol inhibitor will move and disperse, thereby weakening the ability to capture cations, so that the cations can restore the reaction activity and induce the curing of the cationic polymerizable resin, thereby obtaining a polymer with excellent bonding strength. Therefore, the composition of the embodiment of the present application has the characteristics of suitable reaction inertness, precise and controllable curing reaction, and stable bonding effect due to curing application.
[0038] The present application embodiment does not specifically limit the preparation method of the composition, as long as the various components are mixed.
[0039] In the specific implementation process of the embodiment of the present application, the mass ratio of the polymerization inhibitor to the cationic initiator is generally controlled to be above 0.001%. Reasonable control of the amount of polymerization inhibitor added is conducive to further improving the stability of the composition, so the mass ratio of the polymerization inhibitor to the cationic initiator can be made not less than 0.01%. The inventors have found that as the amount of the polymerization inhibitor increases within a certain range, the stability of the composition first shows an increasing trend, and then remains basically unchanged, but when the polymerization inhibitor is added too much, the bonding strength of the polymer after the curing reaction will be affected to a certain extent. Therefore, for the dual consideration of improving stability and bonding strength, the mass ratio of the polymerization inhibitor to the cationic initiator is generally controlled to be (0.01-20):100.
[0040] Of course, the use of different inhibitors, or even different cationic polymerizable resins or cationic initiators in the cationic composition will have an impact on the properties of the composition, including stability and curing performance. Therefore, generally speaking, for the above-mentioned different inhibitors, cationic initiators, and cationic polymerizable resins, when the mass ratio of the inhibitor to the cationic initiator is controlled within the range of (0.1-10):100, the performance of the composition can basically be optimized.
[0041] The present invention does not specifically limit the mass percentage of the cationic polymerizable resin in the composition, and can be determined according to the required crosslinking density and physical properties (such as glass transition temperature, elastic modulus, etc.) of the polymer. In the specific implementation of the embodiment of the present application, the mass ratio of the inhibitor to the cationic polymerizable resin is not less than 1:10, for example, 1:(20-1000).
[0042] In a specific implementation process, the cationic polymerizable resin includes an epoxy compound. The epoxy compound refers to a compound including an epoxy group in the molecule. Specifically, the present application does not limit the number of epoxy groups in the epoxy compound.
[0043] The epoxy compound includes at least one of bisphenol epoxy compounds, aromatic epoxy compounds, novolac epoxy compounds, and aliphatic epoxy compounds. Among them, the bisphenol epoxy compounds include at least one of bisphenol A type epoxy resin compounds, bisphenol A type epoxy acrylate compounds, bisphenol F type epoxy compounds, bisphenol AD type epoxy compounds, bisphenol E type epoxy compounds, and bisphenol S type epoxy compounds; the aromatic epoxy compounds include at least one of polyglycidyl ether aromatic epoxy compounds, polyglycidyl ester aromatic epoxy compounds, glycidyl amine aromatic epoxy resins, biphenyl diglycidyl ether epoxy resins, and naphthalene epoxy compounds; the novolac epoxy compounds include cresol novolac epoxy resins and phenol novolac epoxy resins. At least one of the epoxy resins of the type; the aliphatic epoxy compound includes at least one of 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate, bis(3,4-epoxycyclohexylmethyl)adipate, vinylcyclohexene diepoxide, N-methyl-4,5-epoxycyclohexane-1,2-dicarboximide, polyglycidyl ether aliphatic epoxy compounds, polyglycidyl ester aliphatic epoxy compounds, glycidyl amine aliphatic epoxy resin, N-ethyl-4,5-epoxycyclohexane-1,2-dicarboximide, and can even be a compound including an aliphatic epoxy substituent.
[0044] Furthermore, from the perspective of reducing the curing reaction time, since the alicyclic epoxy compounds have epoxy groups present near the alicyclic ring, the ring-opening reaction is faster, and thus they can exhibit better cationic polymerization curing reactivity compared to other epoxy compounds.
[0045] Further, in addition to epoxy compounds, cationic polymer resin also includes oxetane compounds.Oxetane compounds refer to compounds with oxetane groups, and specifically, the present application does not limit the number of oxetane groups in oxetane compounds. Exemplarily, oxetane compounds include biphenyl dioxetane, 3-ethyl-3{[(3-ethyloxetane-3-yl)methoxy]methyl}oxetane, 3-ethyl-3 hydroxymethyloxetane, 3-(methyl)allyloxymethyl-3-ethyloxetane, (3-ethyl-3-oxetane methoxy)methylbenzene, 2-ethylhexyl (3-ethyl-3-oxetane methyl) ether, dicyclopentadiene (3-ethyl-3-oxetane methyl) ether at least one.
[0046] In a specific embodiment, the inhibitor has a structure shown in either Formula 1 or Formula 2,
[0047]
[0048] wherein R1 and R2 independently represent a hydrogen atom, a single bond, or a monovalent organic group, R4, R5, R6, and R7 independently represent a hydrogen atom, a single bond, an alkyl group or an alkylene group having 1 to 5 carbon atoms, and at most one of R4 and R5 is a hydrogen atom, and at most one of R6 and R7 is a hydrogen atom; R 12 represents a hydrogen atom, a single bond or a monovalent organic group, R 13 , R 14 Each independently represents a single bond, an alkyl group or an alkylene group having 1 to 8 carbon atoms.
[0049] The monovalent organic group referred to in the embodiments of the present application refers to a monovalent organic group, such as a hydroxyl group, an alkyl group, a halogen substituent, a (substituted) aryl group, a (substituted) alkoxy group, a (substituted) amino group, an ester group, and the like.
[0050] The above formula 1 shows a hindered amine structure.
[0051] In Formula 1, when R1 and R2 are independently a hydrogen atom or a monovalent organic group, R4, R5, R6, and R7 are independently a hydrogen atom or an alkyl group having 1 to 5 carbon atoms, and at most one of R4 and R5 is a hydrogen atom, and at most one of R6 and R7 is a hydrogen atom, the structure shown in Formula 1 is a compound and the compound is a hindered amine compound; when at least one of R1 and R2 is a single bond, and / or at least one of R4, R5, R6, and R7 is a single bond or an alkylene group having 1 to 5 carbon atoms, the structure shown in Formula 1 can be substituted as a hindered amine substituent on other compounds (such as polyamine compounds, polyester compounds, and polyacrylate compounds).
[0052] Illustratively, the hindered amine compound having the above structure is 2,2,6,6-tetramethylpiperidine and its derivatives, 1,2,2,6,6-pentamethylpiperidine and its derivatives.
[0053] The above formula 2 shows the hindered phenol structure.
[0054] In formula 2, when R 12 is a hydrogen atom or a monovalent organic group, and R 13 With R 14 When each of R is independently an alkyl group having 1 to 8 carbon atoms, the structure shown in Formula 2 is a compound and the compound is a hindered phenol compound; when R 12 is a single bond, and / or, R 13 With R 14 When at least one of the groups is a single bond and an alkylene group having 1 to 8 carbon atoms, the structure shown in Formula 2 can be substituted on other compounds as a hindered phenol substituent.
[0055] Illustratively, the hindered phenol compound having the above structure is 2,6-di-tert-butyl-p-cresol, β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, pentaerythritol tetrakis[β-(3,5-di-tert-butyl-4-hydroxyphenyl) propionate, N,N'-bis-(3-(3,5-di-tert-butyl-4-hydroxyphenyl) propionyl)hexanediamine, and the like.
[0056] In a specific embodiment, the cationic initiator comprises a salt of a quaternary ammonium cation and / or a sulfonium cation. The anion in the salt comprises, for example, at least one of hexafluoroantimonate anion, hexafluorophosphate anion, trifluoromethanesulfonate anion, perfluorobutanesulfonate anion, dinonylnaphthalenesulfonate anion, p-toluenesulfonate anion, dodecylbenzenesulfonate anion or tetrakis(pentafluorophenyl)borate anion.
[0057] In addition to the cationic polymerizable resin, cationic initiator and inhibitor, at least one functional auxiliary agent may be added to the composition according to further application requirements. The auxiliary agent includes but is not limited to at least one of a conductive agent, a solvent, a film former, a toughening agent, a filler, a reinforcing agent, a stabilizer, a coupling agent and a colorant.
[0058] Specifically, when the polymer obtained by curing the composition has a conductive requirement, such as a conductive adhesive, a conductive agent may also be included in the composition. Conductive agents include, for example, metals and conductive carbon. Exemplarily, the metal is selected from at least one of Au, Ag, Ni, Cu, solder, etc. In one embodiment, the conductive agent may be a core-shell coating structure. In detail, in the conductive agent of the core-shell coating structure, the material of the core includes at least one of non-conductive glass, ceramic, plastic, etc., and the material of the shell coated on at least part of the surface of the core is selected from the conductive agent mentioned above. Further, the conductive agent may be conductive particles having an average particle size of 1-20 μm. It can be understood that when the content of the conductive agent is too high, a short circuit may occur, and when the content of the conductive agent is too low, it is not conducive to the realization of electrical conduction. Therefore, the mass percentage of the conductive agent in the composition is 0.1-30%, and further 0.1-10%. It should be noted that when the composition of the embodiment of the present application including the conductive particles is cured to generate an anisotropic conductive adhesive, even if the composition has a long storage or transportation cycle before curing, the resistance change rate does not exceed 20%.
[0059] The embodiments of the present application do not limit the form of the composition, for example, it may be a solid mixture, or it may be a liquid with a certain viscosity and fluidity. It can be understood that when the composition is in a liquid state, it is more conducive to applying it to the surface of the object to be bonded to initiate curing. Therefore, a suitable amount of solvent can be added to the solid polymer composition so that it is at least partially dissolved into a liquid state. The embodiments of the present application do not particularly limit the solvent, as long as the reaction inertness of the composition can be maintained and it does not react with the composition. In a specific embodiment, the boiling point of the solvent is 50 to 150. If the boiling point is lower than 50°C, there is a risk of volatilization at room temperature. If the boiling point exceeds 150°C, the solvent is difficult to volatilize, which may have an adverse effect on the reliability after curing.
[0060] In another embodiment, the composition can also be a solid film. When applied, the solid film is attached to the surface of the object to be bonded, and then solidification is initiated. In order to make the polymer have excellent film-forming properties, a film-forming agent can be added thereto. For example, a solid composition including a film-forming agent is heated and melted (the temperature of heating and melting is lower than the curing temperature), pressed, and cooled to obtain a film-like composition; or, a liquid composition including a film-forming agent and a solvent is pressed and dried to obtain a film-like composition. Specifically, the heated and melted composition or the composition dissolved by a solvent is coated on a strippable substrate such as a fluororesin film, a polyethylene terephthalate film, a release paper, etc., and after pressure, cooling or drying, the film is separated from the glass substrate to obtain a film-like composition.
[0061] The film-forming agent of the embodiment of the present application is a polymer that does not hinder the curing reaction, for example, including at least one of polyimide, polyamide, phenoxy resin, polymethacrylate, polyacrylate, polyurethane, polyester, polyester urethane, polyvinyl butyral, SBS and its epoxy-modified products, SEBS and its modified products, etc. In addition, these polymers may also contain siloxane bonds and fluorine substituents. Generally, polymers with a weight average molecular weight Mw of 5000 to 150000 are selected, and further 10000 to 80000. When the weight average molecular weight of the polymer is less than 5000, there is a tendency for the film-forming property to deteriorate. If it exceeds 150000, there is a phenomenon of deterioration in compatibility with other components. In addition, the film-forming property and the bonding strength after curing can also be improved by controlling the mass ratio of the polymer and the cationic polymerizable resin. Specifically, the mass ratio of the polymer and the cationic polymerizable resin is (20 to 300):100.
[0062] The toughening agent is used to increase the mechanical stress of the polymer after the composition is cured to avoid warping, cracking, etc. The toughening agent can be, for example, rubber elastic material particles, illustratively including at least one of butadiene elastomer, silicone elastomer, acrylic copolymer, styrene-butadiene elastomer (SBS), methyl methacrylate-butadiene-styrene copolymer (MBS), methyl methacrylate-acrylonitrile-butadiene-styrene copolymer (MABS), amino-terminated butadiene-acrylonitrile copolymer (ATBN) and carboxyl-terminated butadiene-acrylonitrile rubber copolymer (CTBN).
[0063] The filler is selected from, for example, silicon dioxide, talc, titanium oxide, calcium carbonate, magnesium oxide, etc. By controlling the mass percentage of the filler in the composition, the polymer conductive particle capture rate after the composition is cured can be enhanced.
[0064] The reinforcing agent is used to improve the mechanical properties of the composition, for example, selected from glass fiber, asbestos fiber, carbon fiber, silica fiber, boron nitride fiber, silicon nitride fiber, metal fiber, wood powder, hollow glass sphere, glass flake and other fibers, and at least one of the structural strength and mechanical properties.
[0065] The stabilizer is used to improve the weather resistance of the composition, such as thermal stability and light stability, and includes, for example, at least one of hydrazine compounds, phosphorus compounds, benzophenone compounds, benzotriazole compounds and oxalic acid anilide compounds.
[0066] The coupling agent is used to further enhance the bonding strength of the composition. Exemplarily, the coupling agent of the embodiment of the present application includes can be appropriately selected according to the purpose, such as vinyl tris (2-methoxyethoxy) silane, vinyl triethoxy silane, vinyl trimethoxy silane, 3-phenylvinyl trimethoxy silane, 3-methacryloxy propyl trimethoxy silane, 3-acryloxy propyl trimethoxy silane, 3-glycidyloxy propyl trimethoxy silane, 3-glycidyloxy propyl methyl diethoxy silane, 2- (3,4-epoxy cyclohexyl) ethyl triethoxy silane, N-2- (aminoethyl) -3-aminopropyl trimethoxy silane, N-2- (aminoethyl) -3-aminopropyl methyl dimethoxy silane, 3-aminopropyl triethoxy silane, N-phenyl -3-aminopropyl trimethoxy silane, 3-mercaptopropyl trimethoxy silane, 3-chloropropyl trimethoxy silane, etc. At least one.
[0067] When the composition does not contain a colorant, the cured polymer has a higher transparency. When the composition contains a colorant, the colorant may be a pigment or a dye, and the cured polymer has a color consistent with the colorant.
[0068] The second aspect of the embodiment of the present application provides a polymer, which is obtained by curing the composition of the first aspect; the polymer includes a cross-linking unit formed by a cationic polymerizable resin as a cross-linking monomer and the inhibitor.
[0069] Specifically, the cationic initiator in the composition releases cations under certain induction conditions (light or heating), and the cationic polymerizable resin in the composition undergoes a certain degree of polymerization and cross-linking in the presence of cations and inhibitors to form cross-linking units. Finally, a polymer including cross-linking units and inhibitors dispersed in the cross-linking units is obtained.
[0070] On the one hand, the aforementioned composition has high storage stability, and on the other hand, it can also be cured in a relatively short time under relatively mild conditions (such as lower heating temperature), and the cured polymer also has the characteristics of high bonding strength. Therefore, the bonding effect of the polymer of the embodiment of the present application is excellent, stable and reliable, and is not prone to warping, breaking and the like. The products bonded by the polymer have significant advantages in terms of structural accuracy and production yield.
[0071] A third aspect of an embodiment of the present application provides a method for preparing a polymer, comprising curing the composition of the first aspect to obtain a polymer; the curing treatment comprises light treatment or heating treatment.
[0072] The embodiments of the present application do not limit the specific parameters of the curing process.
[0073] Taking heating treatment as an example, the temperature and time of curing treatment are particularly related to the selection of cationic initiator. Too low curing temperature will cause defects such as poor stability, while high temperature will cause warping and breakage caused by excessive stress of the polymer after curing. In addition, too long curing time will lead to the occurrence of side reactions that reduce the bonding properties of the polymer, and too short time will lead to the inability to fully carry out the curing treatment (for example, the conversion rate of cationic polymerizable resin is not less than 80%). Therefore, a more matching cationic initiator can be selected according to the temperature and time requirements of the specific application. For example, a cationic initiator is selected based on the curing temperature (i.e., curing temperature) of 60°C to 200°C, further 80°C to 180°C, and the curing time (i.e., curing time) of 0.1 seconds to 10 hours, and further 1 second to 1 hour, and finally a polymer with excellent bonding strength and strong stability is obtained.
[0074] A fourth aspect of the embodiments of the present application further provides a display screen, which includes a first structural member, an adhesive layer and a second structural member, wherein the first structural member and the second structural member are bonded via the adhesive layer, and the adhesive layer includes the polymer of the second aspect.
[0075] The polymer is used as a bonding medium to achieve the connection between the first structural members and the second structural members in the display screen.
[0076] The embodiments of the present application do not limit the selection of the first structural member and the second structural member. Exemplarily, the first structural member and the second structural member are each independently selected from a chip, a screen, a flexible printed circuit, and a package. More specifically, the screen can be, for example, an organic light-emitting semiconductor (Organic Light-Emitting Diode, OLED) or a liquid crystal display (Liquid Crystal Display, LCD), and the package can be TCP.
[0077] In a specific embodiment, the adhesive layer comprising the aforementioned polymer is used for bonding a chip to a liquid crystal display, bonding an FPC to a liquid crystal display, bonding a TCP to an FPC, and the like.
[0078] Specifically, the composition is applied to the surface to be bonded of the first structural member (an object to be bonded), and then the surface to be bonded of the second structural member (another object to be bonded) is covered on the surface of the composition. After curing, a display screen including the first structural member, the bonding layer and the second bonding layer is obtained. During the curing process, the system including the first structural member, the composition and the second structural member can be pressurized to further improve the bonding effect. For example, the pressure is 0.1 to 30 MPa, and the pressurization time is 0.5 to 120 seconds.
[0079] A fifth aspect of an embodiment of the present application further provides an electronic device, which includes a housing and a display screen according to the fifth aspect, wherein the housing and the display screen are connected.
[0080] The electronics include but are not limited to mobile phones, tablet computers, laptops, ultra-mobile personal computers (UMPCs), handheld computers, walkie-talkies, netbooks, POS machines, personal digital assistants (PDAs), driving recorders, wearable devices, virtual reality devices, photoelectric curtain walls and other mobile or fixed terminals with display screens.
[0081] Among them, in the embodiments of the present application, a mobile phone is taken as an example of the above-mentioned electronic device for description. The mobile phone can be a foldable mobile phone, or a straight-screen mobile phone, or a sliding mobile phone. The following is a specific description taking a straight-screen mobile phone as an example.
[0082] Figure 1 A three-dimensional diagram of an electronic device provided in this application, Figure 2 For an exploded view of an electronic device provided in this application, see Figure 1 and Figure 2 As shown, the electronic device 100 may include a display screen 20, a back cover 30 and a middle frame 11, wherein the middle frame 11 is located between the display screen 20 and the back cover 30, wherein the middle frame 11 and the back cover 30 form a housing.
[0083] The electronic device 100 may further include a battery 40 and a circuit board 50, which may be disposed on the middle frame 11, for example, the battery 40 and the circuit board 50 may be disposed on a side of the middle frame 11 facing the back cover 30. Alternatively, in some embodiments, the battery 40 and the circuit board 50 may also be disposed on a side of the middle frame 11 facing the display screen 20. The back cover 30 may be a metal back cover, a glass back cover, a plastic back cover, or a ceramic back cover.
[0084] The electronic device includes a display screen and thus has excellent use reliability and life reliability.
[0085] The composition of the present application is described in detail below through specific examples.
[0086] Example 1
[0087] The preparation method of the composition of this embodiment comprises:
[0088] 100 g of a cationic polymerizable resin (3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate shown in Formula A1), 5 g of a cationic initiator (antimony hexafluoride quaternary ammonium salt shown in Formula B1) and 0.15 g of a hindered amine (bis(2,2,6,6,-tetramethyl-4-piperidinyl)sebacate shown in Formula C1) are uniformly mixed to obtain the composition of this embodiment.
[0089] Example 2 to Example 8, Comparative Example 1 to Comparative Example 6
[0090] The preparation methods of the compositions of Examples 2 to 8 and Comparative Examples 1 to 6 are the same as that of Example 1. The specific compositions of each are shown in Table 1.
[0091]
[0092] The following parameters were tested for all the above examples and comparative examples:
[0093] 1.DSC thermal analysis
[0094] The compositions of the examples and comparative examples were tested using DSC (differential scanning calorimeter, TA Instruments, Mettler Toledo TGA / DSC1 StarSystem) at a rate of 10°C / min in a temperature range of 0°C to 300°C in a nitrogen atmosphere, and the respective DSC exotherm onset temperatures T O With peak temperature T P . T O T is defined as the temperature at the time point when the slope of the DSC curve increases for the first time due to heat generation during DSC testing, and is used to characterize the stability of the composition; P Used to characterize the curing temperature of the composition. The results are shown in Table 1.
[0095] 2. Gel time
[0096] The hot plate method was used to measure the gel time of the compositions of the examples and comparative examples at 100° C., 120° C. and 140° C. The results are shown in Table 1.
[0097] 3. Storage stability
[0098] The viscosity η1 of each of the compositions of Examples and Comparative Examples was measured using a viscometer ("DV2T" manufactured by Brookfield) at 25°C and 200 rpm.
[0099] The compositions of the examples and comparative examples were stored at 60°C for 1 to 6 hours, and their respective viscosities η2 were measured under the same conditions as the viscosity η1. The storage stability was determined according to the following criteria: the greater the change rate of η2 relative to η1, the worse the storage stability. The results are shown in Table 2.
[0100] [Standards for storage stability]
[0101] ○○: Viscosity η2 is less than 110% of viscosity η1
[0102] ○: Viscosity η2 exceeds 110% of viscosity η1 and is 130% or less
[0103] △: Viscosity η2 exceeds 130% and is 150% or less of viscosity η1
[0104] ×: Viscosity η2 exceeds 150% and is 200% or less of viscosity η1
[0105] ××: Viscosity η2 exceeds 200% of viscosity η1
[0106] Table 1
[0107]
[0108] Table 2
[0109]
[0110]
[0111] According to Table 1 and Table 2, we can know that:
[0112] 1. Compared with Comparative Example 1, Comparative Examples 2-6 and all Examples showed more suitable stability temperature and curing temperature in DSC detection.
[0113] 2. In Table 2, compared with the comparative example, the embodiments all showed excellent stability.
[0114] Example 9
[0115] The preparation method of the composition of this embodiment comprises:
[0116] 1) Using a planetary mixer, 100 parts by mass of a methyl ethyl ketone solution of a bisphenol A type phenoxy resin (Mw=70000) (phenoxy resin and methyl ethyl ketone are each 50 parts by mass), 10 parts by mass of 3',4'-epoxycyclohexylmethyl-3,4-epoxycyclohexanecarboxylate (represented by formula A1), 20 parts by mass of 3,4,3',4'-diepoxybicyclohexane (represented by formula A2), 10 parts by mass of biphenylbisoxetane (represented by formula A3), 5 parts by mass of antimony hexafluoride quaternary ammonium salt (represented by formula B1), 0.075 parts by mass of a hindered amine (represented by formula C2), 5 parts by mass of MBS copolymer core-shell particles, 20 parts by mass of fumed silica, 1 part by mass of 2-(3,4-epoxycyclohexyl)ethyltriethoxysilane, and 3 parts by mass of nickel-plated polystyrene particles (average particle size 5 μm) as conductive particles were mixed to prepare a resin solution.
[0117] 2) The resin solution was applied to a polyethylene terephthalate release film having a thickness of 50 μm, and one side was coated using a coating device, followed by hot air drying at 70° C. for 5 minutes to obtain a film-like composition having a thickness of 25 μm. Figure 3 Schematic diagram of the structure of the film-like composition in Example 9 of the present application, wherein the amount of conductive particles 1 added in the film-like composition 10 is 5000 pcs / mm 2 .
[0118] Example 10, Comparative Examples 7 to 9
[0119] The preparation methods of the compositions of Example 10 and Comparative Examples 7 to 9 are the same as that of Example 9. The specific compositions of each are shown in Table 3.
[0120]
[0121] The following parameters were tested for Examples 9 to 10 and Comparative Examples 7 to 9:
[0122] 1.DSC thermal analysis
[0123] The compositions of Examples 9 to 10 and Comparative Examples 7 to 9 were tested using DSC (Differential Scanning Calorimeter, TA Instruments, Mettler Toledo TGA / DSC1 StarSystem) at a rate of 10°C / min in a temperature range of 0°C to 300°C in a nitrogen atmosphere, and the DSC exothermic starting temperature T of each initial state was recorded. O With peak temperature T P . T O It is defined as the temperature at the time point when the slope of the DSC curve increases for the first time due to heat generation during DSC detection. The results are shown in Table 4.
[0124] 2. On-resistance
[0125] The film-like compositions obtained in Examples 9 to 10 and Comparative Examples 7 to 9 were cut into a size of 1.0x20mm, attached to an ITO glass substrate (size: 20mm x 20mm x 1.1mm, surface resistance: 30Ω / □), pressed at 70°C, 0.5MPa, 0.5s, and then the release film was removed. A flexible printed circuit board (width 20mm, PI thickness 25μm, copper thickness 18μm, Line / Space=80μm / 80μm) for measuring resistance was then attached to the ACF, and the joint between the glass substrate and the flexible printed circuit board was heat-pressed at 170°C, 3MPa, 8s to initiate curing, and then a multimeter was used to evaluate the on-resistance value R1 between the electrodes in the initial state. Figure 4As shown in FIG. 1 , the conductive particles 1 in the film-state polymer 10a realize the conduction between the electrode 201 of the glass substrate 200 and the electrode 301 of the flexible printed circuit board 300. Figure 3 The film-like composition 10 shown is obtained by heat pressing.
[0126] Subsequently, the connected body of the glass substrate and the flexible printed circuit board after the measurement of R1 was subjected to a high temperature and high humidity test under the conditions of 85°C and 85% RH for 168 hours, and then the on-resistance value R2 was measured.
[0127] 3. Bond strength
[0128] The connection body of the glass substrate and the flexible printed circuit board after the on-resistance R1 was detected in the initial state was evaluated in accordance with the standard JIS-Z0237, and the bonding strength S1 of the connection body was measured by the 90-degree peeling method. Here, as the bonding strength measuring device, QC-508E (peeling speed 50 mm / min, 25° C.) manufactured by Guanglei Enterprise Co., Ltd. was used.
[0129] In addition, the connection of the glass substrate and the flexible printed circuit board after the on-resistance R1 was measured in the initial state was subjected to a high temperature and high humidity test at 85°C and 85% RH for 168 hours, and the bonding strength S2 was measured according to the above method.
[0130] 4. Storage stability
[0131] After the film compositions of Examples 9 to 10 and Comparative Examples 7 to 9 were placed at room temperature (25° C.) for 1 week, 2 weeks, 3 weeks and 1 month, the DSC exothermic onset temperature T of each film was measured according to the above-mentioned detection method. O , peak temperature T P , on-resistance R and bonding strength S, the results are shown in Table 4 and Table 5 (wherein, due to the T of each film after 1 week, 2 weeks, and 3 weeks O and T P , and T of each membrane after 1 month O and T P The T values of each membrane after 1 week, 2 weeks, and 3 weeks are basically the same. Table 4 does not show the T values of each membrane after 1 week, 2 weeks, and 3 weeks. O and T P ).
[0132] Table 3
[0133]
[0134] Table 4
[0135]
[0136] Table 5
[0137]
[0138] According to Table 4 and Table 5, compared with the comparative example, the composition of the embodiment of the present application has excellent low-temperature rapid curing and storage stability, and therefore has excellent and continuously stable and reliable characteristics in terms of bonding strength, conductivity, etc. Especially in comparative example 9, after high temperature and high humidity treatment and room temperature storage, its bonding effect is extremely unstable and has poor reliability.
[0139] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A composition, characterized in that It includes a cationic polymerizable resin, a cationic initiator and an inhibitor; The polymerization inhibitor is a hindered amine compound and / or a hindered phenol compound, and the PKa of the polymerization inhibitor is greater than 7.
0.
2. The composition according to claim 1, characterized in that The mass ratio of the polymerization inhibitor to the cationic initiator is (0.01-20):
100.
3. The composition according to claim 1 or 2, characterized in that The mass ratio of the polymerization inhibitor to the cationic polymerizable resin is not less than 1:
10.
4. The composition according to claim 1, characterized in that The cationically polymerizable resin includes an epoxy compound.
5. The composition according to claim 4, characterized in that The cationic polymerizable resin further includes an oxetane compound.
6. The composition according to claim 1, characterized in that The polymerization inhibitor has a structure shown in either Formula 1 or Formula 2, wherein R1 and R2 each independently represent a hydrogen atom, a single bond, or a monovalent organic group, R4, R5, R6, and R7 each independently represent a hydrogen atom, a single bond, an alkyl group or an alkylene group having 1 to 5 carbon atoms, and at most one of R4 and R5 is a hydrogen atom, and at most one of R6 and R7 is a hydrogen atom; R 12 represents a hydrogen atom, a single bond or a monovalent organic group, R 13 , R 14 Each independently represents a single bond, an alkyl group or an alkylene group having 1 to 8 carbon atoms.
7. The composition according to any one of claims 1 to 6, characterized in that The invention also includes auxiliary agents, which include at least one of a conductive agent, a solvent, a film former, a toughening agent, a filler, a reinforcing agent, a stabilizer, a coupling agent and a colorant.
8. A polymer, characterized in that The polymer is obtained by curing the composition according to any one of claims 1 to 7; the polymer comprises a cross-linking unit formed by the cationic polymerizable resin as a cross-linking monomer and the polymerization inhibitor.
9. A method for preparing a polymer, characterized in that: Curing the composition according to any one of claims 1 to 7 to obtain the polymer; The curing process includes light treatment or heating treatment.
10. A display screen, characterized in that: The invention comprises a first structural member, a bonding layer and a second structural member, wherein the first structural member and the second structural member are bonded via the bonding layer, and the bonding layer comprises the polymer according to claim 8.
11. The display screen according to claim 10, characterized in that: The first structural member and the second structural member are independently selected from one of a chip, a screen, a flexible printed circuit, and a packaging member.
12. An electronic device, characterized in that: It comprises a shell and the display screen according to claim 10 or 11; the display screen is connected to the shell.