High-temperature-resistant epoxy resin inductance flexible glue and preparation method thereof

By using polyols and toughening resins to form toughening agents in epoxy resin inductance soft glue, the problem of the reduction of strength of epoxy resin inductance soft glue at high temperatures is solved, and the stability and toughness at high temperatures are improved, which meets the needs of the large-scale Thermal stability requirements of power inductors and reduce production costs.

CN118978885APending Publication Date: 2024-11-19HUIZHOU SHENGSHIDA TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411012590.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-26
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The strength of the existing epoxy resin inductor soft glue decreases under high temperature conditions, resulting in inductor failure, making it difficult to meet the thermal stability requirements of high-power inductors.

Method used

The toughening agent is composed of polyols and toughening resins. The high-temperature resistant epoxy resin inductive soft glue is prepared through vacuum stirring and filtration, which improves the viscosity and toughness of the adhesive and enhances the bonding performance at high temperatures.

Benefits of technology

It maintains good toughness and bonding properties under high temperature conditions, expands the scope of product application, reduces production costs, and meets industrial production needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004964817600000101
    Figure BDA0004964817600000101
  • Figure BDA0004964817600000111
    Figure BDA0004964817600000111
Patent Text Reader

Abstract

The invention discloses a high-temperature-resistant epoxy resin inductance flexible glue and a preparation method thereof, and the high-temperature-resistant epoxy resin inductance flexible glue comprises the following components: epoxy resin, a toughening agent, a diluent, a curing agent, an accelerant, a filling pigment, a flatting agent, a defoaming agent, a dispersing agent and a rheological additive, a small amount of polyhydric alcohol can promote crosslinking among toughening groups, and compared with existing commercial toughening resin, the toughening agent provided by the scheme can improve the toughness and the thermal stability of a product, and has great application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to a high temperature resistant epoxy resin inductor soft adhesive and a preparation method thereof. Background Art

[0002] An inductor is a component that can convert electrical energy into magnetic energy and store it. It is generally composed of a skeleton, windings, a shielding cover, packaging materials, a magnetic core or an iron core, etc. The packaging materials usually include epoxy resin materials, silicone materials, polyurethane materials, etc. Among them, epoxy resin can be cross-linked with a curing agent to form a three-dimensional network structure, and the composite material skeleton structure is stably wrapped in the network structure. The epoxy resin and the curing agent are combined in proportion to form an adhesive. The resulting epoxy resin adhesive has stable chemical properties and has the characteristics of acid and alkali resistance, corrosion resistance, high bonding strength and electrical insulation. Therefore, using epoxy resin to prepare inductor soft glue can not only weaken the influence of internal stress on the performance of the inductor during the curing process of the epoxy resin, but also can play a role in reducing vibration during the use of the inductor. It is widely used in the bonding of packaging materials.

[0003] The epoxy resin curing system usually uses bisphenol A epoxy resin or bisphenol F epoxy resin to react with amines, anhydride curing agents, synthetic resin curing agents or latent curing agents. However, due to the special structure of epoxy resin, it is easy to have problems such as excessive brittleness, excessive stress, and poor thermal stability after curing. Existing products increase strength and reduce brittleness by adding plasticizers, but the problem of heat resistance of the product is not solved. At high temperatures, ordinary products will cause inductance failure due to the reduced strength of the soft glue.

[0004] As the application field of inductors continues to expand, the requirements for inductor power are getting higher and higher, and the increase in power is often accompanied by the release of a large amount of heat energy. This requires not only that the inductor soft glue has good viscosity and hardness, but also better thermal stability. However, for high-power inductors that need to withstand high temperatures for a long time, many adhesives on the market are difficult to meet the requirements. Solving the problem of inductor soft glue's heat resistance is of great significance to the promotion of inductors. Summary of the invention

[0005] In view of the above problems, the present invention provides a high temperature resistant epoxy resin inductor soft glue and a preparation method thereof, which is achieved through the following technical solutions:

[0006] A high temperature resistant epoxy resin inductor soft glue, composed of the following components by weight:

[0007] Epoxy resin: 5-15 parts, toughening agent: 25-50 parts, diluent: 1-15 parts, curing agent: 3-10 parts, accelerator: 0-3 parts, pigments and fillers: 20-50 parts, leveling agent: 0.3-5 parts, defoaming agent: 0.3-2 parts, dispersant: 0.3-2 parts, rheological additive: 0.5-2 parts.

[0008] Preferably, the epoxy resin includes one or more of bisphenol A epoxy resin (NPEL-128, NPEL-127, NPEL-134, GY-250), bisphenol F epoxy resin (NPEF-170, GY-281), novolac epoxy resin (NPPN-631, NPPN-638, EPALLOY 8240, NPPN-701, NPPN-702), silicone modified epoxy resin, and multifunctional epoxy resin (MY-720, MY-721, TACTIX742).

[0009] Preferably, the toughened epoxy resin includes one or more of dimer acid modified epoxy resin NPER-172, polyurethane modified epoxy resin NPER-133, NPER-133L, core-shell toughened epoxy resin Japan Kanebuchi MX-125, MX-154, MX-257, and nano-silica toughened epoxy resin.

[0010] Preferably, the long-chain polyol includes one or more of PEG400 and PEG800.

[0011] Preferably, the diluent is 207 diluent.

[0012] Preferably, the curing agent includes one or more of dicyandiamide, phenolic resin, and diaminodiphenyl sulfone (DDS).

[0013] Preferably, the accelerator includes one or more of dimethylimidazole, diphenylimidazole, modified imidazole (2MZ-A, 2E4MZ-CN, 2MZ-OK from Shikoku Chemical), and organic urea accelerator (UR200, UR300, UR500 from Azken, Germany).

[0014] Preferably, the pigments and fillers include one or more of silica powder, calcium carbonate, talcum powder, aluminum hydroxide and carbon black.

[0015] Preferably, the leveling agent is an acrylate leveling agent.

[0016] Preferably, the defoaming agent includes one or more of BYK-052, BYK-057 and BYK-077.

[0017] Preferably, the dispersant includes one or more of BYK-W903 and BYK-109.

[0018] Preferably, the rheological additive includes one or more of BYK-607, fumed silica R-972, and R-974.

[0019] A method for preparing a high temperature resistant epoxy resin inductor soft glue comprises the following steps:

[0020] Add epoxy resin, toughening agent, diluent and dispersant into a vacuum mixer according to the weight ratio;

[0021] Preferably, the stirring revolution speed is 1500-2000 rpm, the dispersion disk speed is 2000-2500 rpm, and the stirring is performed for 15-20 minutes;

[0022] Preferably, the toughening agent is prepared by mixing toughened epoxy resin and long-chain polyol in a mass ratio of 100:10-100:20;

[0023] Add pigment, filler, leveling agent and defoamer into the vacuum mixer according to the weight ratio;

[0024] Preferably, the stirring revolution speed is 1500-2000 rpm, the dispersion disk speed is 2000-2500 rpm, and the stirring is performed for 25-30 minutes;

[0025] Add curing agent, accelerator and rheological additive into vacuum mixer according to weight ratio;

[0026] Preferably, the stirring revolution speed is 1000-1500 rpm, the dispersion disk speed is 800-1200 rpm, and the stirring is performed for 10-15 minutes;

[0027] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0028] Compared with the existing technology, the advantages of this solution are: polyols and toughening resins form a toughening agent, and polyols increase the cross-linking density of the toughening groups of the toughening resin itself, increase the toughening space, and maintain high strength and hardness of the toughening resin while having high impact toughness. The epoxy resin is modified by adding the toughening agent, and the resulting adhesive has high viscosity and hardness, and maintains good toughness and normal bonding properties even under high temperature conditions, and has a wider range of applications than ordinary products. On the other hand, the raw materials used in this product have all been commercialized, and there is no need to make it yourself. The production cost is low, the production process is simple, and it can meet the needs of industrial production. DETAILED DESCRIPTION

[0029] The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention. Without departing from the spirit and essence of the present invention, modifications or substitutions made to the methods, steps or conditions of the present invention all belong to the scope of protection of the present invention. Unless otherwise specified, the experimental materials, reagents, instruments, etc. used in the examples of the present invention are all commercially available; unless otherwise specified, all technical means in the examples of the present invention are conventional means well known to those skilled in the art.

[0030] In order to enable those skilled in the art to better understand the technical solution of the present invention, the product of the present invention is further described in detail below in conjunction with embodiments.

[0031] The raw materials of this product include epoxy resin: 5-15 parts, toughening agent: 25-50 parts, diluent: 1-15 parts, curing agent: 3-10 parts, accelerator: 0-3 parts, pigment and filler: 20-50 parts, leveling agent: 0.3-5 parts, defoaming agent: 0.3-2 parts, dispersant: 0.3-2 parts, rheological additive: 0.5-2 parts.

[0032] Among them, the epoxy resin includes one or more of bisphenol A epoxy resin (NPEL-128, NPEL-127, NPEL-134, GY-250), bisphenol F epoxy resin (NPEF-170, GY-281), phenolic epoxy resin (NPPN-631, NPPN-638, EPALLOY 8240, NPPN-701, NPPN-702), silicone modified epoxy resin, multifunctional epoxy resin (MY-720, MY-721, TACTIX742). Toughened epoxy resin includes dimer acid modified epoxy resin NPER-172, polyurethane modified epoxy resin NPER-133, NPER-133L, core-shell toughened epoxy resin Japan Zhongyuan MX-125, MX-154, MX-257, nano-silica toughened epoxy resin one or more of them. The long-chain polyols include one or more of PEG400 and PEG800.

[0033] The toughening epoxy resin and the long-chain polyol are mixed and evenly mixed in a mass ratio of 100:10-100:20 to form a toughening agent. The reaction of polyol and toughening epoxy resin expands the toughening space, which significantly improves the modification ability of the toughening agent. At the same time, the toughening resins used in this product are all commercial products, and the toughening agent of this product can be obtained by combining a simple process flow.

[0034] Add epoxy resin, toughening agent, diluent and dispersant to a vacuum mixer according to the weight ratio, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; this step can make the active groups of epoxy resin and toughening agent fully react, modify the structure of epoxy resin, and make its molecular structure have the characteristics of high temperature resistance and high toughness. Then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes, so that the modified toughened epoxy resin epoxy group forms a covalent connection with the curing agent, construct a complete cross-linking structure, and obtain a product prototype. Stirring while evacuating, adjusting the stirring revolution speed to 1000-1500 rpm, degassing the product, sufficient stirring can ensure the degassing effect, and avoid the product from failing due to residual oxygen during the storage process. After 1 hour, filter and package the product with an 80-120 mesh screen of a filter press to obtain the product.

[0035] Example 1

[0036] The preparation raw materials include bisphenol A epoxy resin NPEL-128: 11 parts; dimer acid modified epoxy resin NPER-172: 37 parts; polyvinyl alcohol PEG800: 3 parts; 207 diluent: 13 parts; dicyandiamide curing agent: 5 parts; accelerator 2MZ-A: 1.5 parts; filler silicon micropowder: 26 parts; pigment carbon black: 0.8 parts; leveling agent 495: 0.5 parts; defoamer BYK-077: 0.3 parts, dispersant 110: 0.4 parts; rheological additive R-974: 1.5 parts.

[0037] The dimer acid modified epoxy resin NPER-172 and polyvinyl alcohol PEG800 were mixed to prepare a toughening agent;

[0038] Add bisphenol A epoxy resin NPEL-128, toughening agent, diluent and dispersant into a vacuum mixer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 15-20 minutes; then add pigment, filler, leveling agent and defoamer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes;

[0039] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0040] Example 2

[0041] The preparation raw materials include 9 parts of bisphenol A epoxy resin NPEL-128; 38 parts of polyurethane modified epoxy resin EPU-105; 4 parts of polyvinyl alcohol PEG800; 11 parts of 207 diluent; 5 parts of dicyandiamide curing agent; 1.5 parts of accelerator 2MZ-A; 28 parts of filler silicon micropowder; 0.8 parts of pigment carbon black; 0.5 parts of leveling agent 495; 0.3 parts of defoaming agent BYK-077, 0.4 parts of dispersant 110; and 1.5 parts of rheological additive R-974.

[0042] The polyurethane modified epoxy resin EPU-105 and polyvinyl alcohol PEG800 are mixed to prepare a toughening agent;

[0043] Add bisphenol A epoxy resin NPEL-128, toughening agent, diluent and dispersant into a vacuum mixer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 15-20 minutes; then add pigment, filler, leveling agent and defoamer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes;

[0044] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0045] Example 3

[0046] The preparation raw materials include bisphenol F epoxy resin NPEF-170: 12.5 parts; polyurethane modified epoxy resin EPU-105: 33 parts; polyvinyl alcohol PEG800: 2 parts; 207 diluent: 10 parts; DDS curing agent: 7 parts; accelerator 100B: 2 parts; filler calcium carbonate: 30 parts; pigment carbon black: 0.8 parts; leveling agent 495: 0.5 parts; defoaming agent BYK-077: 0.3 parts, dispersant 110: 0.4 parts; rheological additive R-974: 1.5 parts.

[0047] The polyurethane modified epoxy resin EPU-105 and polyvinyl alcohol PEG800 are mixed to prepare a toughening agent;

[0048] Add bisphenol F epoxy resin NPEL-170, toughening agent, diluent and dispersant into a vacuum mixer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 15-20 minutes; then add pigment, filler, leveling agent and defoamer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes;

[0049] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0050] Example 4

[0051] The preparation raw materials include phenolic epoxy resin NPPN-631: 10.5 parts; core-shell toughened epoxy resin MX-154: 39 parts; polyvinyl alcohol PEG800: 8 parts; 207 diluent: 8 parts; DDS curing agent: 7 parts; accelerator 100B: 2 parts; filler calcium carbonate: 32 parts; pigment carbon black: 0.8 parts; leveling agent 495: 0.5 parts; defoamer BYK-077: 0.3 parts, dispersant 110: 0.4 parts; rheological additive R-974: 1.5 parts.

[0052] The core-shell toughened epoxy resin MX-154 and polyvinyl alcohol PEG800 are mixed to prepare a toughening agent;

[0053] Add phenolic epoxy resin NPPN-631, toughening agent, diluent and dispersant into a vacuum mixer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 15-20 minutes; then add pigment, filler, leveling agent and defoamer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes;

[0054] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0055] Comparative Example 1

[0056] The preparation raw materials include bisphenol A epoxy resin NPEL-128: 11 parts; polyvinyl alcohol PEG800: 3 parts; 207 diluent: 13 parts; dicyandiamide curing agent: 5 parts; accelerator 2MZ-A: 1.5 parts; filler silicon micropowder: 26 parts; pigment carbon black: 0.8 parts; leveling agent 495: 0.5 parts; defoamer BYK-077: 0.3 parts, dispersant 110: 0.4 parts; rheological additive R-974: 1.5 parts.

[0057] Add bisphenol A epoxy resin NPEL-128, polyvinyl alcohol PEG800, diluent and dispersant into a vacuum mixer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 15-20 minutes; then add pigment, filler, leveling agent and defoamer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes;

[0058] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0059] Comparative Example 2

[0060] The preparation raw materials include bisphenol A epoxy resin NPEL-128: 11 parts; dimer acid modified epoxy resin NPER-172: 37 parts; 207 diluent: 13 parts; dicyandiamide curing agent: 5 parts; accelerator 2MZ-A: 1.5 parts; filler silicon micropowder: 26 parts; pigment carbon black: 0.8 parts; leveling agent 495: 0.5 parts; defoamer BYK-077: 0.3 parts, dispersant 110: 0.4 parts; rheological additive R-974: 1.5 parts.

[0061] Add bisphenol A epoxy resin NPEL-128, polyvinyl alcohol PEG800, diluent and dispersant into a vacuum mixer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 15-20 minutes; then add pigment, filler, leveling agent and defoamer, stir at a revolution speed of 1500-2000 rpm, a dispersion disk speed of 2000-2500 rpm, and stir for 25-30 minutes; then add curing agent, accelerator and rheological additive, stir at a revolution speed of 1000-1500 rpm, a dispersion disk speed of 800-1200 rpm, and stir for 10-15 minutes;

[0062] The mixture was stirred while vacuuming at a revolution speed of 1000-1500 rpm. After 1 hour, the mixture was filtered and packaged using a filter press with an 80-120 mesh screen to obtain the soft gel.

[0063] Experimental example

[0064] The products obtained from all the above examples and comparative examples were tested for properties such as viscosity, tensile strength, and shear strength. The test results are shown in the following table:

[0065]

[0066]

[0067] It can be seen from the test results that Comparative Example 1 lacks toughening resin during the preparation process, and Comparative Example 2 lacks polyols during the preparation process. Although the gel time of the product is similar to that of Examples 1-4, the viscosity of the product is significantly lower than that of Examples 1-4. Compared with Examples 1-4, there is no significant difference in tensile strength and shear strength at room temperature in Comparative Example 1, but the tensile strength and shear strength of the product obtained in Example 1 drop sharply at high temperature, indicating that the toughening resin is of great significance for the adhesive to maintain structural stability at high temperatures. Compared with Examples 1-4, the tensile strength and shear strength of the two are similar at room temperature. The disadvantage is that under high temperature conditions, the performance of the product obtained in Comparative Example 2 is not as good as that of the embodiment. Although the product of Comparative Example 2 still maintains a certain stability at high temperature, it is far less than the effect of adding polyols to the toughening resin, indicating that polyols can significantly increase the cross-linking density of the internal molecules of the toughening resin, increase the toughening space, and maintain structural stability. The products of Examples 1-4 add toughening agents during the preparation process, and the viscosity is greater than 150,000, the tensile strength is greater than 19MPa under room temperature, and the shear strength is greater than 12Mpa, indicating that the product has good toughness. Under high temperature (150° C.), the tensile strength of the products of Examples 1-4 is still greater than 17.5 MPa, and the shear strength is greater than 11.5 MPa, indicating that the toughening agent provided in this solution can improve the thermal stability of the product.

[0068] It can be understood that the above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the patent scope of the present invention. It should be pointed out that, for ordinary technicians in this field, the above technical features can be freely combined without departing from the concept of the present invention, and several deformations and improvements can be made, which all belong to the protection scope of the present invention. Therefore, all equivalent changes and modifications made to the scope of the claims of the present invention should belong to the coverage of the claims of the present invention.

Claims

1. A high temperature resistant epoxy resin inductor soft glue, characterized in that: The composition comprises the following components in parts by weight: 5-15 parts of epoxy resin; 25-50 parts of toughening agent; 1-15 parts of diluent; 3-10 parts of curing agent; 0-3 parts of accelerator; 20-50 parts of pigment and filler; 0.3-5 parts of leveling agent; 0.3-2 parts of defoaming agent; 0.3-2 parts of dispersant; 0.5-2 parts of rheological additive, wherein the toughening agent is a compound of toughened modified epoxy resin and long-chain polyol.

2. The high temperature resistant epoxy resin inductor soft glue according to claim 1, characterized in that: The epoxy resin includes one or more of bisphenol A epoxy resin, bisphenol F epoxy resin, novolac epoxy resin, silicone-modified epoxy resin, and multifunctional epoxy resin.

3. The high temperature resistant epoxy resin inductor soft glue according to claim 1, characterized in that: The toughening agent includes one or more of dimer acid modified epoxy resin, polyurethane modified epoxy resin, core-shell toughened epoxy resin, and nano-silicon dioxide toughened epoxy resin.

4. The high temperature resistant epoxy resin inductor soft glue according to claim 1, characterized in that: The long-chain polyol includes one or both of polyethylene glycol 400 and polyethylene glycol 800.

5. The high temperature resistant epoxy resin inductor soft adhesive according to claim 1, characterized in that: The diluent is polypropylene glycol diglycidyl ether.

6. The high temperature resistant epoxy resin inductor soft adhesive according to claim 1, characterized in that: The curing agent includes one or more than two of dicyandiamide, phenolic resin and diaminodiphenyl sulfone.

7. The high temperature resistant epoxy resin inductor soft adhesive according to claim 1, characterized in that: The accelerator includes one or more of dimethylimidazole, diphenylimidazole, modified imidazole and organic urea accelerator.

8. The high temperature resistant epoxy resin inductor soft adhesive according to claim 1, characterized in that: The pigment and filler include one or more of silica powder, calcium carbonate, talcum powder, aluminum hydroxide and carbon black.

9. A method for preparing a high temperature resistant epoxy resin inductor as claimed in claim 1, characterized in that: The following steps are involved: Mix the epoxy resin, toughening agent, diluent and dispersant according to the weight ratio and stir for 15-20 minutes; Mix the pigment, filler, leveling agent and defoamer according to the weight ratio and stir for 25-30 minutes; Mix the curing agent, accelerator and rheological additive according to the weight ratio and stir for 10-15 minutes; The high temperature resistant epoxy resin inductor soft glue according to claim 1 is obtained by stirring while vacuuming and filtering.

10. The method according to claim 9, characterized in that: The toughening agent is prepared by uniformly mixing toughening epoxy resin and long-chain polyol in a mass ratio of 100:10-100:20.